A reverse ZrO2 / Co catalyst and its catalytic CO2 hydrogenation to C 5+ Applications of Alkanes

By loading Co on ZrO2 and constructing the ZrO2-Co interface, the problem of traditional catalyst deactivation and C5+ product generation is solved, a highly selective catalyst for converting CO2 into C5+ hydrocarbons is realized, the activity and cycle performance of the catalyst are improved, and the CO2 Efficient use of resources and clean energy production.

CN116173959BActive Publication Date: 2024-10-22SHAANXI UNIV OF SCI & TECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211597604.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-12
Publication Date
2024-10-22
Estimated Expiration
2042-12-12

AI Technical Summary

Technical Problem

When traditional Co-based catalysts catalyze CO2 hydrogenation reactions, metal-support interactions lead to deactivation, making it difficult to generate C5+ products, and it is difficult for existing catalysts to generate liquid hydrocarbons with high selectivity.

Method used

Using a reverse ZrO2/Co catalyst, Co is loaded on ZrO2 as a carrier, and the ZrO2-Co interface is constructed through a specific preparation method to optimize the structure and performance of the catalyst to achieve highly selective adsorption of CO2 and efficient synthesis of C5+ alkanes.

Benefits of technology

It achieves the highly selective generation of C5+ hydrocarbons, avoids the deactivation problem of traditional catalysts, improves the recycling performance of the catalyst, and provides an efficient route for CO2 resource utilization and clean energy production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116173959B_ABST
    Figure CN116173959B_ABST
Patent Text Reader

Abstract

The invention discloses a reverse ZrO2 / Co catalyst and a method for catalyzing CO2 hydrogenation to synthesize C 5+ Application of alkanes. The catalyst is ZrO2 loaded with Co as a carrier, wherein the molar ratio of Co to Zr is 4 to 16:1; the preparation method is as follows: after a soluble cobalt salt and a soluble zirconium salt are fully dissolved in deionized water, they are added dropwise to an alkaline solution under vigorous stirring conditions to form a precipitate, and the precipitate is aged, washed, dried, ground, roasted, reduced with hydrogen, and passivated in an inert atmosphere at room temperature to obtain a reverse ZrO2 / Co catalyst. The catalyst of the present invention can utilize the regulating effect of the ZrO2 component to improve the catalyst's adsorption of CO2 and inhibit H2 adsorption, and can fully utilize the interfacial effect of the ZrO2 / Co catalyst to obtain highly selective C in the CO2 hydrogenation reaction. 5+ Alkanes, and the selectivity reached 78.2%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of CO2 hydrogenation catalysts, and specifically relates to a reverse ZrO2 / Co catalyst and the catalyst for catalyzing CO2 direct hydrogenation to synthesize C 5+ Applications in alkanes. Background Art

[0002] With the increasing degree of industrialization and the sharp increase in population, the current society's demand for energy, especially fossil energy, is also increasing. However, the large-scale consumption of fossil energy has caused the concentration of CO2 in the atmosphere to show a gradual upward trend. According to the World Meteorological Organization (WMO), the concentration of CO2 in the atmosphere has increased from 280ppm before the industrial revolution to 417ppm in 2022, and is expected to reach 570ppm by the end of this century. Converting greenhouse gas CO2 into high-value-added products has broad application prospects. It can not only alleviate the climate problems caused by the increase in CO2 concentration in the atmosphere, but also reduce the pressure of fossil fuel consumption and realize the effective circulation of C1 resources. my country has proposed to reach the peak of CO2 emissions by 2030 and achieve carbon neutrality by 2060. Faced with the increasingly severe pressure of low-carbon emission reduction and the increase in carbon market, efficient conversion and utilization of CO2 is the focus of current research in the field of C1 chemical industry. Hydrogen is not only a clean energy source, but also an important reducing agent. Using renewable hydrogen to convert CO2 into value-added products has been proven to be a solution to achieve this goal. Compared with C1 products such as methane, methanol, and formic acid, products containing two or more carbon atoms (C 2+ ), especially liquid hydrocarbons (C 5+ ) is facing greater challenges in the synthesis of CO2. The heterogeneous catalytic hydrogenation of CO2 to produce industrial basic products such as gasoline, jet fuel, diesel and liquid fuel can not only effectively alleviate the environmental problems caused by large-scale CO2 emissions, but also reduce our excessive dependence on fossil fuels. Therefore, it has very important theoretical significance and practical value.

[0003] Co-based catalysts are commonly used catalysts for catalyzing CO2 hydrogenation reactions. In the art, Co-based catalysts are usually loaded on carriers such as SiO2, Al2O3, TiO2, etc., and when catalyzing CO2 hydrogenation reactions, low-carbon products such as CO, CH4, CH3OH, etc. are mainly produced (J.Am.Chem.Soc., 2014, 136, 2260-2263; Catal.Today, 2002, 71, 411-418; Appl.Catal.A-Gen., 2017, 547, 219-229; Fuel Process.Technol., 2018, 176, 101-106; Chin.J.Catal., 2018, 39, 1294-1302, etc.). These catalysts form inactive Co-support species due to the presence of strong metal-support interaction (SMSI), and as the nano-Co particles grow, the catalyst deactivates. Therefore, these shortcomings limit the further application of this type of catalyst. The ZrO2 support can not only provide a large number of oxygen vacancies, but also regulate the acid-base properties of the catalyst surface, so it is often used as a support for active species such as Co, Cu, and Ni. However, Co / ZrO2 and FeCoK / ZrO2 can only catalyze the hydrogenation of CO2 to produce C1 products such as CO and CH4 (ACS Catal., 2021, 11, 9450-9461; Appl. Catal. B-Environ., 2019, 254, 531-540; Int. J. Hydrogen. Energy, 2020, 745, 15254-15262). In addition to Co / ZrO2 catalysts, most Cu / ZrO2-based catalysts can catalyze the hydrogenation of CO2 to produce CH3OH (Nat. Catal., 2022, 5, 818-831), and Ni / ZrO2 can achieve the catalytic conversion of CO2 hydrogenation to produce C1 products such as methane and methanol (Appl. Surf. Sci., 2022, 600, 154151). It can be seen that traditional supported catalysts are difficult to reduce CO2 to C 5+ product.

[0004] Compared with traditional metal / metal oxide catalysts, reverse metal oxide / metal catalysts have special structural characteristics. In reverse metal oxide / metal catalysts, the existence of the metal oxide / metal interface and the size effect lead to changes in its redox characteristics, which in turn can affect the electronic and chemical properties of the interface through electronic perturbations. Therefore, the use of this type of catalyst can show catalytic properties different from those of traditional metal / metal oxides. For example, recently, researchers developed a reverse ZrO2 / Cu catalyst, which showed the highest methanol production rate (524g / cm2) at 220°C. MeOH kg cat-1 h -1 ), which is 3.3 times more active than traditional Cu / ZrO2 catalyst (Nat. Commun., 2020, 11, 5767). Summary of the invention

[0005] The present invention aims to provide a cheap reverse ZrO2 / Co catalyst and the catalyst for catalyzing CO2 hydrogenation to synthesize C 5+ Application of alkanes. The reverse ZrO2 / Co catalyst of the present invention exhibits different selectivity from conventional catalysts when catalyzing CO2 hydrogenation, and in particular can generate important liquid alkanes with high selectivity. The present invention can not only make large-scale use of CO2 resources in the environment, but also provide an important technical solution and experimental basis for the realization of dual carbon goals.

[0006] The reverse ZrO2 / Co catalyst provided by the present invention uses Co as a carrier to load ZrO2, wherein the molar ratio of Co to Zr is 4 to 16:1; the preparation method thereof is as follows: after a soluble cobalt salt and a soluble zirconium salt are fully dissolved in distilled water, they are dripped into an alkaline solution under vigorous stirring conditions to generate a precipitate, and the precipitate is subjected to aging, washing, drying, grinding, roasting, hydrogen reduction, and passivation in an inert atmosphere at room temperature to obtain a reverse ZrO2 / Co catalyst.

[0007] In the catalyst, the molar ratio of Co to Zr is preferably 9 to 11:1.

[0008] In the preparation method of the catalyst, the soluble cobalt salt is preferably selected from Co(NO3)2 or its hydrate, the soluble zirconium salt is selected from one or two of Zr(NO3)4, ZrClO2 and their hydrates, and the alkali solution is an aqueous solution of any one or more of Na2CO3, NaHCO3, K2CO3, KHCO3, NH3·H2O.

[0009] In the preparation method of the catalyst, the aging temperature is preferably 20-40°C, the drying temperature is 60-100°C, and the time is 6-12 hours; the calcination temperature is preferably 500-600°C, and the time is 3-5 hours; the hydrogen reduction temperature is preferably 500-600°C, and the time is 3-5 hours, and H2 or a mixture of H2 and any one of N2, Ar, and He is used for hydrogen reduction; the time for passivation in an inert atmosphere at room temperature is preferably 3-48 hours, and the inert atmosphere is any one of N2, He, and Ar.

[0010] The reverse ZrO2 / Co catalyst of the present invention is used for catalyzing CO2 hydrogenation to synthesize C 5+ The application of CO2 hydrogenation to synthesize C 5+The reaction of alkanes is carried out in an intermittent reactor. During the reaction, the CO2 pressure is 1-4 MPa, the H2 pressure is 1-4 MPa, the reaction temperature is 160-200°C, and the reaction solvent is cyclohexane or benzene.

[0011] The beneficial effects of the present invention are as follows:

[0012] 1. The present invention avoids the agglomeration and deactivation of the traditional supported Co-based active components by constructing the interface between ZrO2 and Co active components, and at the same time forms a strong interaction at the ZrO2-Co interface, so that the catalyst has a higher catalytic reaction activity;

[0013] 2. The present invention improves the CO2 adsorption performance of the Co-based catalyst by introducing the ZrO2 component, while reducing the hydrogen adsorption performance, thereby increasing the CO2 adsorption density on the catalyst surface and achieving C 5+ Highly selective synthesis of alkanes;

[0014] 3. The catalyst of the present invention has excellent recycling performance, which lays a foundation for its industrial development;

[0015] 4. The preparation of liquid hydrocarbons in the present invention is to synthesize C 5+ The reaction route of alkanes is one of the important routes developed to realize the chemical utilization of CO2 resources. It can not only utilize a large amount of CO2 in the atmosphere, but also provide a large amount of clean energy products (C 5+ Alkanes), enriching the ways to achieve dual-carbon goals and thus having important industrial application value. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 These are the TEM images (a and b) and HAADF-STEM image (c) of the fresh reverse ZrO2 / Co (Co / Zr=9) catalyst prepared in Example 1 and the corresponding EDS elemental maps of Co (d), Zr (e), and O (f).

[0017] Figure 2 1 is an X-ray diffraction analysis diagram of the fresh, used and unreduced reverse ZrO2 / Co (Co / Zr=9) catalyst prepared in Example 1.

[0018] Figure 3 This is the H2-TPR diagram of the reverse ZrO2 / Co (Co / Zr=9) catalyst prepared in Example 1. DETAILED DESCRIPTION

[0019] The present invention is further described in detail below with reference to the accompanying drawings and examples, but the protection scope of the present invention is not limited to these examples. The experimental methods used in the examples are conventional methods unless otherwise specified; the materials, reagents, etc. used in the examples are all commercially available unless otherwise specified.

[0020] Example 1

[0021] According to the molar ratio of Co to Zr in the catalyst of 9:1, Co(NO3)2·6H2O (2.1 g, 7.2 mmol) and Zr(NO3)4·5H2O (0.35 g, 0.8 mmol) were dissolved in 40 mL of deionized water and stirred for 30 minutes. Then, the obtained solution was added dropwise to 100 mL of 0.5 mol / L Na2CO3 aqueous solution at a rate of 0.2 mL / s using a constant pressure dropping funnel under vigorous stirring. After the addition, it was vigorously stirred for 8 hours. The obtained solid precipitate was centrifuged, aged at 25°C, washed with deionized water until the filtrate was neutral, and then dried in an oven at 100°C for 10 hours, ground into powder in an agate mortar, and then transferred to a porcelain ark, calcined at 500°C for 3 hours, reduced at 500°C for 3 hours in a hydrogen atmosphere using a tubular furnace, and then passivated at room temperature for 24 hours in a N2 atmosphere to obtain a reverse ZrO2 / Co (Co / Zr=9) catalyst.

[0022] The obtained reverse ZrO2 / Co (Co / Zr=9) catalyst was characterized. Figures 1 to 3 . Figure 1 The results show that ZrO2 / Co (Co / Zr=9) catalysts are mostly spherical particles of 30 to 50 nm. From the element scanning mapping, it can be seen that ZrO2 is loaded on the Co-based catalyst, indicating that the obtained structure is a reverse ZrO2 / Co (Co / Zr=9) catalyst. Figure 2 X-ray diffraction analysis (XRD) showed that there were two crystalline phases in the ZrO2 / Co (Co / Zr=9) catalyst, namely ZrO2 and elemental Co. Figure 3 The H2-TPR test showed that the presence of ZrO2 could inhibit the reduction of cobalt oxides, indicating a strong interaction between ZrO2 and Co species.

[0023] Example 2

[0024] In this embodiment, according to the molar ratio of Co to Zr in the catalyst being 6:1, Co(NO3)2·6H2O (2.00 g, 6.86 mmol) and Zr(NO3)4·5H2O (0.49 g, 1.14 mmol) were dissolved in 40 mL of deionized water and stirred for 30 minutes. The other steps were the same as in Example 1 to obtain a reverse ZrO2 / Co (Co / Zr=6) catalyst.

[0025] Example 3

[0026] In this embodiment, according to the molar ratio of Co to Zr in the catalyst being 11:1, Co(NO3)2·6H2O (2.13 g, 7.33 mmol) and Zr(NO3)4·5H2O (0.29 g, 0.67 mmol) were dissolved in 40 mL of deionized water and stirred for 30 minutes. The other steps were the same as in Example 1 to obtain a reverse ZrO2 / Co (Co / Zr=11) catalyst.

[0027] Example 4

[0028] In this embodiment, according to the molar ratio of Co to Zr in the catalyst being 16:1, Co(NO3)2·6H2O (2.19 g, 7.53 mmol) and Zr(NO3)4·5H2O (0.20 g, 0.47 mmol) were dissolved in 40 mL of deionized water and stirred for 30 minutes. The other steps were the same as in Example 1 to obtain a reverse ZrO2 / Co (Co / Zr=16) catalyst.

[0029] Comparative Example

[0030] According to the method of Example 1 above, Sm2O3 / Co (Co / Sm=9) catalyst, SrO / Co (Co / Sr=9) catalyst and Ga2O3 / Co (Co / Ga=9) catalyst were prepared.

[0031] The Co / ZrO2 (Co loading of 4%, Co / Zr=0.088) catalyst was prepared by impregnation method. The specific preparation method was as follows: Co(NO3)2·6H2O (0.20 g, 0.687 mmol) was dissolved in 4 mL of deionized water, and then added to 0.96 g of ZrO2 carrier. After impregnation overnight, the catalyst was stirred and dried. The remaining calcination, reduction, passivation and other processes were similar to the catalyst preparation process in Example 1.

[0032] Example 5

[0033] The reverse ZrO2 / Co catalysts prepared in Examples 1 to 4 were used to catalyze the CO2 hydrogenation reaction, and the catalytic performance was compared with that of the catalysts Co3O4, Co, ZrO2, Sm2O3 / Co (Co / Sm=9), SrO / Co (Co / Sr=9), and Ga2O3 / Co (Co / Ga=9), and the effect of the reaction solvent on the reaction results was investigated. The specific method of the hydrogenation reaction is as follows:

[0034] 20 mg of catalyst and 1 g of solvent were added to a 16 mL stainless steel reactor with a polytetrafluoroethylene liner, the reactor was closed, and the gas in the reactor was replaced three times with 1 MPa of carbon dioxide. Before the reaction, 4 MPa of carbon dioxide and 4 MPa of hydrogen were filled at room temperature. The reactor was heated to 200 ° C and the reaction was started. After 15 hours of reaction, the reactor was placed in an ice water bath to cool, and the gas was slowly released and collected in an air bag and analyzed in a gas chromatograph. The liquid phase after the reaction was analyzed by gas chromatography, and 5 μL of toluene was used as an internal standard. The obtained product was qualitatively analyzed by gas chromatography-mass spectrometry, and the results are shown in Table 1.

[0035] Table 1 Effects of different catalytic systems on CO2 hydrogenation reaction

[0036]

[0037]

[0038] As shown in Table 1, among the different bimetallic catalysts, the Co-Zr bimetallic catalyst exhibits 5+ The selectivity of long-chain alkanes is the highest, and the prepared bimetallic catalysts such as Sm2O3 / Co (Co / Sm=9), SrO / Co (Co / Sr=9), and Ga2O3 / Co (Co / Ga=9) all produce highly selective C 1-4 Among the solvents investigated, the catalyst showed higher C 5+ Selectivity, while the C produced in solvent-free system, DMI solvent or water solvent 1-4 In addition, when the conventional Co / ZrO2 catalyst prepared in the comparative example was used in the reaction, all products were mainly CH4 and a small amount of CO, indicating that the reverse ZrO2 / Co catalyst can be used to efficiently produce C 5+ When the reverse ZrO2 / Co catalyst of the present invention has a Co / Zr molar ratio of 9 and is subjected to relatively low temperature conditions (200°C), the C 5+ The selectivity of liquid alkanes is as high as 78.2% and the activity is 9.3mmol CO2 ·g cat -1 ·h -1 , which is higher than other Co / Zr ratios, and can achieve high selectivity in converting CO2 into C 5+ Liquid alkanes have important practical significance for achieving the goal of carbon neutrality.

Claims

1. A reverse ZrO2 / Co catalyst, characterized in that: The reverse ZrO2 / Co catalyst uses Co as a carrier to load ZrO2, wherein the molar ratio of Co to Zr is 4 to 16:1; its preparation method is: after soluble cobalt salt and soluble zirconium salt are fully dissolved in deionized water, they are added dropwise into alkaline solution under vigorous stirring conditions to form a precipitate, and the precipitate is aged, washed, dried, ground, calcined, reduced with hydrogen, and passivated in an inert atmosphere at room temperature to obtain a reverse ZrO2 / Co catalyst.

2. The reverse ZrO2 / Co catalyst according to claim 1, characterized in that: The molar ratio of Co to Zr is 9 to 11:

1.

3. The reverse ZrO2 / Co catalyst according to claim 1, characterized in that: The soluble cobalt salt is selected from Co(NO3)2 or its hydrate; the soluble zirconium salt is selected from one or two of Zr(NO3)4, ZrClO2 and their hydrates.

4. The reverse ZrO2 / Co catalyst according to claim 1, characterized in that: The alkali solution is an aqueous solution of any one or more of Na2CO3, NaHCO3, K2CO3, KHCO3, and NH3·H2O.

5. The reverse ZrO2 / Co catalyst according to claim 1, characterized in that: The aging temperature is 20-40° C., the drying temperature is 60-100° C., and the drying time is 6-12 hours.

6. The reverse ZrO2 / Co catalyst according to claim 1, characterized in that: The calcination temperature is 500-600° C. and the calcination time is 3-5 hours.

7. The reverse ZrO2 / Co catalyst according to claim 1, characterized in that: The temperature of the hydrogen reduction is 500-600° C., the time is 3-5 hours, and the hydrogen reduction is performed using H 2 or a mixed gas of H 2 and any one of N 2 , Ar, and He.

8. The reverse ZrO2 / Co catalyst according to claim 1, characterized in that: The time of the room temperature inert atmosphere passivation is 12 to 36 hours, and the inert atmosphere is any one of N2, He, and Ar.

9. The reverse ZrO2 / Co catalyst according to claim 1 is used for catalyzing CO2 hydrogenation to synthesize C 5+ Applications in alkanes.

10. The reverse ZrO2 / Co catalyst according to claim 9 is used for catalyzing CO2 hydrogenation to synthesize C 5+ Application in alkanes, characterized by: The CO2 hydrogenation synthesis C 5+ The reaction of alkanes is carried out in a batch reactor. The CO2 pressure is 1 to 4 MPa, the H2 pressure is 1 to 4 MPa, the reaction temperature is 160 to 200°C, and the reaction solvent is cyclohexane or benzene.