Construction method of widening the concrete roadbed
By using layered backfilling and a specific filler formulation, the problem of concrete pavement cracking caused by the differential settlement between the old and new roadbeds was solved, noise pollution was reduced, and efficient roadbed widening construction was achieved.
Patent Information
- Application Number
- CN202310220827.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-09
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-03-09
AI Technical Summary
During the widening of existing concrete roadbeds, the settlement difference between the old and new roadbeds makes the concrete pavement prone to cracking, and the compaction machine is noisy and inefficient.
The construction method of layered backfilling is adopted, using fillers with specific formulas (first filler, second filler, third filler, and fourth filler) in conjunction with compaction process to form lower embankment, upper embankment, lower subgrade, and upper subgrade. The expansion agent is used to slowly expand in the later stage of construction to increase the density and reduce settlement.
It improved the compactness and stability of the roadbed, reduced settlement, reduced noise pollution, shortened the construction period, and prevented road surface cracking.
Smart Images

Figure GDA0005040296730000081 
Figure GDA0005040296730000091
Abstract
Description
Technical Field
[0001] The invention relates to the field of road construction, in particular to a construction method for widening a concrete road subgrade. Background Art
[0002] Roads are one of the basic transportation facilities and play an important role in carrying vehicles. With urban planning, most of the roads in the city have been formed, but with the development of the city, the demand for roads will change. Some roads need to be widened to meet the needs of larger traffic flow.
[0003] An essential step in road widening is to widen the roadbed. The roadbed is the main foundation for bearing concrete pavement. The surface of concrete pavement is flat and the driving comfort is high. However, concrete pavement is a rigid pavement with poor crack resistance. Ordinary roadbeds are mainly composed of soil. Although the roadbed will be compacted during roadbed construction, the compaction degree cannot reach 100%. Due to the long-term use of old roads, the old roadbed has completed the settlement due to the weight of the road and the weight of the vehicle. The density is very high and the settlement amplitude in the later period is low. However, the new roadbed has not been affected by the weight of the road and the weight of the vehicle, and the density will always be lower than that of the old roadbed. Therefore, in the process of road use, the new roadbed will always have a greater settlement, resulting in a difference in settlement between the new and old roadbeds. The disadvantage of poor crack resistance of concrete pavement will undoubtedly magnify the problem of the difference in settlement between the new and old roadbeds. However, when the new roadbed settles more, the concrete pavement is prone to cracking. Therefore, when constructing a new roadbed, it is necessary to increase the density of the new roadbed as much as possible.
[0004] Usually, in order to improve the density of the new roadbed, a compactor is used to compact the roadbed. However, the compactor compacts the soil by impacting the roadbed, so a lot of noise will be generated during the compaction process. In addition, the area that the compactor's punch can act on is small. It takes a huge amount of time to compact a large area of roadbed, and the construction period is long. Therefore, there is still room for improvement. Summary of the invention
[0005] In order to shorten the construction period and reduce noise pollution, the present application provides a construction method for widening a concrete roadbed.
[0006] The present application provides a construction method for widening a concrete roadbed using the following technical solutions:
[0007] A construction method for widening a concrete roadbed comprises the following steps:
[0008] Step 1), surface excavation, specifically including:
[0009] Excavate and remove the surface structure in the widened area;
[0010] Step 2), excavating the roadbed foundation pit, specifically including:
[0011] Excavate the soil base of the widened area to form a roadbed foundation pit;
[0012] Step 3), layered backfilling and compaction, specifically including:
[0013] Backfilling the first filler material at the bottom of the foundation pit and compacting it to form a lower embankment, backfilling the second filler material on the lower embankment and compacting it to form an upper embankment, backfilling the third filler material on the upper embankment and compacting it to form a lower roadbed, backfilling the fourth filler material on the lower roadbed and compacting it to form an upper roadbed;
[0014] The lower embankment, upper embankment, lower roadbed and upper roadbed together constitute a roadbed;
[0015] The first filler includes a compound of sand and clay;
[0016] The second filler includes a mixture of sand, clay and crushed stone;
[0017] The third filler includes a compound of sand, clay and expansion agent;
[0018] The fourth filler comprises a compound of sand, clay, reinforcing fiber and cement powder.
[0019] By adopting the above technical scheme, through layered backfilling, the lower embankment, upper embankment, lower roadbed and upper roadbed are formed respectively, and each layer adopts a special filler formula so that each layer has different properties. Through the coordination of each layer, under the compaction process, a higher density can be achieved, the roadbed settlement is low, and it can cooperate well with the old roadbed, so that the concrete pavement is not easy to break due to the difference in settlement of the new and old roadbeds.
[0020] By compounding the first filler including sand and clay, the lower embankment is mainly formed by sand and clay. The addition of clay can improve the structural stability of the lower embankment, making it less likely to break, and it can also have a certain water retention capacity, making it less likely to dry out and crack. Since the lower embankment is far away from the road surface, it is not a main pressure-bearing structure and only needs to have appropriate stability and density.
[0021] The upper embankment is mainly formed of sand, clay and gravel by the compound of the second filler including sand, clay and gravel. The addition of gravel increases the upper limit of bearing pressure and the bearing strength of the roadbed. The addition of clay makes the gravel stably distributed in the upper embankment and has strong structural stability. In the process of compaction, the gravel can help improve the density of the upper embankment due to its rigidity and can provide a certain degree of water permeability, so that the drainage performance of the road is improved.
[0022] By compounding the third filler including sand, clay and expansion agent, the lower roadbed contains expansion material. The expansion agent slowly expands, and after the road is constructed, the soil can be continuously compacted through the expansion effect, so that the density of the lower roadbed is continuously improved, and the expansion of the lower roadbed will affect the upper roadbed and the upper embankment. Through the accumulation effect, the density of the upper roadbed can be continuously improved, and the settlement of the upper roadbed can be supplemented. Although the density of the roadbed cannot reach the optimal extremely high state during the roadbed construction, the expansion deformation of the lower roadbed can supplement the compression deformation of the upper roadbed, so that the road surface height maintains a relatively stable state, and is not prone to settlement and cracking. Since the lower roadbed acts on the upper embankment and the upper roadbed at the same time, the upper roadbed will not float due to excessive expansion, and the concrete pavement will not be affected.
[0023] By compounding the fourth filler including sand, clay, reinforcing fiber and cement powder, the roadbed contains fiber reinforcement, which makes the roadbed less likely to crack and form local weak points, and can withstand greater rolling pressure, making the roadbed denser after rolling. Moreover, by adding cement powder, under the slow wetting of water, the cement powder will slowly form a colloid with a certain viscosity and slowly condense to form a certain rigid skeleton in the roadbed, further improving the structural stability of the roadbed, with stronger load-bearing capacity and less likely to be compressed as a whole. Moreover, due to the lack of sufficient water, the hydration reaction of the cement is carried out slowly and gradually, which can make the formed cement skeleton more adaptable to the compacted roadbed, with a high degree of coordination and better effect of reinforcing the roadbed. The roadbed is not prone to local damage, resulting in local depression and cracking of the road surface.
[0024] Preferably, in the first filler, the mass ratio of sand to clay is 100:2.98-3.02;
[0025] In the step 3), when compacting the first filler, a 22t roller is used to roll it 5-6 times for compaction.
[0026] By adopting the above technical scheme, by specifically selecting the ratio of sand and clay, and using a 22t roller for rolling, the compaction degree of the lower embankment is between 93-94%, which well meets the compaction degree requirements of the roadbed, and the construction period is short. The compacted roadbed has good permeability and structural stability, and is not prone to cracking and cracking. If the lower roadbed expands excessively, the pressure on the upper roadbed can be buffered by squeezing the lower embankment, thereby avoiding the phenomenon of road surface cracking due to roadbed expansion.
[0027] Preferably, in the second filler, the mass ratio of sand, clay and gravel is 100:4.98-5.02:29.9-30.1;
[0028] In the step 3), when compacting the second filler, a 25t roller is used to roll it 5-6 times to compact it.
[0029] By adopting the above technical scheme, by specifically selecting the ratio of sand, clay and gravel, and cooperating with a 25T roller for rolling, the compaction degree of the upper embankment is between 94-95%, which well meets the compaction degree requirements of the roadbed, the gravel is not easy to break, the sand, clay and gravel are densely bonded, and have a certain degree of permeability. At the same time, the structure of the upper embankment is stable, the bearing capacity is strong, and it can buffer the expansion deformation of the lower roadbed, avoiding the situation where the expansion deformation acts excessively on the upper roadbed and causes road surface damage.
[0030] Preferably, in the third filler, the mass ratio of sand, clay and expansion agent is 100:3.98-4.02:1.98-2.02;
[0031] In the step 3), when compacting the third filler, first use a 22t roller to roll it 2-3 times, and then use a 30t roller to roll it 7-8 times to compact it.
[0032] By adopting the above technical scheme and specifically selecting the proportions of sand, clay and expansion agent, the expansion amplitude is just right, which can increase the roadbed density in the later stage without damaging the roadbed due to expansion. The roadbed is first rolled with a 22t roller and then with a 30t roller, so that the initial density is high and the density of the lower roadbed reaches 96-97%. In addition, the roadbed will not become loose during the expansion process, thereby better achieving the effect of increasing the roadbed density through expansion.
[0033] Preferably, the expansion agent is anhydrous calcium sulphoaluminate.
[0034] By adopting the above technical solution, anhydrous calcium sulphoaluminate is used as the expansion agent, the expansion process needs to absorb water, and the expansion cycle is relatively long. The expansion agent can be replenished with water through rainwater or road sprinkling, and it will not expand rapidly to cause roadbed damage. It is better adapted to the road construction process. When the road surface is poured, the weight of the road surface will act on the roadbed. Under the weight of the road surface and the weight of the vehicle, the roadbed is further compacted and compressed. At the same time, the expansion agent expands slowly and synchronously to compensate for the compression deformation. After the construction is completed, the effect of resisting settlement through continuous slow expansion is achieved. There is no need for a large amount of compaction work to increase the density, and the construction is convenient and the noise is low.
[0035] Preferably, in the fourth filler, the mass ratio of sand, clay, reinforcing fiber and cement powder is 100:2.98-3.02:3.99-4.01:0.99-1.01;
[0036] In the step 3), when compacting the fourth filler, first use a 25t roller to roll it 2-3 times, and then use a 32t roller to roll it 9-10 times to compact it.
[0037] By adopting the above technical solution and specifically selecting the proportions of sand, clay, reinforcing fiber and cement powder, the effect of reinforcing the upper roadbed with cement powder and reinforcing fiber is better. The upper roadbed is first rolled with a 25t roller and then with a 32t roller, so that the density of the upper roadbed reaches 96-97%, meeting the density requirements, and the surface reinforcing fibers are not damaged due to sudden excessive pressure.
[0038] Preferably, the reinforcing fiber is glass fiber.
[0039] By adopting the above technical solution and using glass fiber, the tensile performance is better, so that the upper roadbed is not easy to crack and the concrete road surface is stably supported.
[0040] Preferably, the glass fiber has a length of 8-10 mm.
[0041] By adopting the above technical solution and specifically selecting the length of the glass fiber, the glass fiber reinforcement effect is better and the roadbed is more stable.
[0042] Preferably, the cement powder has a particle size of 5-6.5 microns.
[0043] By adopting the above technical solution and specifically selecting the particle size of cement powder, the cement powder is evenly distributed to form a perfect cement skeleton, which has a better effect of reinforcing the roadbed.
[0044] Preferably, the water content of the sand is 10-11%, and the water content of the clay is 20-21%.
[0045] By adopting the above technical solution and specifically selecting the moisture content of sand and clay, the compaction effect is better, it is easier to achieve the required density of each layer, and it is easy to construct.
[0046] In summary, this application has the following beneficial effects:
[0047] 1. Since the present application forms a lower embankment, an upper embankment, a lower roadbed and an upper roadbed through layered backfilling, and each layer adopts a special filler formula so that each layer has different properties, through the coordination of each layer, under the compaction process, a higher density can be achieved, the roadbed settlement is low, and it can cooperate well with the old roadbed, so that the concrete pavement is not easy to break due to the difference in settlement between the new and old roadbeds.
[0048] 2. In the present application, it is preferred to specifically select the proportions of the components of the first filler, the second filler, the third filler, and the fourth filler, and cooperate with the specific compaction processes of the lower embankment, the upper embankment, the lower roadbed, and the upper roadbed, so that the initial density of each layer is just right and cooperates with each other, and then cooperates with the special position of the expansion agent, the special selection of the expansion agent, and the special amount of the expansion agent, so that the volume shrinkage of the roadbed can be compensated by the expansion agent during the process of further compaction due to long-term stress, thereby reducing the surface settlement of the roadbed and improving the stability of the road. DETAILED DESCRIPTION
[0049] The present application is further described in detail below with reference to the embodiments.
[0050] Example 1
[0051] A construction method for widening a concrete roadbed comprises the following steps:
[0052] Step 1), surface excavation, as follows:
[0053] Set up fences, remove the green belt in the widened area, and then use a breaker to destroy the concrete structure in the widened area, remove the waste debris and clean it up into the soil layer to avoid accidental damage to the original road surface during construction.
[0054] Step 2), excavate the roadbed foundation pit, as follows:
[0055] Measure and lay out on the soil layer, and excavate the roadbed foundation pit according to the widened area. The distance from the bottom of the foundation pit to the top of the old roadbed is 200cm.
[0056] Step 3), layered backfilling and compaction, specifically including:
[0057] The first filling material is backfilled at the bottom of the foundation pit and rolled 5 times by a 22t roller to compact it. After compaction, a lower embankment is formed. The thickness of the lower embankment is 50cm and the density of the lower embankment is 93%.
[0058] The second filling material is backfilled on the surface of the lower embankment and rolled 5 times by a 25t roller to compact it to form an upper embankment. The thickness of the upper embankment is 70cm and the density of the upper embankment is 94%.
[0059] The third filling material is backfilled on the surface of the upper embankment. It is first rolled twice with a 22t roller and then rolled seven times with a 30t roller to compact it to form a lower roadbed. The thickness of the lower roadbed is 50cm and the density of the lower roadbed is 96%.
[0060] The fourth filler is backfilled on the surface of the lower roadbed, first rolled twice with a 25t roller, then changed to a 32t roller and rolled 9 times to compact it to form an upper roadbed. The thickness of the upper roadbed is 30cm and the density of the upper roadbed is 96%.
[0061] The lower embankment, upper embankment, lower roadbed and upper roadbed together form the roadbed.
[0062] Among them, the first filler is a compound of sand and clay, and the mass ratio of sand to clay is 100:3.
[0063] The preparation method of the first filler is as follows:
[0064] Weigh sand and clay in proportion, put them into a roller mixer, and stir for 5 minutes until they are evenly mixed to obtain the first filler.
[0065] Among them, the second filler is a compound of sand, clay and crushed stone. The mass ratio of sand, clay and crushed stone is 100:5:30, and the particle size of the crushed stone is 12 cm.
[0066] The preparation method of the second filler is as follows:
[0067] Weigh sand, clay and gravel in proportion, put them into a roller mixer, and stir for 5 minutes until they are evenly mixed to obtain the second filler.
[0068] The third filler is compounded by sand, clay and expansion agent, the mass ratio of sand, clay and expansion agent is 100:4:2, the expansion agent is anhydrous calcium sulphoaluminate, and the anhydrous calcium sulphoaluminate is powder passing through an 800-mesh sieve.
[0069] The preparation method of the third filler is as follows:
[0070] Weigh sand, clay and expansion agent in proportion, put them into a roller mixer, stir for 5 minutes, and stir evenly to obtain the third filler.
[0071] Among them, the fourth filler is a compound of sand, clay, reinforcing fiber and cement powder. The mass ratio of sand, clay, reinforcing fiber and cement powder is 100:3:4:1. The reinforcing fiber is glass fiber with a length of 8 mm. The cement powder is silicate cement and the cement powder is a powder with a mesh size of 2500.
[0072] The preparation method of the fourth filler is as follows:
[0073] Weigh sand, clay, reinforcing fiber and cement powder according to proportion, put them into a roller mixer, and stir for 5 minutes until they are evenly mixed to obtain the fourth filler.
[0074] Example 2
[0075] A construction method for widening a concrete roadbed comprises the following steps:
[0076] Step 1), surface excavation, as follows:
[0077] Set up fences, remove the green belt in the widened area, and then use a breaker to destroy the concrete structure in the widened area, remove the waste debris and clean it up into the soil layer to avoid accidental damage to the original road surface during construction.
[0078] Step 2), excavate the roadbed foundation pit, as follows:
[0079] Measure and lay out on the soil layer, and excavate the roadbed foundation pit according to the widened area. The distance from the bottom of the foundation pit to the top of the old roadbed is 200cm.
[0080] Step 3), layered backfilling and compaction, specifically including:
[0081] The first filling material is backfilled at the bottom of the foundation pit and rolled 6 times by a 22t roller to compact it. After compaction, a lower embankment is formed. The thickness of the lower embankment is 50cm and the density of the lower embankment is 94%.
[0082] The second filling material is backfilled on the surface of the lower embankment and rolled 6 times by a 25t roller to compact it, thereby forming an upper embankment. The thickness of the upper embankment is 70cm and the density of the upper embankment is 95%.
[0083] The third filling material is backfilled on the surface of the upper embankment. It is first rolled 3 times with a 22t roller and then rolled 8 times with a 30t roller to compact it to form a lower roadbed. The thickness of the lower roadbed is 50cm and the density of the lower roadbed is 97%.
[0084] The fourth filler is backfilled on the surface of the lower roadbed, first rolled 3 times with a 25t roller, then changed to a 32t roller and rolled 10 times to compact it to form an upper roadbed. The thickness of the upper roadbed is 30cm and the density of the upper roadbed is 97%.
[0085] The lower embankment, upper embankment, lower roadbed and upper roadbed together form the roadbed.
[0086] Among them, the first filler is a compound of sand and clay, and the mass ratio of sand to clay is 100:3.
[0087] The preparation method of the first filler is as follows:
[0088] Weigh sand and clay in proportion, put them into a roller mixer, and stir for 5 minutes until they are evenly mixed to obtain the first filler.
[0089] Among them, the second filler is a compound of sand, clay and crushed stone. The mass ratio of sand, clay and crushed stone is 100:5:30, and the particle size of the crushed stone is 12 cm.
[0090] The preparation method of the second filler is as follows:
[0091] Weigh sand, clay and gravel in proportion, put them into a roller mixer, and stir for 5 minutes until they are evenly mixed to obtain the second filler.
[0092] The third filler is compounded by sand, clay and expansion agent, the mass ratio of sand, clay and expansion agent is 100:4:2, the expansion agent is anhydrous calcium sulphoaluminate, and the anhydrous calcium sulphoaluminate is powder passing through an 800-mesh sieve.
[0093] The preparation method of the third filler is as follows:
[0094] Weigh sand, clay and expansion agent in proportion, put them into a roller mixer, stir for 5 minutes, and stir evenly to obtain the third filler.
[0095] Among them, the fourth filler is a compound of sand, clay, reinforcing fiber and cement powder. The mass ratio of sand, clay, reinforcing fiber and cement powder is 100:3:4:1. The reinforcing fiber is glass fiber with a length of 10 mm. The cement powder is silicate cement and the cement powder is a powder with a mesh size of 2000.
[0096] The preparation method of the fourth filler is as follows:
[0097] Weigh sand, clay, reinforcing fiber and cement powder according to proportion, put them into a roller mixer, and stir for 5 minutes until they are evenly mixed to obtain the fourth filler.
[0098] Comparative Example 1
[0099] Compared with Example 1, the only difference is:
[0100] In the third filler, an equal amount of stone powder is used to replace the expansion agent.
[0101] Comparative Example 2
[0102] Compared with Example 1, the only difference is:
[0103] In the third filler, the expansion agent is a commercially available U-shaped expansion agent.
[0104] Comparative Example 3
[0105] Compared with Example 1, the only difference is:
[0106] In the first filler, the mass ratio of sand to clay is 100:5;
[0107] In the second filler, the mass ratio of sand, clay and gravel is 100:6:25;
[0108] In step 3):
[0109] Backfill the first filling material at the bottom of the foundation pit, first use a 22t roller to roll it twice, then change to a 30t roller to roll it 7 times to compact it. After compaction, a lower embankment is formed. The thickness of the lower embankment is 50cm and the density of the lower embankment is 96%.
[0110] The second filling material is backfilled on the surface of the lower embankment. It is first rolled twice with a 22t roller and then rolled seven times with a 30t roller to compact it. The thickness of the upper embankment is 70cm and the density of the upper embankment is 96%.
[0111] Comparative Example 4
[0112] Compared with Example 1, the only difference is:
[0113] In the third filler, the mass ratio of sand, clay and expansion agent is 100:4:1.
[0114] Comparative Example 5
[0115] Compared with Example 1, the only difference is:
[0116] In the third filler, the mass ratio of sand, clay and expansion agent is 100:4:3.
[0117] Experiment 1
[0118] An experimental site was selected with uniform soil, no obvious faults, no groundwater leakage and other defects.
[0119] First, the site is leveled, and the roadbed is constructed in the site using the construction methods of the embodiments and comparative examples.
[0120] The roadbed is 10m long, 3m wide, and the roadbed pit depth is 255cm.
[0121] The distance between adjacent roadbeds is 5m.
[0122] After the roadbed construction is completed, a crushed stone base layer is laid on the roadbed surface with a thickness of 15 cm. A 3% cement-stabilized crushed stone layer is laid on the surface of the crushed stone base layer with a thickness of 15 cm. A C35 plain concrete surface layer is laid on the surface of the 3% cement-stabilized crushed stone layer with a thickness of 25 cm. The road is watered for 7 days and then left to stand for 28 days to obtain a test road, the surface of which is exactly flush with the surface of the test site.
[0123] Containers are placed on the experimental road. The containers are evenly distributed on the experimental road. There is a gap between adjacent containers. The distance between adjacent containers is 0.5m. The containers are filled with heavy objects. The total weight of all containers and heavy objects is 50t.
[0124] After placing the container for 6 months, measure the distance from the test road surface to the test site plane. If the test road surface is lower than the test site plane, it is expressed as a negative number. If the test road surface is higher than the test site surface, it is expressed as a positive number. Calculate the height change rate using the following formula:
[0125] The distance from the test road surface to the test site plane ÷ 255 (cm) × 100%.
[0126] If cracks appear on the test road surface, the distance from the test road surface to the test site plane will no longer be tested and the cracks will be judged to be due to expansion.
[0127] The specific test data of Experiment 1 are shown in Table 1.
[0128] Table 1
[0129]
[0130]
[0131] According to the data comparison between Example 1 and Comparative Example 1 in Table 1, it can be obtained that by adding the expansion agent, the volume compression caused by the increase in the roadbed density can be effectively compensated, so that the volume change of the roadbed is reduced, thereby reducing the height drop of the road surface. In actual construction, it is not easy to produce a huge settlement difference with the old roadbed, so that the road surface is not easy to be torn apart and cracked due to the sedimentation difference, and the road surface is not easy to be damaged, and the durability is better. In addition, there is no need to adopt a compaction process, which reduces noise pollution during the construction process and shortens the construction period.
[0132] According to the data comparison between Example 1 and Comparative Examples 2-5 in Table 1, the embodiment generally designs the initial density of the lower embankment, the upper embankment, the lower roadbed, and the upper roadbed, designs the filler components and proportions of each layer, and selects a specific expansion agent, so that when the roadbed is compressed, the expansion agent produces a just right expansion effect, effectively compensating for the volume change of the roadbed, and avoiding the phenomenon of reverse damage to the road surface caused by excessive volume expansion of the expansion agent.
[0133] Through the density design of each layer, part of the expansion effect of the expansion agent can act on the lower embankment and the upper embankment, avoiding the situation where the volume expansion is concentrated on the upper roadbed, and thus making it less likely for the upper roadbed to move up and cause road cracks.
[0134] However, when the density of the lower embankment and the upper embankment is changed, the expansion effect of the expansion agent is difficult to release through the lower embankment and the upper embankment, which can easily cause the volume of the roadbed to expand and lead to the danger of road cracking.
[0135] However, when the dosage of the expansion agent is changed and the amount of expansion agent added is reduced, the pavement settlement is still large, which can easily cause the new and old pavements to break.
[0136] However, when the amount of expansion agent added is too high, the expansion effect is too large, the road base moves up, and it is easy to cause road cracks.
[0137] However, when a specific expansion agent is not selected, the amount of expansion will change and cannot match the density of each layer, and the effect of reducing the surface settlement of the roadbed will decrease.
[0138] In Experiment 1, the containers were placed at intervals so that the part without the force of the containers became the release area for the upward movement of the soil layer. Therefore, cracks were likely to occur in the adjacent parts of the containers.
[0139] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A construction method for widening a concrete roadbed, characterized in that: The following steps are involved: Step 1), surface excavation, including: Excavate and remove the surface structure in the widened area; Step 2) excavate the roadbed foundation pit, including: Excavate the soil base of the widened area to form a roadbed foundation pit; Step 3), backfilling and compacting in layers, including: Backfilling the first filler material at the bottom of the foundation pit and compacting it to form a lower embankment, backfilling the second filler material on the lower embankment and compacting it to form an upper embankment, backfilling the third filler material on the upper embankment and compacting it to form a lower roadbed, backfilling the fourth filler material on the lower roadbed and compacting it to form an upper roadbed; The lower embankment, upper embankment, lower roadbed and upper roadbed together constitute a roadbed; The first filler includes a compound of sand and clay; The second filler includes a mixture of sand, clay and crushed stone; The third filler includes a compound of sand, clay and expansion agent; The fourth filler comprises a compound of sand, clay, reinforcing fiber and cement powder; In the first filler, the mass ratio of sand to clay is 100:2.98-3.02; In the step 3), when compacting the first filler, a 22t roller is used to roll it 5-6 times to compact it; In the second filler, the mass ratio of sand, clay and gravel is 100:4.98-5.02:29.9-30.1; In the step 3), when compacting the second filler, a 25t roller is used to roll it 5-6 times to compact it; In the third filler, the mass ratio of sand, clay and expansion agent is 100:3.98-4.02:1.98-2.02; In the step 3), when compacting the third filler, first use a 22t roller to roll it 2-3 times, and then use a 30t roller to roll it 7-8 times to compact it.
2. A construction method for widening a concrete roadbed according to claim 1, characterized in that: The expansion agent is anhydrous calcium sulphoaluminate.
3. A construction method for widening a concrete roadbed according to claim 1, characterized in that: In the fourth filler, the mass ratio of sand, clay, reinforcing fiber and cement powder is 100: 2.98-3.02: 3.99-4.01: 0.99-1.01; In the step 3), when compacting the fourth filler, first use a 25t roller to roll it 2-3 times, and then use a 32t roller to roll it 9-10 times to compact it.
4. A construction method for widening a concrete roadbed according to claim 3, characterized in that: The reinforcing fiber is glass fiber.
5. A construction method for widening a concrete roadbed according to claim 4, characterized in that: The length of the glass fiber is 8-10 mm.
6. A construction method for widening a concrete roadbed according to claim 3, characterized in that: The particle size of the cement powder is 5-6.5 microns.
7. A construction method for widening a concrete roadbed according to any one of claims 1 to 6, characterized in that: The water content of the sand is 10-11%, and the water content of the clay is 20-21%.