Metal element and molecular sieve composite catalytic material and preparation method and application thereof

By introducing heteroatom precursors and metal precursors during the hydrothermal synthesis of molecular sieves, composite catalytic materials of metal oxide nanoparticles and molecular sieves are prepared, which solves the problems of dispersion of metal nanoparticles and formation of hierarchical pore structures in the existing technology. problem, achieving synergistic catalysis between framework heteroatoms and metal nanoparticles, significantly improving catalytic activity.

CN116174012BActive Publication Date: 2024-10-15CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202111424547.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-26
Publication Date
2024-10-15
Estimated Expiration
2041-11-26

AI Technical Summary

Technical Problem

The existing technology is difficult to simultaneously achieve high dispersion of metal nanoparticles in molecular sieves and the formation of hierarchical pore structures through one method, and fails to effectively exert the synergistic catalytic effect of framework heteroatom sites and metal nanoparticles in molecular sieve channels.

Method used

By introducing heteroatom precursors, metal precursors, dendrimers and silanization reagents during the hydrothermal synthesis process of molecular sieves, and performing hydrothermal crystallization and roasting treatments, composite catalytic materials of metal oxide nanoparticles and molecular sieves are prepared. Uniform dispersion of metal nanoparticles and formation of hierarchical pore structure, and optimization of catalytic performance by controlling the ratio of UV-Vis spectral features.

Benefits of technology

A catalytic material with a large specific surface area and rich pore volume was obtained. The metal nanoparticles were uniformly dispersed in the hierarchical pore structure, which significantly improved the catalytic activity of macromolecular substrate reactions, especially in the co-oxidation reaction of cyclooctene and isobutyraldehyde. Demonstrated efficient catalytic effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116174012B_ABST
    Figure CN116174012B_ABST
Patent Text Reader

Abstract

The present invention relates to a metal element and molecular sieve composite catalytic material and a preparation method and application thereof. The composite catalytic material comprises a framework heteroatom molecular sieve and a metal element M dispersed in the crystal of the molecular sieve; the framework heteroatom molecular sieve is a molecular sieve in which at least part of the silicon in the framework of the all-silicon molecular sieve is replaced by a heteroatom element Q, and the heteroatom element Q is one or more selected from titanium, boron, zirconium, tin, aluminum, phosphorus and germanium; the composite catalytic material has the following UV-Vis characteristics: in the peak separation result of the wavelength of 460-740nm in the UV-Vis spectrum of the composite catalytic material, the peak area of ​​the spectrum peak in the wavelength range of 460-540nm is recorded as A1, and the total peak area in the wavelength range of 460-740nm in the UV-Vis spectrum of the composite catalytic material is recorded as A2, and A0 defined by the following formula (1) is an arbitrary value between 10% and 20%; A0=A1 / A formula (1).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the field of catalytic materials, and in particular, to a metal element and molecular sieve composite catalytic material and a preparation method and application thereof. Background Art

[0002] Framework heteroatom substituted molecular sieves are important materials for achieving shape and size selective catalysis. The effectiveness of these materials for the desired catalytic reaction depends critically on the dispersed interaction between the zeolite micropores and the reactant molecules stabilized therein. The bimetallic or multimetallic synergistic effect in the field of chemistry refers to the performance produced by doping two or more metals that is higher than the performance produced when any of the components exist alone. These properties may refer to chemical properties. For example, catalytic activity, or an increase in catalytic life. It is generally believed that the generation of catalytic synergistic effects comes from the mixing of more than one active metal; or the generation of proton positions; or changes in the electronic structure caused by changes in the surface morphology of nanoparticles.

[0003] Direct hydrothermal synthesis generally refers to the direct introduction of metal precursors during the crystallization of molecular sieves. During the hydrothermal crystallization process, the metal precursors can interact with the secondary structure of the molecular sieve through electrostatic effects or van der Waals forces. Therefore, during the self-assembly process of the secondary structural units, the metal nanoparticles are evenly embedded in the molecular sieve framework. Since the above process is carried out under strong alkalinity and high temperature hydrothermal conditions, the metal precursors are very easy to form hydroxide precipitation. To solve this problem, the precursor metal ions often form complexes with ligands containing lone pairs of electrons (such as organic amine ligands or ammonia, etc.). In addition to preventing coagulation, the complexing agent can also play the role of isolation and dispersion, which helps to form highly dispersed metal nanoparticles. Highly dispersed metal nanoparticles help to inhibit the sintering of metals at high temperatures.

[0004] Wang Baorong et al. (CN 111847471 A) prepared a multi-level porous molecular sieve encapsulating active metals by introducing a silanization agent into a direct hydrothermal synthesis method. However, since the above process is carried out under strong alkalinity and high temperature hydrothermal conditions, the metal precursor is very likely to form hydroxide precipitation. Without solving this problem, the precursor metal ions often form complexes with ligands containing lone pairs of electrons (such as organic amine ligands or ammonia). For example, Wang et al. used ethylenediamine ligands to form complexes with PdCl 2 Formation of [Pd(NH 2 CH 2 CH 2 NH 2 )]Cl 2 The complex precursor was then directly synthesized by hydrothermal crystallization method to directly synthesize silicalite-1 molecular sieve embedded with uniformly dispersed Pd nanoparticles (Pd@silicalite-1).

[0005] Dendrimers are a new type of highly branched, symmetrical, radial functional polymers, also known as dendritic grafted macromolecules or ultra-high branched polymers. Due to their highly branched structure and unique monodispersity, these compounds have special properties and functions, and are widely used in research fields such as host-guest chemistry, catalysts, metal nanomaterials, nanocomposite catalytic materials, membrane materials, surfactants, and medicine. Their rich coordination sites, large-volume steric hindrance, and controllability are expected to be used in the synthesis of metal nanocatalysts.

[0006] In summary, the prior art highly disperses metal nanoparticles in the molecular sieve crystals by complexing metal precursors with organic ligands and then introducing them into the molecular sieve hydrothermal crystallization process, and expands the pores by introducing silanization agents into the molecular sieve synthesis process. However, the prior art cannot achieve the above two effects at the same time through a single preparation method; nor can it achieve the synergistic catalytic effect of the framework heteroatom sites and the metal nanoparticles in the molecular sieve pores. Summary of the invention

[0007] The purpose of the present disclosure is to provide a composite catalytic material of metal elements and molecular sieves, and a preparation method and application thereof. The composite catalytic material has a large specific surface area, pore volume and reaction activity of macromolecular substrates; the metal nanoparticles have uniform particle sizes and are evenly dispersed in the skeleton heteroatom molecular sieve crystals with a multi-level pore structure, and can exert a synergistic catalytic effect with the heteroatoms in the skeleton.

[0008] In order to achieve the above-mentioned object, the first aspect of the present disclosure provides a composite catalytic material of metal oxide nanoparticles and molecular sieves, comprising a framework heteroatom molecular sieve and a metal element M dispersed in the crystal of the molecular sieve; the framework heteroatom molecular sieve is a molecular sieve in which at least part of the silicon in the framework of the all-silicon molecular sieve is replaced by a heteroatom element Q, and the heteroatom element Q is one or more selected from titanium, boron, zirconium, tin, aluminum, phosphorus and germanium; the composite catalytic material has the following UV-Vis characteristics: in the peak separation result of the wavelength of 460 to 740 nm in the UV-Vis spectrum of the composite catalytic material, the peak area of ​​the spectrum peak in the wavelength range of 460 to 540 nm is recorded as A 1 The total peak area within the wavelength range of 460 to 740 nm in the UV-Vis spectrum of the composite catalytic material is recorded as A 2 , A defined by the following formula (1) 0 Any value between 10% and 20%; A 0 =A 1 / A 2 Formula (1).

[0009] Optionally, the A 0 It is any value between 12 and 18%.

[0010] Optionally, the framework heteroatom molecular sieve in the composite catalytic material is at least one of MFI structure molecular sieve, MEL structure molecular sieve, BEA structure molecular sieve, MWW structure molecular sieve, two-dimensional hexagonal structure molecular sieve, MOR structure molecular sieve and TUN structure molecular sieve; preferably one or more selected from MFI structure molecular sieve, MEL structure molecular sieve, BEA structure molecular sieve, MCM structure molecular sieve and SBA structure molecular sieve; further preferably one or more selected from MFI structure molecular sieve, MEL structure molecular sieve and BEA structure molecular sieve;

[0011] The metal element M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum, copper and gold.

[0012] Optionally, in the composite catalytic material, the molar ratio of the framework heteroatom element to the silicon element is (0.002-0.07):1, preferably (0.002-0.04):1;

[0013] The molar ratio of the metal M element to the silicon element is (0.001-0.2):1, preferably (0.002-0.18):1.

[0014] Optionally, the BET specific surface area of ​​the composite catalytic material is 400 to 800 m 2 / g, the total pore volume is 0.3-0.65mL / g, the micropore volume is 0.1-0.19mL / g, the mesopore volume is 0.2-0.46mL / g, and the metal element M in the composite catalytic material exists in the form of metal nanoparticles, and the average particle size of the metal nanoparticles is 0.5-10nm.

[0015] The second aspect of the present disclosure provides a method for preparing a composite catalytic material of metal nanoparticles and molecular sieves, comprising the following steps:

[0016] S1, mixing a template, a silicon source, a framework heteroatom precursor, water, a metal M precursor, a dendrimer and a silanization agent to obtain a reaction mixture;

[0017] S2, subjecting the reaction mixture to hydrothermal crystallization and calcination treatments;

[0018] The heteroatom element Q contained in the skeleton heteroatom precursor is selected from one of titanium, boron, zirconium, tin, aluminum, phosphorus and germanium; and the silanization agent contains at least one coordination group complexed with the metal element M.

[0019] Optionally, in step S1, SiO 2The molar ratio of the silicon source in terms of the silicon source: the template agent: the skeleton heteroatom precursor in terms of the heteroatom element Q: water: the metal element M: the silanization agent is 1: (0.005-1): (0.002-0.07): (10-80): (0.001-0.2): (0.025-0.5), preferably 1: (0.005-1): (0.002-0.04): (10-80): (0.002-0.18): (0.025-0.3); the mass of the dendritic macromolecule is 10 times that of the SiO 2 The ratio of the amount of the silicon source is (0.01-3):1, preferably (0.05-2):1.

[0020] Optionally, step S1 includes the following steps:

[0021] a. mixing a template, a silicon source, a framework heteroatom precursor and water to obtain a silicon hydrolysis solution;

[0022] b. adding the dendritic macromolecule to the aqueous solution of the metal M precursor to obtain a first mixed material; and mixing the first mixed material with the hydrolyzed solution of silicon to obtain a second mixed material;

[0023] c. adding a silanization agent to the second mixed material, and mixing to obtain the reaction mixture;

[0024] Preferably, the mixing conditions in step c include: stirring at 20-80° C. for 0.5-2 hours.

[0025] Optionally, the silicon source is selected from at least one of organic silicone grease, solid silica gel, white carbon black and silica sol; preferably, it is selected from at least one of organic silicone grease, solid silica gel and white carbon black;

[0026] More preferably, the organic silicone grease has the general formula of the structure shown in the following formula (A):

[0027]

[0028] Where R a , R b , R c , R d Each is independently selected from an alkyl group having 1 to 6 carbon atoms, wherein the alkyl group is a branched or straight chain alkyl group; preferably, R a , R b , R c , R d Each is independently selected from a straight-chain alkyl group having 1 to 4 carbon atoms or a branched-chain alkyl group having 3 to 4 carbon atoms; further preferably, the R a , R b , R c , Rd Each is independently selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl or tert-butyl; further preferably, the organic silicone grease is selected from one or more of tetramethyl silicate, tetraethyl silicate, tetrabutyl silicate and dimethyl diethyl silicone grease.

[0029] Optionally, the template is an organic base, preferably at least one selected from quaternary ammonium bases, aliphatic amines and aliphatic alcohol amines; further preferably, the template is at least one selected from quaternary ammonium bases having a structure represented by the following formula (B):

[0030] Where R 1 , R 2 , R 3 and R 4 are independently selected from an alkyl group having 1 to 4 carbon atoms, preferably a straight-chain alkyl group having 1 to 4 carbon atoms and a branched-chain alkyl group having 3 to 4 carbon atoms, more preferably R 1 , R 2 , R 3 and R 4 Each of the following is selected from the group consisting of methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl and tert-butyl;

[0031] Further preferably, the molecular sieve in the composite catalyst material is an MFI type molecular sieve, and the template agent is tetrapropylammonium hydroxide or a mixture of tetrapropylammonium hydroxide and one or more selected from tetrapropylammonium chloride and tetrapropylammonium bromide; or

[0032] The molecular sieve in the composite catalytic material is a MEL type molecular sieve, and the template agent is tetrabutylammonium hydroxide or a mixture of tetrabutylammonium hydroxide and one or more selected from tetrabutylammonium chloride and tetrabutylammonium bromide; or

[0033] The molecular sieve in the composite catalytic material is a Beta molecular sieve, and the template agent is tetraethylammonium hydroxide or a mixture of tetraethylammonium hydroxide and one or more selected from tetraethylammonium chloride and tetraethylammonium bromide.

[0034] Optionally, in step a, the silicon source is organic silicone grease, and after the template, organic silicone grease, skeleton heteroatom precursor and water are mixed, a hydrolysis and alcohol removal treatment is further performed to obtain the hydrolysis solution;

[0035] The conditions for the hydrolysis and alcohol removal treatment include: stirring and hydrolyzing at 0 to 95° C. for 2 to 10 hours; preferably stirring and hydrolyzing at 50 to 95° C. for 2 to 8 hours.

[0036] Optionally, in step S1, the skeleton heteroatom precursor includes at least one of an organic skeleton heteroatom precursor and an inorganic skeleton heteroatom precursor; the inorganic skeleton heteroatom precursor is at least one selected from chlorides, nitrates and sulfates of heteroatom element Q; the inorganic skeleton heteroatom precursor is an organic acid ester containing heteroatom element Q, selected from at least one of the structures represented by the following formula (C):

[0037]

[0038] Where R 5 , R 6 , R 7 and R 8 are each selected from an alkyl group having 1 to 6 carbon atoms, preferably a straight-chain alkyl group having 1 to 4 carbon atoms and a branched-chain alkyl group having 3 to 6 carbon atoms, and more preferably R 5 , R 6 , R 7 and R 8 are independently selected from a straight chain alkyl group having 2 to 4 carbon atoms and a branched chain alkyl group having 2 to 4 carbon atoms;

[0039] Optionally, R 5 , R 6 , R 7 and R 8 Each of the following groups is independently selected from one of methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, tert-butyl, isopentyl, hexyl and isohexyl; preferably each of the following groups is independently selected from one of ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl and tert-butyl;

[0040] Preferably, when the skeleton heteroatom is titanium, the skeleton heteroatom precursor is selected from one or more of titanium tetrachloride, titanium sulfate, titanium nitrate, tetraethyl titanate, tetrapropyl titanate and tetrabutyl titanate; when the skeleton heteroatom is boron, the skeleton heteroatom precursor is selected from one or more of boric acid and borate; when the skeleton heteroatom is tin, the skeleton heteroatom precursor is selected from one or more of tin halide, stannous halide, stannous sulfate, tin sulfate, stannate, stannate, tin nitrate, tin oxide and stannous oxide; when the skeleton heteroatom is aluminum, the skeleton heteroatom precursor is selected from one or more of sodium aluminate, aluminum sulfate, boehmite, metallic aluminum, aluminum nitrate, aluminum isopropoxide and aluminum hydroxide; when the skeleton heteroatom is phosphorus, the skeleton heteroatom precursor is selected from one or more of orthophosphoric acid, triethyl phosphoric acid and metaphosphate; when the skeleton heteroatom is germanium, the skeleton heteroatom precursor is selected from one or more of germanium oxide, germanium alkoxide, germanium chloride and sodium germanate.

[0041] Optionally, in step S1, the metal M precursor is one or more of an inorganic metal compound and an organic metal compound; the inorganic metal compound is a water-soluble inorganic salt of the metal element M; the water-soluble inorganic salt of the metal element M is selected from one or more of the chloride, hydrated chloride, sulfate, hydrated sulfate and nitrate of the metal element M; the organic metal compound is an organic ligand compound of the metal element M; preferably, the metal M precursor is a water-soluble inorganic salt of the metal element M;

[0042] The metal element M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum, copper and gold;

[0043] Preferably, the metal M precursor is an aqueous solution of the metal M precursor, and the molar ratio of the metal element M to water in the aqueous solution of the metal M precursor is 1:(50-500).

[0044] Optionally, in step S1, the dendritic macromolecule is selected from one or more of polyamide-amine macromolecules and polyarylether macromolecules;

[0045] Preferably, the polyamidoamine macromolecule is selected from one or more of the 2nd generation PAMAM with an ethylenediamine core, the 3rd generation PAMAM with an ethylenediamine core, and the 4th generation PAMAM with an ethylenediamine core;

[0046] The polyarylether macromolecule is selected from one or more of polyarylether nitrile, polyarylether sulfone and polyarylether ketone;

[0047] Preferably, the dendrimer has a weight average molecular weight of 4000 to 85000, an intrinsic viscosity at 30° C. of 0.025 to 0.045 dL / g, and a degree of branching of 4000 to 18000 (in terms of Mw).

[0048] Optionally, in step S1, the general formula of the silanization agent is R 9 Si(R 10 )(R 11 )R 12 , where R 9 , R 10 , R 11 , R 12 are independently halogen, alkyl, alkoxy, aromatic, mercapto or amine, and R 9 , R 10 , R 11 , R 12 At least one of them is an alkyl group, an alkoxy group, an aromatic group, a thiol group or an amine group; the carbon number of the alkyl group, the alkoxy group, the thiol group and the amine group is independently selected from any integer from 1 to 18, and the carbon number of the aromatic group is any integer from 6 to 18;

[0049] Preferably, the silanization agent is selected from one or more of dimethyldichlorosilane, N-phenyl-3-aminopropyltrimethoxysilane, phenyltrimethoxysilane, 1,7-dichlorooctylmethyltetrasiloxane, hexadecyltrimethoxysilane, octyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane; further preferably, it is at least one of N-phenyl-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane.

[0050] Optionally, in step S2, the conditions of the hydrothermal crystallization treatment include: being carried out under autogenous pressure, the hydrothermal crystallization time is 0.5 to 10 days, and the hydrothermal crystallization temperature is 110 to 200° C.; preferably, the hydrothermal crystallization time is 0.5 to 5 days, and the hydrothermal crystallization temperature is 150 to 200° C.;

[0051] The conditions for the calcination treatment include: a calcination temperature of 400 to 900° C. and a calcination time of 1 to 16 hours; preferably, the calcination temperature is 400 to 800° C. and the calcination time is 2 to 8 hours.

[0052] A third aspect of the present disclosure provides a metal nanoparticle and molecular sieve composite catalytic material prepared according to the method described in the second aspect of the present disclosure.

[0053] The fourth aspect of the present disclosure provides the use of the metal nanoparticles and molecular sieve composite catalytic material described in the first aspect or the third aspect of the present disclosure in catalyzing the co-oxidation reaction of macromolecular aldehydes / olefins; preferably, the use in catalyzing the co-oxidation reaction of cyclooctene and isobutyraldehyde.

[0054] Through the above technical scheme, the present disclosure provides a metal nanoparticle and molecular sieve composite catalytic material and its preparation method and application. The present disclosure introduces a heteroatom precursor in the molecular sieve crystallization synthesis process, and the heteroatom mainly enters the molecular sieve framework during crystallization. The present disclosure also introduces a metal element precursor, a dendritic macromolecule and a silanization agent into the reaction mixture. The molecular sieve of the prepared composite catalytic material has a multi-level pore structure and a large specific surface area, pore volume and macromolecular substrate reaction activity; and the metal oxide nanoparticles have a uniform particle size and are evenly dispersed in the crystal of the multi-level pore heteroatom framework molecular sieve (for example, in the mesoporous channel). And in the present disclosure, by controlling A 0 By setting the value to any value between 10% and 20% (i.e. controlling the proportion of the peak area of ​​the spectrum peak in the wavelength range of 460-540nm to the total peak area in the wavelength range of 460-740nm), more active components can be contained in the composite catalytic material and the catalytic effect can be better.

[0055] Other features and advantages of the present disclosure will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS

[0056] The accompanying drawings are used to provide a further understanding of the present disclosure and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present disclosure but do not constitute a limitation of the present disclosure. In the accompanying drawings:

[0057] Figure 1 This is the UV-Vis spectrum of the cobalt-containing multi-level pore MFI structure molecular sieve prepared in Example 1 of the present disclosure.

[0058] Figure 2 This is a peak separation diagram of the UV-Vis spectrum of the cobalt-containing multi-level pore MFI structured molecular sieve prepared in Example 1 of the present disclosure.

[0059] Figure 3 This is the XRD spectrum of the cobalt-containing multi-level pore MFI structured molecular sieve prepared in Example 1.

[0060] Figure 4 This is a SEM image of the cobalt-containing multi-level pore MFI structure molecular sieve prepared in Example 1. DETAILED DESCRIPTION

[0061] The specific implementation of the present disclosure is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described herein is only used to illustrate and explain the present disclosure, and is not used to limit the present disclosure.

[0062] The first aspect of the present disclosure provides a composite catalytic material of metal nanoparticles and molecular sieves, comprising a framework heteroatom molecular sieve and a metal element M dispersed in the crystal of the molecular sieve; the framework heteroatom molecular sieve is a molecular sieve in which at least part of the silicon in the framework of the all-silicon molecular sieve is replaced by a heteroatom element Q, and the heteroatom element Q is one or more selected from titanium, boron, zirconium, tin, aluminum, phosphorus and germanium;

[0063] The composite catalytic material has the following UV-Vis characteristics:

[0064] In the peak separation results of the wavelength of 460 to 740 nm in the UV-Vis spectrum of the composite catalytic material, the peak area of ​​the spectrum peak within the wavelength range of 460 to 540 nm is recorded as A 1 The total peak area within the wavelength range of 460 to 740 nm in the UV-Vis spectrum of the composite catalytic material is recorded as A 2 ,

[0065] A is defined as follows: 0 Any value between 10% and 20%;

[0066] A 0 =A1 / A 2 Formula (1).

[0067] The present disclosure provides a composite catalytic material of metal oxide nanoparticles and molecular sieves. The molecular sieve of the composite catalytic material has a multi-level pore structure and a large specific surface area, pore volume and macromolecular substrate reaction activity; and the metal oxide nanoparticles have uniform particle sizes and are evenly dispersed in the mesoporous channels of the multi-level pore heteroatom framework molecular sieve. There is an obvious interaction between the metal elements of the metal oxide particles and the heteroatoms in the framework. After the heteroatoms are introduced into the molecular sieve framework, the two metal sites in the composite catalytic material can play a synergistic catalytic role, effectively improving the catalytic activity of the composite catalytic material for macromolecular substrates. And in the present disclosure, by controlling A 0 Any value between 10 and 20% (i.e. controlling the proportion of the peak area of ​​the spectrum peak in the wavelength range of 460 to 540 nm in the total peak area in the wavelength range of 460 to 740 nm) can make the composite catalytic material contain more active components and achieve better catalytic effect.

[0068] The inventors of the present disclosure surprisingly discovered through a large number of experiments that heteroatom precursors, metal M precursors, dendritic macromolecules and silanization agents (including at least one coordination group complexed with the metal element M) are introduced into the reaction raw materials for crystallization synthesis of molecular sieves, and after hydrothermal crystallization and calcination treatments, heteroatoms can be introduced into the molecular sieve framework, and the skeleton heteroatom molecular sieve of the obtained composite catalytic material has a multi-level pore structure (micropores and mesopores) and a large specific surface area and pore volume, the metal oxide nanoparticles have a high uniformity in particle size and can be evenly dispersed in the pores of the skeleton heteroatom molecular sieve, and a certain amount of metal M nanoparticles will also exist on the surface of the pores; the heteroatom metal sites on the molecular sieve framework and the metal sites (nanoparticles) of the metal element M in the pores can also play a synergistic catalytic effect, further improving the catalytic activity in the co-oxidation reaction of macromolecular aldehydes / olefins.

[0069] The inventors further found that for the peak separation results of the UV-Vis spectrum of the composite catalytic material at 460 to 740 nm, as the peak area (A 1 ) accounts for the total peak area (A) in the wavelength range of 460 to 740 nm 2 ) ratio, the catalytic performance of the composite catalytic material showed a downward trend, and when the peak area (A 1 ) accounts for the total peak area (A) in the wavelength range of 460 to 740 nm 2 ) ratio (i.e. A 0 ) is controlled to any value between 10 and 20%, the composite catalytic material exhibits ideal catalytic activity in the co-oxidation reaction of cyclooctene and isobutyraldehyde.

[0070] In the present disclosure, the peak separation of UV-Vis spectrum may be performed using conventional peak separation methods and software in the art.

[0071] In a preferred embodiment, A 0 The composite catalytic material in this embodiment has higher catalytic activity, higher cyclooctene conversion rate and higher epoxycyclooctene selectivity.

[0072] In one embodiment, the skeleton heteroatom molecular sieve in the composite catalytic material is one or more of MFI structure molecular sieve (such as S-1), MEL structure molecular sieve (such as S-2), BEA structure molecular sieve (such as Beta), MWW structure molecular sieve (such as MCM-22), two-dimensional hexagonal structure molecular sieve (such as MCM-41, SBA-15), MOR structure molecular sieve (such as MOR), TUN structure molecular sieve (such as TUN) and silicon molecular sieves of other structures (such as ZSM-48, MCM-48); preferably, it is one or more selected from MFI structure molecular sieve, MEL structure molecular sieve, BEA structure molecular sieve, MCM structure molecular sieve and SBA structure molecular sieve; further preferably, it is one or more of MFI structure molecular sieve, MEL structure molecular sieve and BEA structure molecular sieve, such as the silicon molecular sieve is one of S-1, S-2 and Beta; further preferably, it is an MFI structure molecular sieve, such as S-1.

[0073] In one embodiment, the metal element M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum, copper and gold.

[0074] In one embodiment, in the composite catalytic material, the molar ratio of the framework heteroatom element to the silicon element is (0.002-0.07):1, preferably (0.002-0.04):1;

[0075] The molar ratio of the metal M element to the silicon element is (0.001-0.2):1, preferably (0.002-0.18):1.

[0076] In one embodiment, the BET specific surface area of ​​the composite catalytic material is 400 to 800 m 2 / g, preferably 436 to 800 m 2 / g; total pore volume is 0.3-0.65mL / g, preferably 0.37-0.63mL / g; micropore volume is 0.1-0.19mL / g, preferably 0.11-0.18mL / ; mesopore volume is 0.2-0.46mL / g, preferably 0.22-0.46mL / g, the metal element M in the composite catalytic material exists in the form of metal nanoparticles, and the average particle size of the metal nanoparticles is 0.5-10nm, preferably 0.5-8nm. The composite catalytic material disclosed in the present invention has a multi-level pore structure, which is conducive to catalyzing reaction substrates of different sizes, especially catalyzing the reaction of macromolecular substrates.

[0077] The second aspect of the present disclosure provides a method for preparing a composite catalytic material of metal oxide nanoparticles and molecular sieves, comprising the following steps:

[0078] S1, mixing a template, a silicon source, a framework heteroatom precursor, water, a metal M precursor, a dendrimer and a silanization agent to obtain a reaction mixture;

[0079] S2, subjecting the reaction mixture to hydrothermal crystallization and calcination treatments;

[0080] The heteroatom element Q contained in the skeleton heteroatom precursor is selected from one of titanium, boron, zirconium, tin, aluminum, phosphorus and germanium; and the silanization agent contains at least one coordination group complexed with the metal element M.

[0081] The present disclosure introduces heteroatom precursors into the reaction mixture for synthesizing molecular sieves, and the heteroatom mainly enters the molecular sieve framework during crystallization. The present disclosure also introduces metal element precursors, dendritic macromolecules and silanization agents into the reaction mixture. On the one hand, metal ions are complexed with groups such as amine groups contained in the dendritic macromolecules to achieve the effect of dispersing and stabilizing metals; at the same time, at least one coordination group (such as amine groups, thiol groups, oxygen-containing coordination groups, etc.) carried by the silanization agent can also be complexed with metal ions to achieve the effect of fixing and dispersing metals, so that the metal oxide nanoparticles in the molecular sieve channels obtained after hydrothermal crystallization and calcination have high dispersion; on the other hand, the alkyl chain of the silanization agent also ensures the realization of the molecular sieve support layer expansion effect of the synthesized composite catalytic material, and the molecular volume of the dendritic macromolecule is very large, which can play a good role in supporting layer isolation during the crystallization of the molecular sieve. So that a skeleton heteroatom molecular sieve with a multi-level pore structure is finally prepared, and the metal M oxide nanoparticles can also be evenly dispersed in the mesoporous channels of the multi-level pore skeleton heteroatom molecular sieve.

[0082] In one embodiment, in step S1, SiO 2The molar ratio of the silicon source in terms of the silicon source: the template agent: the skeleton heteroatom precursor in terms of the heteroatom element Q: water: the metal element M: the silanization agent is 1: (0.005-1): (0.002-0.07): (10-80): (0.001-0.2): (0.025-0.5), preferably 1: (0.005-1): (0.002-0.04): (10-80): (0.002-0.18): (0.025-0.3); the mass of the dendritic macromolecule is 10 times that of the SiO 2 The ratio of the amount of the silicon source is (0.01-3):1, preferably (0.05-2):1.

[0083] Specifically, the water used in step S1 can be water commonly used in synthesizing molecular sieves. In order to avoid the introduction of heteroatoms, deionized water is preferred.

[0084] In a preferred embodiment, step S1 comprises the following steps:

[0085] a. mixing a template, a silicon source, a framework heteroatom precursor and water to obtain a silicon hydrolysis solution;

[0086] b. adding the dendritic macromolecule to the aqueous solution of the metal M precursor to obtain a first mixed material; and mixing the first mixed material with the hydrolyzed solution of silicon to obtain a second mixed material;

[0087] c. adding a silanization agent to the second mixed material, and mixing to obtain the reaction mixture;

[0088] Preferably, the mixing conditions in step c include: stirring at 20-80° C. for 0.5-2 hours.

[0089] In one embodiment, the silicon source is selected from at least one of organic silicone grease, solid silica gel, white carbon black and silica sol; preferably, it is selected from at least one of organic silicone grease, solid silica gel and white carbon black;

[0090] More preferably, the organic silicone grease has the general formula of the structure shown in the following formula (A):

[0091]

[0092] Where R a , R b , R c , R d Each is independently selected from an alkyl group having 1 to 6 carbon atoms, wherein the alkyl group is a branched or straight chain alkyl group; preferably, R a , R b , R c , R dEach is independently selected from a straight-chain alkyl group having 1 to 4 carbon atoms or a branched-chain alkyl group having 3 to 4 carbon atoms; further preferably, the R a , R b , R c , R d Each is independently selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl or tert-butyl.

[0093] In a preferred embodiment, the organic silicone grease is selected from one or more of tetramethyl silicate, tetraethyl silicate, tetrabutyl silicate and dimethyl diethyl silicone grease.

[0094] According to the present disclosure, in step S1, the template agent is an organic base, preferably at least one selected from quaternary ammonium base, aliphatic amine and aliphatic alcohol amine. The quaternary ammonium base can be an organic quaternary ammonium base; the aliphatic amine can be NH 3 A compound formed by replacing at least one hydrogen in the aliphatic hydrocarbon group (such as an alkyl group); the aliphatic alcohol amine can be various NH 3 A compound formed by replacing at least one hydrogen in a moiety with a hydroxyl-containing aliphatic group (such as an alkyl group).

[0095] In a further preferred embodiment, the template is at least one selected from quaternary ammonium bases having a structure represented by the following formula (B):

[0096] Where R 1 , R 2 , R 3 and R 4 are independently selected from an alkyl group having 1 to 4 carbon atoms, preferably a straight-chain alkyl group having 1 to 4 carbon atoms and a branched-chain alkyl group having 3 to 4 carbon atoms, more preferably R 1 , R 2 , R 3 and R 4 Each of the following is selected from one of methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl and tert-butyl.

[0097] In a preferred embodiment, the molecular sieve in the composite catalyst material is an MFI type molecular sieve, and the template agent is tetrapropylammonium hydroxide or a mixture of tetrapropylammonium hydroxide and one or more selected from tetrapropylammonium chloride and tetrapropylammonium bromide; or

[0098] In another preferred embodiment, the molecular sieve in the composite catalyst material is a MEL type molecular sieve, and the template agent is tetrabutylammonium hydroxide or a mixture of tetrabutylammonium hydroxide and one or more selected from tetrabutylammonium chloride and tetrabutylammonium bromide; or

[0099] In another preferred embodiment, the molecular sieve in the composite catalyst material is a Beta molecular sieve, and the template is tetraethylammonium hydroxide or a mixture of tetraethylammonium hydroxide and one or more selected from tetraethylammonium chloride and tetraethylammonium bromide.

[0100] In one embodiment, in step a, the silicon source is organic silicone grease, and after the template, organic silicone grease, skeleton heteroatom precursor and water are mixed, a hydrolysis and alcohol removal treatment is also performed to obtain the hydrolysis solution;

[0101] The conditions for the hydrolysis and alcohol removal treatment include: stirring hydrolysis at 0-95°C for 2-10 hours; preferably stirring hydrolysis at 50-95°C for 2-8 hours; wherein the hydrolysis and alcohol removal treatment makes the mass content of alcohol produced by hydrolysis of the organosilicon source in the hydrolysis solution less than 10 ppm.

[0102] According to the present disclosure, the optional range of types of the metal precursor is relatively wide, and any substance containing the metal element (such as a compound containing the metal element and / or a metal element) can achieve the purpose of the present disclosure.

[0103] In one embodiment, in step S1, the skeleton heteroatom precursor includes at least one of an organic skeleton heteroatom precursor and an inorganic skeleton heteroatom precursor; the inorganic skeleton heteroatom precursor is at least one of a chloride, a nitrate or a sulfate of a heteroatom element; the inorganic skeleton heteroatom precursor is an organic acid ester containing a heteroatom element, selected from at least one of the structures represented by the following formula (C):

[0104]

[0105] Where R 5 , R 6 , R 7 and R 8 are each selected from an alkyl group having 1 to 6 carbon atoms, preferably a straight-chain alkyl group having 1 to 4 carbon atoms and a branched-chain alkyl group having 3 to 6 carbon atoms, and more preferably R 5 , R 6 , R 7 and R 8 are independently selected from a straight chain alkyl group having 2 to 4 carbon atoms and a branched chain alkyl group having 2 to 4 carbon atoms;

[0106] Optionally, R 5 , R 6 , R 7 and R 8Each of the following groups is independently selected from one of methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, tert-butyl, isopentyl, hexyl and isohexyl; preferably each of the following groups is independently selected from one of ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl and tert-butyl.

[0107] In an optional embodiment, the skeleton heteroatom is titanium, and the skeleton heteroatom precursor is selected from one or more of titanium tetrachloride, titanium sulfate, titanium nitrate, tetraethyl titanate, tetrapropyl titanate and tetrabutyl titanate; in an optional embodiment, the skeleton heteroatom is boron, and the skeleton heteroatom precursor is selected from one or more of boric acid and borate; in an optional embodiment, the skeleton heteroatom is tin, and the skeleton heteroatom precursor is selected from one or more of tin halide, stannous halide, stannous sulfate, tin sulfate, stannate, stannate, tin nitrate, tin oxide and stannous oxide. In one optional embodiment, the framework heteroatom is aluminum, and the framework heteroatom precursor is selected from one or more of sodium aluminate, aluminum sulfate, boehmite, metallic aluminum, aluminum nitrate, aluminum isopropoxide and aluminum hydroxide; in one optional embodiment, the framework heteroatom is phosphorus, and the framework heteroatom precursor is selected from one or more of orthophosphoric acid, triethylphosphoric acid and metaphosphate; in one optional embodiment, the framework heteroatom is germanium, and the framework heteroatom precursor is selected from one or more of germanium oxide, germanium alkoxide (such as ethanol germanium, isopropoxide germanium), germanium chloride and sodium germanate.

[0108] In one embodiment, in step S1, the metal M precursor is one or more of an inorganic metal compound and an organic metal compound; the inorganic metal compound is a water-soluble inorganic salt of the metal element M; the water-soluble inorganic salt of the metal element M is selected from one or more of the chloride, hydrated chloride, sulfate, hydrated sulfate and nitrate of the metal element M; the organic metal compound is an organic ligand compound of the metal element M; preferably, the metal M precursor is a water-soluble inorganic salt of the metal element M;

[0109] The metal element M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum, copper and gold;

[0110] Preferably, the metal M precursor is an aqueous solution of a metal M precursor, and the molar ratio of the metal element M to water in the aqueous solution of the metal M precursor is 1:(50-500).

[0111] In one embodiment, in step S1, the dendritic macromolecule is selected from polyamide-amine macromolecules, phenylacetylene macromolecules, polyarylether macromolecules, and polyarylester macromolecules.

[0112] In a preferred embodiment, the dendritic macromolecule is selected from one or more of polyamide-amine macromolecules and polyarylether macromolecules;

[0113] Preferably, the polyamidoamine macromolecule is selected from one or more of the 2nd generation PAMAM with an ethylenediamine core, the 3rd generation PAMAM with an ethylenediamine core, and the 4th generation PAMAM with an ethylenediamine core;

[0114] The polyarylether macromolecule is selected from one or more of polyarylether nitrile, polyarylether sulfone and polyarylether ketone;

[0115] Preferably, the dendrimer has a weight average molecular weight of 4000 to 85000, an intrinsic viscosity at 30° C. of 0.025 to 0.045 dL / g, and a degree of branching of 4000 to 18000 (in terms of Mw).

[0116] In one embodiment, in step S1, the general formula of the silanization agent is R 9 Si(R 10 )(R 11 )R 12 , where R 9 , R 10 , R 11 , R 12 are independently halogen, alkyl, alkoxy, aromatic, mercapto or amine, and R 9 , R 10 , R 11 , R 12 At least one of them is an alkyl group, an alkoxy group, an aromatic group, a thiol group or an amine group; the number of carbon atoms of the alkyl group, the alkoxy group, the thiol group and the amine group is independently selected from any integer in the range of 1 to 18, preferably any integer in the range of 1 to 12; the number of carbon atoms of the aromatic group can be any integer in the range of 6 to 18, preferably any integer in the range of 6 to 12.

[0117] Preferably, the silanization agent is selected from one or more of dimethyldichlorosilane, N-phenyl-3-aminopropyltrimethoxysilane, phenyltrimethoxysilane, 1,7-dichlorooctylmethyltetrasiloxane, hexadecyltrimethoxysilane, octyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane; further preferably, it is at least one of N-phenyl-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane.

[0118] In the present disclosure, different silanization agents can be selected for different metal elements M. For example, when the metal element M is Co, the silanization agent is at least one of N-phenyl-3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane and N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane; when the metal element M is Au or Pt, the silanization agent is at least one of 3-mercaptopropyltrimethoxysilane and 3-mercaptopropyltriethoxysilane.

[0119] In one embodiment, in step S2, the conditions of the hydrothermal crystallization treatment include: being carried out under autogenous pressure, the hydrothermal crystallization time is 0.5 to 10 days, and the hydrothermal crystallization temperature is 110 to 200°C; preferably, the hydrothermal crystallization time is 0.5 to 5 days, and the hydrothermal crystallization temperature is 150 to 200°C.

[0120] In one embodiment, in step S2, the conditions of the calcination treatment include: a calcination temperature of 400-900° C., and a calcination time of 1-16 hours; preferably, the calcination temperature is 400-800° C., and the calcination time is 2-8 hours.

[0121] The third aspect of the present disclosure provides a composite catalytic material of metal oxide nanoparticles and molecular sieves prepared according to the method described in the second aspect of the present disclosure.

[0122] The fourth aspect of the present disclosure provides the use of the metal oxide nanoparticles and molecular sieve composite catalytic material described in the first aspect or the third aspect of the present disclosure in catalyzing the co-oxidation reaction of macromolecular aldehydes / olefins; preferably, the use in catalyzing the co-oxidation reaction of cyclooctene and isobutyraldehyde.

[0123] In a specific embodiment, the reaction conditions in the use of catalyzing the co-oxidation reaction of cyclooctene and isobutyraldehyde include: the molar ratio of isobutyraldehyde to cyclooctene is 2 to 8:1, the weight ratio of the metal nanoparticles to the molecular sieve composite catalytic material is 5 to 20 weight % based on the total weight of isobutyraldehyde and cyclooctene; the oxygen pressure is 0.1 to 2 MPa, the reaction temperature is 20 to 120° C., and the reaction time is 2 to 48 hours. Optionally, the reaction is carried out in a slurry bed reactor.

[0124] When the composite catalytic material is used to catalyze the co-oxidation reaction of cyclooctene and isobutyraldehyde, the conversion rate of cyclooctene is not less than 75 mol %, the selectivity of the target product epoxy cyclooctene is not less than 85 mol %, and the conversion rate of isobutyraldehyde is not less than 98 mol %.

[0125] In the present disclosure, the UV-visible diffuse reflectance spectrum (UV-vis) of the sample solid was measured on a SHIMADZU UV-3100 UV-visible spectrometer in the test range of 400 to 4000 cm -1 .

[0126] The X-ray diffraction (XRD) crystal phase diagram of the sample was measured on a Siemens D5005 X-ray diffractometer, the radiation source was Kα (Cu), and the test range 2θ was 0.5-70°.

[0127] The SEM images of the samples were obtained on a Hitachi S4800 high-resolution cold field emission scanning electron microscope.

[0128] The TEM images of the samples were obtained on a FEI Tecnai G2F20S-TWIN transmission electron microscope. The average particle size of the metal oxide nanoparticles was obtained based on TEM electron microscope testing.

[0129] The total specific surface area and total pore volume of the sample were measured on a Micromeritics ASAP245 static nitrogen adsorption instrument according to the ASTM D4222-98 standard method. The adsorption isotherm and desorption isotherm of low-temperature nitrogen adsorption of the sample were measured according to the ASTM D4222-98 standard method.

[0130] In the following examples, among the dendritic macromolecules used, PAMAM is a polyamide-amine type dendritic macromolecule purchased from Inokai, wherein PAMAM (ethylenediamine core, 2nd generation) has a molecular weight of 9858, an intrinsic viscosity at 30°C of 0.037 dL / g, and a degree of branching of 4300 (Mw); PAMAM (ethylenediamine core, 3rd generation) has a molecular weight of 9858, an intrinsic viscosity at 30°C of 0.035 dL / g, and a degree of branching of 5200 (Mw); PAMAM (ethylenediamine core, 4th generation) has a molecular weight of 26000, an intrinsic viscosity at 30°C of 0.031 dL / g, and a degree of branching of 16000 (Mw); polyarylether macromolecules purchased from Inokai, polyarylether nitrile molecular weight of 83000. The weight average molecular weight and degree of branching of the dendritic macromolecules in the present disclosure are obtained by reagent labels; the intrinsic viscosity at 30°C is obtained by Ubbelohde viscometer and conventional determination methods.

[0131] Example 1

[0132] (1) 1.63 g of 25.05 wt % tetrapropylammonium hydroxide (TPAOH, 0.002 mol) aqueous solution, 20.8 g of tetraethyl silicate (0.1 mol), 0.170 g of tetrabutyl titanate (0.0005 mol) and 9 g (0.5 mol) of water were added to a 500 mL beaker in sequence, and the mixture was placed on a magnetic stirrer with heating and stirring functions to mix evenly, and stirred at 80° C. for 2 hours, and the evaporated water was replenished regularly to obtain a colorless and transparent silica gel solution;

[0133] (2) 0.3 g of cobalt nitrate hexahydrate (0.001 mol) and 1.8 g of water (0.1 mol) were stirred evenly, and then 0.06 g of PAMAM (ethylenediamine core, second generation) was added, and the aqueous solution of cobalt was mixed with the hydrolyzed solution of silicon obtained in step (1);

[0134] (3) Add 0.64 g of N-phenyl-3-aminopropyltrimethoxysilane (PHAPTMS, 0.0025 mol) to the mixture of step (2) and stir for 0.5 hour;

[0135] (4) The mixture obtained in step (2) is transferred to a stainless steel closed reactor and crystallized at a constant temperature of 170° C. for 28 hours to obtain a sample. The obtained sample is filtered, washed, dried at 120° C. for 6 hours, and then calcined at 600° C. in a muffle furnace for 6 hours to obtain a metal nanoparticle and molecular sieve composite catalytic material product, which is recorded as CAT-1.

[0136] The UV-Vis spectrum of CAT-1 is as follows Figure 1 As shown, Figure 1 The peak near 220nm in the spectrum represents titanium species; the UV-Vis peak analysis is shown in Figure 2 shown. Figure 2 The peaks in the range of 460 to 740 nm indicate that there is an interaction between the Co species and the Si skeleton. The peak at 520 nm represents the species inside the cobalt oxide nanoparticles, the peak at 590 nm represents the species at the interface between the cobalt oxide nanoparticles and the silicon skeleton, and the peak at 660 nm represents the species on the surface of the cobalt oxide nanoparticles (active centers). The XRD spectrum of CAT-1 is shown in Figure 1. Figure 3 As shown in Figure 1, XRD analysis shows that it has an MFI structure. The SEM spectrum of CAT-1 is shown in Figure 1. Figure 4 The BET specific surface area, total pore volume, micropore volume, mesopore volume and average particle size of the metal nanoparticles contained in CAT-1 are listed in Table 2.

[0137] Comparative Example 1

[0138] This comparative example was prepared according to the method of Example 1, except that no silanization agent was added. The proportions, synthesis conditions and results are shown in Table 1. Other conditions and operations were similar to those of Example 1, and the obtained product was recorded as D-1.

[0139] Comparative Example 2

[0140] Under stirring conditions, ethyl orthosilicate, tetrapropylammonium hydroxide, cobalt nitrate hexahydrate and deionized water were mixed and stirred at 50°C for 2h to obtain a molar ratio of SiO 2 :Structure directing agent: TiO 2 :Co:H 2O=1:0.2:0.03:0.01:30 first mixture; then SiO 2 : silanization agent = 1:0.025 molar ratio, PHAPTMS was added to the above first mixture, and after continuing to stir for 0.5h, the obtained second mixture was transferred to a pressure-resistant stainless steel reactor; heated to 170°C and crystallized under autogenous pressure for 8h under stirring conditions. After the stainless steel pressure-resistant reactor cooled to room temperature, the crystallized product was recovered, dried at 110°C for 6h, and then calcined at 550°C for 4h to obtain a multi-level porous molecular sieve encapsulating cobalt. The obtained product was recorded as D-2.

[0141] Comparative Example 3

[0142] Under stirring conditions, tetraethyl orthosilicate, tetrapropylammonium hydroxide, tetrabutyl titanate, cobalt acetylacetonate and deionized water were mixed and stirred at 80°C for 8h to obtain a molar ratio of SiO 2 :Structure directing agent: TiO 2 :Co:H 2 O=1:0.2:0.025:0.01:50 first mixture; then SiO 2 : silanization agent = 1:0.12 molar ratio, phenyltriethoxysilane was added to the above first mixture, and after continuing to stir for 2 hours, the obtained second mixture was transferred to a pressure-resistant stainless steel reactor; heated to 170°C and crystallized under autogenous pressure for 8 hours under stirring conditions. After the stainless steel pressure-resistant reactor cooled to room temperature, the crystallized product was recovered, dried at 110°C for 6 hours, and then calcined at 550°C for 4 hours to obtain a multi-level porous titanium silicon molecular sieve encapsulating cobalt. The obtained product was recorded as D-3.

[0143] Embodiments 2 to 9

[0144] The corresponding products CAT-2 to CAT-9 were prepared according to the method of Example 1, and their proportions, synthesis conditions and results are shown in Table 1. Other conditions and operations are similar to those of Example 1.

[0145] Example 10

[0146] In this example, a cobalt-containing multi-level porous β molecular sieve was prepared, referring to the method of Example 1, but the ratio and template agent were changed, and the template agent used was tetraethylammonium hydroxide (TEAOH), and the ratio, synthesis conditions and results are shown in Table 1. The obtained product was recorded as CAT-10.

[0147] Embodiment 11

[0148] In this example, a cobalt-containing multi-level porous MEL molecular sieve was prepared, referring to the method of Example 1, but the ratio and template agent were changed, and the template agent used was tetrabutylammonium hydroxide (TBAOH). The ratio, synthesis conditions and results are shown in Table 1. The obtained product was recorded as C-11.

[0149] Example 12

[0150] The corresponding product was prepared according to the method of Example 1, and its ratio, synthesis conditions and results are shown in Table 1. Other conditions and operations refer to Example 1, and the obtained product is recorded as CAT-12. The hydrothermal crystallization temperature is 120°C, the hydrothermal crystallization time is 7 days, the calcination temperature is 850°C, and the calcination time is 9 hours.

[0151] Embodiment 13

[0152] A multi-level porous MFI molecular sieve containing nickel nanoparticles was prepared, wherein the framework heteroatom was tin, according to the method of Example 1. The proportions, synthesis conditions and results are shown in Table 1. The obtained product was recorded as CAT-13.

[0153] The BET specific surface area, total pore volume, micropore volume and mesopore volume of the products obtained in the above examples and comparative examples, as well as the average particle size of the metal nanoparticles in the products are listed in Table 2 below.

[0154] Table 1

[0155]

[0156] m / 10×c*, where m represents the mass of the dendrimer, and c represents the mass of SiO 2 Measure the amount of silicon source substance.

[0157] In Table 1, cobalt nitrate is cobalt nitrate hexahydrate; TPAOH is tetrapropylammonium hydroxide, TPABr is tetrapropylammonium bromide, TBAOH is tetrabutylammonium hydroxide, TEAOH is tetraethylammonium hydroxide; PHAPTMS is N-phenyl-3-aminopropyltrimethoxysilane, APTES is 3-aminopropyltriethoxysilane, KH792 is silane coupling agent kh792 (bisamino functional group silane, N-aminoethyl-γ-aminopropyltrimethoxysilane). The reagents used in the present disclosure can be obtained through conventional purchasing channels.

[0158] Table 2

[0159]

[0160] Among them, pores with a diameter less than 2nm are micropores, and pores with a diameter between 2 and 50nm are mesopores.

[0161] According to Table 2, compared with D-1 prepared in Comparative Example 1 (without adding a silanizing agent), the products CAT-1 to CAT-13 obtained in Examples 1 to 13 of the present disclosure have a higher mesoporous volume by adding a silanizing agent during the preparation process, indicating that the method provided by the present disclosure can effectively expand the pores of the molecular sieve. The metal nanoparticles of the products CAT-1 to CAT-13 obtained in Examples 1 to 13 of the present disclosure have a smaller particle size, indicating that the degree of aggregation of the metal nanoparticles is lower and the dispersion is higher.

[0162] Test Case

[0163] This test example illustrates the reaction effects of the samples prepared in the examples and comparative examples provided in the present disclosure for the co-oxidation reaction of cyclooctene and isobutyraldehyde.

[0164] The reagents used in this test example are all commercially available chemically pure reagents, and the concentrations of various substances after the reaction are quantitatively analyzed using gas chromatography. The gas chromatograph used is a 6890 gas chromatograph produced by Agilent; the analytical chromatographic column used is an HP-5 column.

[0165] The conversion rate of cyclooctene, the conversion rate of isobutyraldehyde and the selectivity of cyclooctene oxide in the examples are calculated according to the following formulas (2)-(4):

[0166]

[0167]

[0168]

[0169] The samples prepared in the comparative example and the example were taken respectively, and were uniformly stirred and mixed in a slurry bed according to a molar ratio of isobutyraldehyde:cyclooctene=3:1. The slurry bed closed system was connected to a normal pressure pure oxygen balloon as an oxygen source, the oxygen pressure was 0.1MPa, the amount of cyclooctene was 1mmol, the amount of catalyst was 50mg, and the amount of solvent acetonitrile was 2.5mL. The reaction was stable at 25°C for 6 hours, and the samples were taken for analysis. The results are shown in Table 3.

[0170] Table 3

[0171]

[0172]

[0173] As can be seen from Table 3, compared with the products D-1 to D-3 obtained in Comparative Examples 1 to 3, the composite catalytic materials CAT-1 to CAT-13 prepared in Examples 1 to 13 of the present disclosure have an A 0When CAT-1 to CAT-13 are used for the co-oxidation reaction of cyclooctene and isobutyraldehyde, they have higher catalytic activity and can obtain higher cyclooctene conversion rate, isobutyraldehyde conversion rate and epoxycyclooctene selectivity.

[0174] Comparing CAT-1 to CAT-13, it can be seen that compared with CAT-12, the A 0 When the content is between 12% and 18%, CAT-1 to CAT-11 and CAT-13 have higher catalytic activity and can obtain higher cyclooctene conversion rate, isobutyraldehyde conversion rate and epoxycyclooctene selectivity.

[0175] The preferred embodiments of the present disclosure are described in detail above in conjunction with the accompanying drawings; however, the present disclosure is not limited to the specific details in the above embodiments. Within the technical concept of the present disclosure, a variety of simple modifications can be made to the technical solution of the present disclosure, and these simple modifications all fall within the protection scope of the present disclosure.

[0176] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present disclosure will not further describe various possible combinations.

[0177] In addition, various embodiments of the present disclosure may be arbitrarily combined, and as long as they do not violate the concept of the present disclosure, they should also be regarded as the contents disclosed by the present disclosure.

Claims

1. A metal nanoparticle and molecular sieve composite catalytic material, characterized in that: It comprises a framework heteroatom molecular sieve and a metal element M dispersed in the crystal of the molecular sieve, wherein the metal element M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum, copper and gold; the framework heteroatom molecular sieve is a molecular sieve in which at least part of the silicon in the framework of the all-silicon molecular sieve is replaced by a heteroatom element Q, wherein the heteroatom element Q is selected from one or more of titanium, zirconium, tin and germanium; The composite catalytic material has the following UV-Vis characteristics: In the peak separation result of the wavelength of 460-740 nm in the UV-Vis spectrum of the composite catalytic material, the peak area of ​​the spectrum peak in the wavelength range of 460-540 nm is recorded as A1, and the total peak area in the wavelength range of 460-740 nm in the UV-Vis spectrum of the composite catalytic material is recorded as A2. A0 defined by the following formula (1) is any value between 10% and 20%; A0=A1 / A2 (1); The metal nanoparticle and molecular sieve composite catalytic material is prepared by a method comprising the following steps: S1, mixing a template, a silicon source, a framework heteroatom precursor, water, a metal M precursor, a dendrimer and a silanization agent to obtain a reaction mixture; S2, subjecting the reaction mixture to hydrothermal crystallization and calcination treatments; Wherein, the skeleton heteroatom precursor comprises the heteroatom element Q; and the silanization agent comprises at least one coordination group complexed with the metal element M.

2. The composite catalytic material according to claim 1, characterized in that: The A0 is any value between 12% and 18%.

3. The composite catalytic material according to claim 1, characterized in that: The framework heteroatom molecular sieve in the composite catalytic material is at least one of an MFI structure molecular sieve, a MEL structure molecular sieve, a BEA structure molecular sieve, an MWW structure molecular sieve, a two-dimensional hexagonal structure molecular sieve, a MOR structure molecular sieve and a TUN structure molecular sieve.

4. The composite catalytic material according to claim 3, characterized in that: The framework heteroatom molecular sieve in the composite catalytic material is selected from one or more of the MFI structure molecular sieve, MEL structure molecular sieve, BEA structure molecular sieve, MCM structure molecular sieve and SBA structure molecular sieve.

5. The composite catalytic material according to claim 4, characterized in that: The framework heteroatom molecular sieve in the composite catalytic material is selected from one or more of MFI structure molecular sieve, MEL structure molecular sieve and BEA structure molecular sieve.

6. The composite catalytic material according to claim 1, characterized in that: In the composite catalytic material, the molar ratio of the framework heteroatom element to the silicon element is (0.002-0.07):1; The molar ratio of metal M element to silicon element is (0.001~0.2):

1.

7. The composite catalytic material according to claim 6, characterized in that: In the composite catalytic material, the molar ratio of the framework heteroatom element to the silicon element is (0.002-0.04):1; The molar ratio of metal M element to silicon element is (0.002~0.18):

1.

8. The composite catalytic material according to claim 1, characterized in that: The BET specific surface area of ​​the composite catalytic material is 400-800 m 2 / g, the total pore volume is 0.3~0.65mL / g, the micropore volume is 0.1~0.19mL / g, the mesopore volume is 0.2~0.46mL / g, and the metal element M in the composite catalytic material exists in the form of metal nanoparticles, and the average particle size of the metal nanoparticles is 0.5~10nm.

9. The composite catalytic material according to claim 1, characterized in that: In step S1, the molar ratio of the silicon source calculated as SiO2: the template: the skeleton heteroatom precursor calculated as the heteroatom element Q: water: the metal element M: the silanization agent is 1: (0.005~1): (0.002~0.07): (10~80): (0.001~0.2): (0.025~0.5); the ratio of the mass of the dendritic macromolecule to 10 times the amount of the silicon source calculated as SiO2 is (0.01~3):

1.

10. The composite catalytic material according to claim 9, characterized in that: In step S1, the molar ratio of the silicon source calculated as SiO2: the template: the skeleton heteroatom precursor calculated as the heteroatom element Q: water: the metal element M: the silanization agent is 1: (0.005~1): (0.002~0.04): (10~80): (0.002~0.18): (0.025~0.3); the ratio of the mass of the dendritic macromolecule to 10 times the amount of the silicon source calculated as SiO2 is (0.05~2):

1.

11. The composite catalytic material according to claim 1, characterized in that: Step S1 includes the following steps: a. mixing a template, a silicon source, a framework heteroatom precursor and water to obtain a silicon hydrolysis solution; b. adding the dendritic macromolecule to the aqueous solution of the metal M precursor to obtain a first mixed material; and mixing the first mixed material with the hydrolyzed solution of silicon to obtain a second mixed material; c. Adding a silanization agent into the second mixed material and mixing them to obtain the reaction mixture.

12. The composite catalytic material according to claim 11, characterized in that: The mixing conditions in step c include: stirring at 20-80° C. for 0.5-2 hours.

13. The composite catalytic material according to claim 1, characterized in that: The silicon source is selected from at least one of organic silicone grease, solid silica gel, white carbon black and silica sol.

14. The composite catalytic material according to claim 13, characterized in that: The silicon source is selected from at least one of organic silicone grease, solid silica gel and white carbon black.

15. The composite catalytic material according to claim 14, characterized in that: The silicon source is organic silicone grease, and the general formula of the organic silicone grease is the structure shown in the following formula (A): (A); Where R a , R b , R c , R d Each is independently selected from an alkyl group having 1 to 6 carbon atoms, and the alkyl group is a branched or straight chain alkyl group.

16. The composite catalytic material according to claim 15, characterized in that: In formula (A), R a , R b , R c , R d Each is independently selected from a straight-chain alkyl group having 1 to 4 carbon atoms or a branched-chain alkyl group having 3 to 4 carbon atoms.

17. The composite catalytic material according to claim 16, characterized in that: The R a , R b , R c , R d Each is independently selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl or tert-butyl.

18. The composite catalytic material according to claim 17, characterized in that: The organic silicone grease is selected from one or more of tetramethyl silicate, tetraethyl silicate, tetrabutyl silicate and dimethyl diethyl silicone grease.

19. The composite catalytic material according to claim 1, characterized in that: The template agent is an organic base.

20. The composite catalytic material according to claim 19, characterized in that The template agent is selected from at least one of quaternary ammonium base, aliphatic amine and aliphatic alcohol amine.

21. The composite catalytic material according to claim 20, characterized in that: The template is selected from at least one quaternary ammonium base having a structure represented by the following formula (B): (B); wherein R1, R2, R3 and R4 are independently selected from an alkyl group having 1 to 4 carbon atoms.

22. The composite catalytic material according to claim 21, characterized in that In formula (B), R1, R2, R3 and R4 are selected from a linear alkyl group having 1 to 4 carbon atoms and a branched alkyl group having 3 to 4 carbon atoms.

23. The composite catalytic material according to claim 22, characterized in that: In formula (B), R1, R2, R3 and R4 are each selected from one of methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl and tert-butyl.

24. The composite catalytic material according to claim 1, characterized in that The molecular sieve in the composite catalyst material is an MFI molecular sieve, and the template agent is tetrapropylammonium hydroxide or a mixture of tetrapropylammonium hydroxide and one or more selected from tetrapropylammonium chloride and tetrapropylammonium bromide; or The molecular sieve in the composite catalytic material is a MEL type molecular sieve, and the template agent is tetrabutylammonium hydroxide or a mixture of tetrabutylammonium hydroxide and one or more selected from tetrabutylammonium chloride and tetrabutylammonium bromide; or The molecular sieve in the composite catalytic material is a Beta molecular sieve, and the template agent is tetraethylammonium hydroxide or a mixture of tetraethylammonium hydroxide and one or more selected from tetraethylammonium chloride and tetraethylammonium bromide.

25. The composite catalytic material according to claim 11, characterized in that: In step a, the silicon source is organic silicone grease, and after the template, organic silicone grease, skeleton heteroatom precursor and water are mixed, a hydrolysis and alcohol removal treatment is also performed to obtain the hydrolysis solution; The conditions of the hydrolysis and alcohol removal treatment include: stirring and hydrolyzing at 0-95° C. for 2-10 hours.

26. The composite catalytic material according to claim 25, characterized in that The conditions of the hydrolysis and alcohol removal treatment include: stirring and hydrolyzing at 50-95° C. for 2-8 hours.

27. The composite catalytic material according to claim 1, characterized in that In step S1, the skeleton heteroatom precursor includes at least one of an organic skeleton heteroatom precursor and an inorganic skeleton heteroatom precursor; the inorganic skeleton heteroatom precursor is at least one selected from chlorides, nitrates and sulfates of heteroatom element Q; the organic skeleton heteroatom precursor is an organic acid ester containing heteroatom element Q, selected from at least one of the structures shown in the following formula (C): (C); wherein R5, R6, R7 and R8 are independently selected from an alkyl group having 1 to 6 carbon atoms.

28. The composite catalytic material according to claim 27, characterized in that In formula (C), R5, R6, R7 and R8 are independently selected from a linear alkyl group having 1 to 4 carbon atoms and a branched alkyl group having 3 to 6 carbon atoms.

29. The composite catalytic material according to claim 28, characterized in that In formula (C), R5, R6, R7 and R8 are independently selected from a linear alkyl group having 2 to 4 carbon atoms and a branched alkyl group having 2 to 4 carbon atoms.

30. The composite catalytic material according to claim 27, characterized in that In formula (C), R5, R6, R7 and R8 are independently selected from one of methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, tert-butyl, isopentyl, hexyl and isohexyl.

31. The composite catalytic material according to claim 30, characterized in that In formula (C), R5, R6, R7 and R8 are each independently selected from one of ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl and tert-butyl.

32. The composite catalytic material according to claim 1, characterized in that When the skeleton heteroatom is titanium, the skeleton heteroatom precursor is selected from one or more of titanium tetrachloride, titanium sulfate, titanium nitrate, tetraethyl titanate, tetrapropyl titanate and tetrabutyl titanate; when the skeleton heteroatom is tin, the skeleton heteroatom precursor is selected from one or more of tin halide, stannous halide, stannous sulfate, tin sulfate, stannate, stannate, tin nitrate, tin oxide and stannous oxide; when the skeleton heteroatom is germanium, the skeleton heteroatom precursor is selected from one or more of germanium oxide, germanium alkoxide, germanium chloride and sodium germanate.

33. The composite catalytic material according to claim 1, characterized in that In step S1, the metal M precursor is one or more of an inorganic metal compound and an organic metal compound; the inorganic metal compound is a water-soluble inorganic salt of the metal element M; the water-soluble inorganic salt of the metal element M is selected from one or more of the chloride, hydrated chloride, sulfate, hydrated sulfate and nitrate of the metal element M; the organic metal compound is an organic ligand compound of the metal element M.

34. The composite catalytic material according to claim 33, characterized in that The metal M precursor is a water-soluble inorganic salt of the metal element M.

35. The composite catalytic material according to claim 11, characterized in that The molar ratio of the metal element M to water in the aqueous solution of the metal M precursor is 1:(50-500).

36. The composite catalytic material according to claim 1, characterized in that In step S1, the dendritic macromolecules are selected from one or more of polyamide-amine macromolecules and polyarylether macromolecules.

37. The composite catalytic material according to claim 36, characterized in that The polyamide-amine macromolecule is selected from one or more of the second generation PAMAM with an ethylenediamine core, the third generation PAMAM with an ethylenediamine core, and the fourth generation PAMAM with an ethylenediamine core; The polyarylether macromolecule is selected from one or more of polyarylether nitrile, polyarylether sulfone and polyarylether ketone.

38. The composite catalytic material according to claim 36, characterized in that The dendritic macromolecule has a weight average molecular weight of 4000-85000, an intrinsic viscosity of 0.025-0.045 dL / g at 30° C., and a branching degree of 4000-18000.

39. The composite catalytic material according to claim 1, characterized in that In step S1, the general formula of the silanization agent is R9Si(R 10 )(R 11 )R 12 , where R9, R 10 , R 11 , R 12 are independently halogen, alkyl, alkoxy, aromatic, mercapto or amine, and R9, R 10 , R 11 , R 12 At least one of them is an alkyl group, an alkoxy group, an aromatic group, a thiol group or an amino group; the number of carbon atoms of the alkyl group, the alkoxy group, the thiol group and the amino group is independently selected from any integer in the range of 1 to 18, and the number of carbon atoms of the aromatic group is any integer in the range of 6 to 18.

40. The composite catalytic material according to claim 39, characterized in that The silanization agent is selected from one or more of dimethyldichlorosilane, N-phenyl-3-aminopropyltrimethoxysilane, phenyltrimethoxysilane, hexadecyltrimethoxysilane, octyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane.

41. The composite catalytic material according to claim 40, characterized in that The silanization agent is selected from at least one of N-phenyl-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane.

42. The composite catalytic material according to claim 1, characterized in that In step S2, the conditions of the hydrothermal crystallization treatment include: being carried out under autogenous pressure, the hydrothermal crystallization time is 0.5 to 10 days, and the hydrothermal crystallization temperature is 110 to 200°C; The conditions of the calcination treatment include: a calcination temperature of 400-900° C. and a calcination time of 1-16 hours.

43. The composite catalytic material according to claim 42, characterized in that In step S2, the conditions of the hydrothermal crystallization treatment include: the hydrothermal crystallization time is 0.5 to 5 days, and the hydrothermal crystallization temperature is 150 to 200°C; The conditions of the calcination treatment include: a calcination temperature of 400-800° C. and a calcination time of 2-8 hours.

44. Use of the metal nanoparticle and molecular sieve composite catalytic material according to any one of claims 1 to 43 in catalyzing the co-oxidation reaction of aldehydes and olefins.

45. The use according to claim 44, characterized in that The use includes use of the metal nanoparticles and molecular sieve composite catalytic material in catalyzing the co-oxidation reaction of cyclooctene and isobutyraldehyde.

Citation Information

Patent Citations

  • Hierarchical pore titanium silicalite molecular sieve for packaging active metal and preparation method thereof

    CN111847471A

  • High-dispersion dual-functional catalyst for hydrogenating and deoxidizing phenol and preparation method of catalyst

    CN102698788A

  • All-silicon molecular sieve and synthetic method thereof

    CN104556087A

  • ZSM-12 molecular sieve supported high-dispersion Pt catalyst and preparation method thereof

    CN109772443A

  • Packaged platinum group sub-nanometallic supported porous-grade titanium silicon molecular sieve catalyst as well as preparation and application thereof

    CN109999902A