Oxide target material and preparation method thereof
Through specific oxide combinations and multiple sintering technologies, the problems of density and grain size of oxide targets in the sintering process are solved, and an oxide target with high density and uniform structure is achieved, improving the stability of the material. and performance.
Patent Information
- Application Number
- CN202211636891.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-16
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-12-16
AI Technical Summary
It is difficult for existing oxide targets to achieve high density, small grain size and uniform element distribution during the sintering process, resulting in material composition deviation and cracking problems.
Using a specific combination of oxide target formulas, including oxides of indium, gallium, zinc, cerium, praseodymium, scandium and other elements, the crystal phase structure is controlled through multiple sintering processes, combined with gas environment and temperature gradient management, to prepare high-performance Oxide target material with dense density and uniform structure.
The high density, low resistivity and uniform element distribution of the oxide target material are achieved, ensuring the stability and performance optimization of the material.
Smart Images

Figure CN116199497B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of semiconductor materials, and in particular to an oxide target material and a preparation method thereof. Background Art
[0002] With the increasing market competitiveness of China's new display industry in recent years, as the world's largest TFT-LCD display panel production base, oxide targets have also become a research hotspot in China. Thin films sputtered using targets such as ZnO, IZO, and IGZO can be used for TFT active layers. In the application of LCD, OLED and electronic paper flat panel displays (FPD), they have attracted great attention from a large number of researchers and industry professionals due to their excellent performance.
[0003] The density, grain size, composition and structural uniformity of oxide targets affect various electrical and optical properties of sputtered films. In order to improve the quality of oxide targets to meet the needs of the high-end display panel industry, many researchers have improved and upgraded the powder raw materials of oxide targets. For example, Chinese invention patent CN107146816A discloses an oxide semiconductor film and a thin film transistor prepared therefrom, which improves the optical stability of oxide thin film transistor devices by doping with rare earth oxides.
[0004] However, due to the fact that the ionic radius of rare earth elements is smaller than that of In in the main oxide 3+ , Zn 2+ , Ga 3+ , Sn 4+ The ion radius is large, and the rare earth oxide Ln2O3 is usually a hexagonal system, in which the metal ion coordination number is seven, six oxygen atoms occupy the six corners of the octahedron, and the seventh oxygen atom is at the center of one face of the octahedron. This is quite different from the ferromanganese structure of the cubic system of In2O3, the corundum structure of Ga2O3, the sphalerite or wurtzite structure of ZnO, and the rutile structure of SnO2. This makes it difficult to achieve substitutional doping of rare earth oxides in the target material. During the sintering process, the doped rare earth elements will accumulate at the grain boundaries, resulting in deviations in the material composition in the micro-region. In addition, the grain size of the mass-produced IGZO target is commonly 10-30μm. This size is too large, making it easier for the doping elements to concentrate excessively at limited grain boundaries, resulting in cracking of the oxide target. Summary of the invention
[0005] In view of this, it is necessary to provide an oxide target material and a preparation method thereof to address the above-mentioned problems. The prepared oxide target material has high density, small grain size, and uniform element distribution and microstructure.
[0006] To achieve the above object, the present invention adopts the following technical solutions:
[0007] In a first aspect, the present invention provides an oxide target material, comprising an oxide of element A, an oxide of element B, an oxide of element R, and an oxide of element M;
[0008] The element A is indium;
[0009] The element B is one or a combination of two or more of gallium, zinc and tin;
[0010] The element R is one or a combination of two or more of cerium, praseodymium, ytterbium, dysprosium and terbium;
[0011] The element M is one or a combination of two or more of scandium, silicon, titanium, tantalum, germanium and antimony.
[0012] Furthermore, in the above oxide target, the atomic molar ratios of elements A, B, R and M in the oxide target are x, y, z and m respectively, wherein 0.6≤x≤0.9994, 0≤y≤0.3994, 0.0005≤z≤0.05, 0.001≤m≤0.02, and x+y+z+m=1.
[0013] Furthermore, in the above oxide target, 0.76≤x≤0.9994, 0.005≤m≤0.015.
[0014] Furthermore, in the above oxide target, the resistivity of the oxide target is less than 10 mΩ·cm.
[0015] Furthermore, in the above oxide target, the relative density of the oxide target is greater than 98.5%.
[0016] Furthermore, in the above oxide target material, the maximum particle size of the oxide target material grains is less than 8 μm.
[0017] Preferably, in the above oxide target, the size of the oxide target grains is 3 to 5 μm.
[0018] In a second aspect, the present invention provides a method for preparing the above-mentioned oxide target, comprising the following steps:
[0019] Step 1, pressing the powder into a target blank;
[0020] Step 2, drying the target blank and then degreasing it;
[0021] Step 3, heating the degreased target blank in a gas environment to a first sintering temperature at a first heating rate, then heating the blank to a second sintering temperature at a second heating rate, and finally cooling the blank to the first sintering temperature at a first cooling rate and continuing to sinter;
[0022] Step 4: After sintering, the temperature is lowered at a second cooling rate in a gas environment until the temperature reaches room temperature, so as to obtain a sintered target body;
[0023] Step 5: Processing and binding the target sintered body.
[0024] Furthermore, in the above-mentioned method for preparing the oxide target, the average particle size of the oxide of element A in the powder is 0.05 μm to 0.5 μm; the average particle size of the oxide of element B is 0.05 μm to 0.5 μm, the average particle size of the oxide of element R is 0.05 μm to 1.5 μm, and the average particle size of the oxide of element M is 0.05 to 1.5 μm.
[0025] Furthermore, in the above-mentioned method for preparing the oxide target, the specific method of step 1 is:
[0026] Step 1.1, mix the powders according to the proportion, add dispersant, water and binder and grind to obtain slurry;
[0027] Step 1.2: spray granulate the slurry, dry it, and screen the particle size D of the granulated powder. 50 =1.50-2.75μm, D 10 ≥1.0μm, D 90 ≤3.5μm, particle size distribution coefficient P=(D 90 -D 10 ) / D 50 ≤2.0;
[0028] Step 1.3: Press the screened powder into a target blank.
[0029] Preferably, in step 1.1, the oxide of element A, the oxide of element B, a dispersant and water are first mixed and ground into slurry one; then the oxide of element R, the oxide of element M, a dispersant and water are mixed and ground into slurry two; finally, slurry one, slurry two and a binder are mixed and ground.
[0030] Preferably, in step 1.1, the oxide of element R, the oxide of element M, a dispersant and water are first mixed and ground into slurry one; the oxide of element A and the oxide of element B are added to slurry one in sequence, and after each oxide is added, a dispersant and water are added accordingly to grind into slurry two; finally, a binder is added to slurry two and grinding is continued.
[0031] Preferably, ultrasonic or vacuum degassing can be added during the slurry preparation process.
[0032] More preferably, the mass percentage of the dispersant is 0.1-2.0%, the mass percentage of the binder is 0.1-1.5%, the grinding is performed using a sand mill, and the mass percentage of the ball milling medium is 40-60%. The mass percentage is the ratio of the mass of each substance to the total mass.
[0033] Preferably, in step 1.2, the granulation temperature is 180-200° C., and the feed rate is 5-20 rpm.
[0034] Preferably, the molding in step 1.3 is performed under a hydraulic press, the pressure is 20 to 100 MPa, and the holding time is 2 to 15 minutes.
[0035] More preferably, the target blank molded in step 1.3 is covered with a flexible mold and further pressed by isostatic pressing; the isostatic pressing pressure is 220 to 300 MPa, and the time is 10 to 30 minutes.
[0036] Furthermore, the degreasing treatment in step 2 is to first raise the temperature of the target blank to 600-800° C. at a heating rate of 0.2-1° C. / min; the degreasing time is 50-100 hours.
[0037] Preferably, the heating rate is 0.5° C. / min. If the heating rate is too fast, the oil will evaporate at a constant rate or fail to evaporate completely, which may easily cause pores or cracks, thereby affecting the quality of the target material.
[0038] Furthermore, the gas environment in step 3 includes one or a mixture of two or more of air, water vapor, nitrogen, oxygen, ozone, and laughing gas. Among them, a certain amount of oxidizing gas can keep the oxide of element R in a higher valence state, so that the light stabilizer can be better utilized and it is beneficial to obtain a target material with uniform color; in addition, the introduction of a certain amount of water vapor is beneficial to rapid cooling.
[0039] Furthermore, the gas environment in different sintering processes in step 3 and the gas environment in step 4 may be the same or different.
[0040] Furthermore, the first heating rate is 0.1-5°C / min, preferably 0.1-2.5°C / min; and the first sintering temperature is 1200°C-1400°C.
[0041] Furthermore, the second heating rate is 5-10°C / min, and the second sintering temperature is 1410-1600°C.
[0042] Furthermore, the sintering process of step 3 is repeated multiple times, and the first sintering temperature, the second sintering temperature, the first heating rate, the second heating rate, and the first cooling rate can be the same or different during the multiple repetitions. By repeating the sintering process of step 3 multiple times, the crystal phase structure is controlled, and the prepared oxide target has a smaller grain size.
[0043] Furthermore, the first sintering temperature is kept warm for 50 to 250 hours each time; and the second sintering temperature is kept warm for 10 to 60 minutes each time.
[0044] Furthermore, the first cooling rate is 1-10°C / min.
[0045] Furthermore, the second cooling rate in step 4 is 1-5°C / min.
[0046] The beneficial effects of the present invention are:
[0047] (1) The present invention introduces oxides of M into the oxide target, thereby refining the grain size of the oxide target, making the relative density of the oxide target higher, and the element distribution and microstructure more uniform.
[0048] (2) During the sintering process for preparing the oxide target material of the present invention, a first sintering temperature and a second sintering temperature are set. The temperature is rapidly increased from the first sintering temperature to the second sintering temperature, and the temperature is maintained for a short time to inhibit grain growth. The temperature is then lowered to the first sintering temperature for a longer period of low-temperature sintering, thereby obtaining a fully dense oxide target material. In addition, the present invention can achieve the purpose of controlling the crystal phase structure by repeating the above sintering process multiple times, so that the oxide target material has a smaller grain size and a uniform microstructure. BRIEF DESCRIPTION OF THE DRAWINGS
[0049] Figure 1 This is the appearance diagram of the oxide target material of Example 7;
[0050] Figure 2 is a SEM image of the oxide target of Example 7;
[0051] Figure 3 is a grain size diagram of the oxide target material of Example 7;
[0052] Figure 4 This is the metal element distribution diagram of the oxide target material of Example 7. DETAILED DESCRIPTION
[0053] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be further clearly and completely described in combination with the embodiments of the present invention. It should be noted that the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0054] In the description of the present invention, it should be noted that, if the specific conditions are not specified in the examples, the experiments were carried out according to conventional conditions or the conditions recommended by the manufacturer. The reagents or instruments used, if the manufacturer is not specified, are all conventional products that can be purchased commercially.
[0055] The average particle size of the oxide of element A in the powder of the embodiment of the present invention is 0.05 μm to 0.5 μm; the average particle size of the oxide of element B is 0.05 μm to 0.5 μm, the average particle size of the oxide of element R is 0.05 μm to 1.5 μm, and the average particle size of the oxide of element M is 0.05 to 1.5 μm.
[0056] Example 1
[0057] An oxide target material comprises an oxide of element A, an oxide of element B, an oxide of element R and an oxide of element M;
[0058] The element A is indium (In);
[0059] The element B is gallium (Ga) and zinc (Zn); the molar ratio of gallium to zinc is 1:2;
[0060] The element R is cerium (Ce);
[0061] The element M is scandium (Sc);
[0062] In the above oxide target, the atomic molar ratios of elements A, B, R and M in the oxide target are x, y, z and m respectively, wherein x=0.65, y=0.33, z=0.005 and m=0.015.
[0063] That is, the molar ratio of metal atoms in the target material satisfies In:Ga:Zn:Ce:Sc=0.65:0.11:0.22:0.005:0.015.
[0064] The above oxide target is prepared by the following method:
[0065] Step 1: Press the powder into a target blank;
[0066] Step 1.1: First, weigh the oxide powders of elements A, B, R, and M according to the molar ratio of the target metal atoms, with a total weight of 6 kg. Premix the oxide powders of element A, element B, a certain amount of polyvinyl pyrrolidone and pure water, wherein polyvinyl pyrrolidone accounts for 1.2% of the total mass after mixing, and the solid content of the premixed mixed solution is 50%. Ultrasonic pre-dispersion for 30 minutes, grind into slurry 1 with a sand mill, the speed is 800 rpm, and the grinding time is 20 hours; the average particle size of the mixed powder in slurry 1 is less than 0.8 μm, and vacuum degassing is performed; then premix the oxide of element R, the oxide of element M, polyvinyl pyrrolidone and a certain amount of pure water, wherein polyvinyl pyrrolidone accounts for 1.2% of the total mass after mixing, and the solid content of the premixed mixed solution is 50%. Ultrasonic pre-dispersion for 30 minutes, grinding into slurry 2 with a sand mill, the speed is 800 rpm, and the grinding time is 20 hours; the average particle size of the mixed powder in slurry 2 is less than 0.8μm, and vacuum degassing is performed; finally, slurry 1, slurry 2, polyvinyl alcohol and polyethylene glycol are mixed, wherein the content of polyvinyl alcohol and polyethylene glycol respectively accounts for 1.2% of the total mass after mixing, and the solid content of the mixed slurry is 42%. Grinding with a sand mill, the grinding time is 5 hours, and the average particle size of the mixed powder in the final slurry is less than 0.8μm, and vacuum degassing is performed;
[0067] Step 1.2: The final slurry is spray granulated at a granulation temperature of 200°C and a feed rate of 10 rpm; after drying, the particle size D of the granulated powder is screened. 50 =1.6μm, D 10 ≥1.0μm, D 90 ≤3.0μm, particle size distribution coefficient P=(D 90 -D 10 ) / D 50 =1.0;
[0068] Step 1.3: The screened powder is molded under a hydraulic press at a pressure of 80 MPa for 5 minutes; then further pressed by isostatic pressing at a pressure of 280 MPa for 30 minutes;
[0069] Step 2: After drying the target blank, degreasing is performed; specifically, the target blank is heated to 700°C at a heating rate of 0.5°C / min; the degreasing time is 60 hours;
[0070] Step 3: heating from 700°C to a first sintering temperature of 1250°C at a first heating rate of 1°C / min, and keeping the temperature for 10 hours in a gas environment with an oxygen content of 20-30% in air; heating to a second sintering temperature of 1420°C at a second heating rate of 8°C / min, and keeping the temperature for 30 minutes in a gas environment with an oxygen content of 40-50% in air; then cooling to a first sintering temperature of 1250°C at a first cooling rate of 3°C / min, and keeping the temperature for 10 hours in a gas environment with an oxygen content of 40-50% in air;
[0071] Rapidly heat up to the second sintering temperature of 1460°C at a heating rate of 8°C / min, and keep warm for 30 minutes in a gas environment with an oxygen content of 60-70% in air; then cool down to the first sintering temperature of 1250°C at a cooling rate of 3°C / min, and keep warm for 10 hours in a gas environment with an oxygen content of 40-50% in air;
[0072] The temperature was rapidly increased to the second sintering temperature of 1500°C at a heating rate of 8°C / min, and kept warm for 30 minutes in a gas environment with an oxygen content of 60-70% in air; then the temperature was reduced to the first sintering temperature of 1250°C at a cooling rate of 3°C / min, and kept warm for 10 hours in a gas environment with an oxygen content of 40-50% in air.
[0073] Step 4: In a gas environment where the oxygen content in air is 20-30%, cooling to room temperature at a second cooling rate of 1°C / min to obtain a target sintered body;
[0074] Step 5: After machining the obtained target sintered body, bind it to the metal back plate using indium binding.
[0075] Example 2
[0076] An oxide target material comprises an oxide of element A, an oxide of element B, an oxide of element R and an oxide of element M;
[0077] The element A is indium (In);
[0078] The element B is gallium (Ga) and zinc (Zn); the molar ratio of gallium to zinc is 1:2;
[0079] The element R is praseodymium (Pr);
[0080] The element M is titanium (Ti);
[0081] In the above oxide target, the atomic molar ratios of elements A, B, R and M in the oxide target are x, y, z and m respectively, wherein x=0.64, y=0.33, z=0.015, m=0.015.
[0082] In the method for preparing oxide targets, indium oxide (In2O3), gallium oxide (Ga2O3), zinc oxide (ZnO), praseodymium oxide (Pr6O 11 ) and titanium oxide (TiO2) powders were weighed according to the atomic molar ratio of In:Ga:Zn:Pr:Ti=0.64:0.11:0.22:0.015:0.015, and the total weight of the powders was 6 kg. The rest was the same as the preparation method in Example 1.
[0083] Example 3
[0084] An oxide target material comprises an oxide of element A, an oxide of element B, an oxide of element R and an oxide of element M;
[0085] The element A is indium (In);
[0086] The element B is gallium (Ga) and zinc (Zn); the molar ratio of gallium to zinc is 1:2;
[0087] The element R is ytterbium (Yb);
[0088] The element M is silicon (Si);
[0089] In the above oxide target, the atomic molar ratios of elements A, B, R and M in the oxide target are x, y, z and m respectively, wherein x=0.64, y=0.33, z=0.029 and m=0.001.
[0090] In the preparation method of the oxide target material, indium oxide (In2O3), gallium oxide (Ga2O3), zinc oxide (ZnO), ytterbium oxide (Yb2O3) and silicon oxide (SiO2) powders are weighed according to the atomic molar ratio of In:Ga:Zn:Yb:Si=0.64:0.11:0.22:0.029:0.001, and the total weight of the powder is 6 kg. The rest is the same as the preparation method in Example 1.
[0091] Example 4
[0092] An oxide target material comprises an oxide of element A, an oxide of element B, an oxide of element R and an oxide of element M;
[0093] The element A is indium (In);
[0094] The element B is gallium (Ga) and zinc (Zn); the molar ratio of gallium to zinc is 1:2;
[0095] The element R is dysprosium (Dy);
[0096] The element M is tantalum (Ta);
[0097] In the above oxide target, the atomic molar ratios of elements A, B, R and M in the oxide target are x, y, z and m respectively, wherein x=0.64, y=0.33, z=0.025 and m=0.005.
[0098] In the preparation method of the oxide target material, indium oxide (In2O3), gallium oxide (Ga2O3), zinc oxide (ZnO), dysprosium oxide (Dy2O3) and tantalum oxide (Ta2O5) powders are weighed according to the atomic molar ratio of In:Ga:Zn:Dy:Ta=0.64:0.11:0.22:0.025:0.005, and the total weight of the powder is 6 kg. The rest is the same as the preparation method in Example 1.
[0099] Example 5
[0100] An oxide target material comprises an oxide of element A, an oxide of element B, an oxide of element R and an oxide of element M;
[0101] The element A is indium (In);
[0102] The element B is gallium (Ga) and zinc (Zn); the molar ratio of gallium to zinc is 1:2;
[0103] The element R is praseodymium (Pr);
[0104] The element M is germanium (Ge);
[0105] In the above oxide target, the atomic molar ratios of elements A, B, R and M in the oxide target are x, y, z and m respectively, wherein x=0.64, y=0.33, z=0.015, m=0.015.
[0106] In the method for preparing oxide targets, indium oxide (In2O3), gallium oxide (Ga2O3), zinc oxide (ZnO), praseodymium oxide (Pr6O 11 ) and germanium oxide (GeO2) powders were weighed according to the atomic molar ratio of In:Ga:Zn:Pr:Ge=0.64:0.11:0.22:0.015:0.015, and the total weight of the powders was 6 kg. The rest was the same as the preparation method in Example 1.
[0107] Example 6
[0108] An oxide target material comprises an oxide of element A, an oxide of element B, an oxide of element R and an oxide of element M;
[0109] The element A is indium (In);
[0110] The element B is gallium (Ga) and zinc (Zn); the molar ratio of gallium to zinc is 1:2;
[0111] The element R is praseodymium (Pr);
[0112] The element M is antimony (Sb);
[0113] In the above oxide target, the atomic molar ratios of elements A, B, R and M in the oxide target are x, y, z and m respectively, wherein x=0.64, y=0.33, z=0.01 and m=0.02.
[0114] In the method for preparing oxide targets, indium oxide (In2O3), gallium oxide (Ga2O3), zinc oxide (ZnO), praseodymium oxide (Pr6O 11 ) and antimony oxide (Sb2O3) powders were weighed according to the atomic molar ratio of In:Ga:Zn:Pr:Sb=0.64:0.11:0.22:0.01:0.02, and the total weight of the powders was 6 kg. The rest was the same as the preparation method in Example 1.
[0115] Example 7
[0116] An oxide target material comprises an oxide of element A, an oxide of element B, an oxide of element R and an oxide of element M;
[0117] The element A is indium (In);
[0118] The element B is gallium (Ga) and zinc (Zn); the molar ratio of gallium to zinc is 1:3;
[0119] The element R is praseodymium (Pr);
[0120] The element M is titanium (Ti);
[0121] In the above oxide target, the atomic molar ratios of elements A, B, R and M in the oxide target are x, y, z and m respectively, wherein x=0.65, y=0.32, z=0.02 and m=0.01.
[0122] In the method for preparing oxide targets, indium oxide (In2O3), gallium oxide (Ga2O3), zinc oxide (ZnO), praseodymium oxide (Pr6O 11 ) and titanium oxide (TiO2) powders were weighed according to the atomic molar ratio of In:Ga:Zn:Pr:Ti=0.65:0.08:0.24:0.02:0.01, and the total weight of the powders was 6 kg. The rest was the same as the preparation method in Example 1.
[0123] The appearance of the prepared 6-inch round target is as follows Figure 1 As shown, the prepared oxide target was characterized by SEM, and its pores are as follows Figure 2The oxide target shows a high density with only a small amount of pores. Its grain size is as follows Figure 3 As shown in Figure 1, the average grain size of the oxide target is 4.1 μm. Its element distribution diagram is shown in Figure 1. Figure 4 As shown, the elements are evenly distributed.
[0124] Example 8
[0125] An oxide target material comprises an oxide of element A, an oxide of element B, an oxide of element R and an oxide of element M;
[0126] The element A is indium (In);
[0127] The element B is gallium (Ga);
[0128] The element R is praseodymium (Pr);
[0129] The element M is titanium (Ti);
[0130] In the above oxide target, the atomic molar ratios of elements A, B, R and M in the oxide target are x, y, z and m respectively, wherein x=0.8, y=0.18, z=0.01 and m=0.01.
[0131] In the method for preparing oxide targets, indium oxide (In2O3), gallium oxide (Ga2O3), praseodymium oxide (Pr6O 11 ) and titanium oxide (TiO2) powders were weighed according to the atomic molar ratio of In:Ga:Pr:Ti=0.8:0.18:0.01:0.01, and the total weight of the powders was 6 kg. The rest was the same as the preparation method in Example 1.
[0132] Example 9
[0133] An oxide target material comprises an oxide of element A, an oxide of element B, an oxide of element R and an oxide of element M;
[0134] The element A is indium (In);
[0135] The element B is zinc (Zn);
[0136] The element R is praseodymium (Pr);
[0137] The element M is titanium (Ti);
[0138] In the above oxide target, the atomic molar ratios of elements A, B, R and M in the oxide target are x, y, z and m respectively, wherein x=0.7, y=0.27, z=0.015, m=0.015.
[0139] In the method for preparing oxide targets, indium oxide (In2O3), zinc oxide (ZnO), praseodymium oxide (Pr6O 11 ) and titanium oxide (TiO2) powders were weighed according to the atomic molar ratio of In:Zn:Pr:Ti=0.7:0.27:0.015:0.015, and the total weight of the powders was 6 kg. The rest was the same as the preparation method in Example 1.
[0140] Example 10
[0141] An oxide target material comprises an oxide of element A, an oxide of element B, an oxide of element R and an oxide of element M;
[0142] The element A is indium (In);
[0143] The element B is tin (Sn) and zinc (Zn), and the molar ratio of tin to zinc is 1:2;
[0144] The element R is praseodymium (Pr);
[0145] The element M is titanium (Ti);
[0146] In the above oxide target, the atomic molar ratios of elements A, B, R and M in the oxide target are x, y, z and m respectively, wherein x=0.61, y=0.36, z=0.01 and m=0.02.
[0147] In the preparation method of oxide targets, indium oxide (In2O3), tin oxide (SnO2), zinc oxide (ZnO), praseodymium oxide (Pr6O 11 ) and titanium oxide (TiO2) powders were weighed according to the atomic molar ratio of In:Sn:Zn:Pr:Ti=0.61:0.12:0.24:0.01:0.02, and the total weight of the powders was 6 kg. The rest was the same as the preparation method in Example 1.
[0148] Embodiment 11
[0149] An oxide target material comprises an oxide of element A, an oxide of element B, an oxide of element R and an oxide of element M;
[0150] The element A is indium (In);
[0151] The element B is gallium (Ga) and zinc (Zn); the molar ratio of gallium to zinc is 1:2;
[0152] The element R is terbium (Tb);
[0153] The element M is antimony (Sb);
[0154] In the above oxide target, the atomic molar ratios of elements A, B, R and M in the oxide target are x, y, z and m respectively, wherein x=0.62, y=0.36, z=0.005, and m=0.015.
[0155] In the preparation method of the oxide target material, indium oxide (In2O3), gallium oxide (Ga2O3), zinc oxide (ZnO), terbium oxide (Tb4O7) and antimony oxide (Sb2O3) powders are weighed according to the atomic molar ratio of In:Ga:Zn:Tb:Sb=0.62:0.12:0.24:0.005:0.015, and the total weight of the powder is 6 kg. The rest is the same as the preparation method in Example 1.
[0156] Example 12
[0157] An oxide target material comprises an oxide of element A, an oxide of element B, an oxide of element R and an oxide of element M;
[0158] The element A is indium (In);
[0159] The element B is gallium (Ga) and zinc (Zn); the molar ratio of gallium to zinc is 1:2;
[0160] The element R is terbium (Tb);
[0161] The element M is antimony (Sb);
[0162] In the above oxide target, the atomic molar ratios of elements A, B, R and M in the oxide target are x, y, z and m respectively, wherein x=0.6, y=0.39, z=0.007, and m=0.003.
[0163] In the preparation method of the oxide target material, indium oxide (In2O3), gallium oxide (Ga2O3), zinc oxide (ZnO), terbium oxide (Tb4O7) and antimony oxide (Sb2O3) powders are weighed according to the atomic molar ratio of In:Ga:Zn:Tb:Sb=0.6:0.13:0.26:0.007:0.003, and the total weight of the powder is 6 kg. The rest is the same as the preparation method in Example 1.
[0164] Example 13
[0165] An oxide target material comprises an oxide of element A, an oxide of element B, an oxide of element R and an oxide of element M;
[0166] The element A is indium (In);
[0167] The element B is gallium (Ga);
[0168] The element R is terbium (Tb);
[0169] The element M is antimony (Sb);
[0170] In the above oxide target, the atomic molar ratios of elements A, B, R and M in the oxide target are x, y, z and m respectively, wherein x=0.9, y=0.08, z=0.01 and m=0.01.
[0171] In the preparation method of the oxide target material, indium oxide (In2O3), gallium oxide (Ga2O3), terbium oxide (Tb4O7) and antimony oxide (Sb2O3) powders are weighed according to the atomic molar ratio of In:Ga:Tb:Sb=0.9:0.08:0.01:0.01, and the total weight of the powder is 6 kg. The rest is the same as the preparation method in Example 1.
[0172] Embodiment 14
[0173] An oxide target material comprises an oxide of element A, an oxide of element B, an oxide of element R and an oxide of element M;
[0174] The element A is indium (In);
[0175] The element B is zinc (Zn);
[0176] The element R is terbium (Tb);
[0177] The element M is antimony (Sb);
[0178] In the above oxide target, the atomic molar ratios of elements A, B, R and M in the oxide target are x, y, z and m respectively, wherein x=0.81, y=0.16, z=0.02 and m=0.01.
[0179] In the preparation method of the oxide target material, indium oxide (In2O3), zinc oxide (ZnO), terbium oxide (Tb4O7) and antimony oxide (Sb2O3) powders are weighed according to the atomic molar ratio of In:Zn:Tb:Sb=0.81:0.16:0.02:0.01, and the total weight of the powder is 6 kg. The rest is the same as the preparation method in Example 1.
[0180] Embodiment 15
[0181] An oxide target material comprises an oxide of element A, an oxide of element B, an oxide of element R and an oxide of element M;
[0182] The element A is indium (In);
[0183] The element B is tin (Sn) and zinc (Zn), and the molar ratio of tin to zinc is 1:2;
[0184] The element R is terbium (Tb);
[0185] The element M is antimony (Sb);
[0186] In the above oxide target, the atomic molar ratios of elements A, B, R and M in the oxide target are x, y, z and m respectively, wherein x=0.62, y=0.36, z=0.0005, and m=0.0195.
[0187] In the preparation method of the oxide target material, indium oxide (In2O3), tin oxide (SnO2), zinc oxide (ZnO), terbium oxide (Tb4O7) and antimony oxide (Sb2O3) powders are weighed according to the atomic molar ratio of In:Sn:Zn:Tb:Sb=0.62:0.13:0.26:0.0005:0.0195, and the total weight of the powder is 6 kg. The rest is the same as the preparation method in Example 1.
[0188] Example 16
[0189] An oxide target material comprises an oxide of element A, an oxide of element B, an oxide of element R and an oxide of element M;
[0190] The element A is indium (In);
[0191] The element B is gallium (Ga);
[0192] The element R is praseodymium (Pr);
[0193] The element M is titanium (Ti);
[0194] In the above oxide target, the atomic molar ratios of elements A, B, R and M in the oxide target are x, y, z and m respectively, wherein x=0.76, y=0.21, z=0.025, and m=0.005.
[0195] That is, the molar ratio of metal atoms in the target material satisfies In:Ga:Pr:Ti=0.76:0.21:0.025:0.005.
[0196] The above oxide target is prepared by the following method:
[0197] Step 1: Press the powder into a target blank;
[0198] Step 1.1: First, weigh the oxide powders of elements A, B, R, and M according to the proportion of the above-mentioned target material, with a total weight of 3kg. Premix the oxide of element R, the oxide of element M, a dispersant, and pure water, wherein the dispersant is polyvinyl pyrrolidone, which accounts for 1.5% of the total mass after mixing, and the solid content of the mixture is 45%. After the above-mentioned mixture is ultrasonically pre-dispersed for 30 minutes, it is ground into slurry 1 with a sand mill at a speed of 1000 rpm and a grinding time of 10 hours; the average particle size of the mixed powder in slurry 1 is less than 0.8μm, and vacuum degassing is performed; then, the oxide of element A and the oxide of element B are added to slurry 1 in sequence, and after each oxide is added, polyvinyl pyrrolidone accounting for 1.5% of the total mass ratio after mixing and an appropriate amount of pure water are added accordingly to make the solid content of the mixture 40%. The mixture was ultrasonically pre-dispersed for 30 minutes, and then ground into slurry 2 with a sand mill at a speed of 1000 rpm for 20 hours; finally, polyvinyl alcohol and polyethylene glycol were added to slurry 2, each accounting for 1.5% of the total mass after mixing, and ground with a sand mill for 5 hours. The average particle size of the mixed powder in the final slurry was less than 0.8 μm, and vacuum degassing was performed;
[0199] Step 1.2: The final slurry is spray granulated at a granulation temperature of 180°C and a feed rate of 10 rpm; after drying, the particle size D of the granulated powder is screened. 50 <2μm;
[0200] Step 1.3: The screened powder is molded under a hydraulic press at a pressure of 80 MPa for 5 minutes; then further pressed by isostatic pressing at a pressure of 300 MPa for 20 minutes;
[0201] Step 2: After drying the target blank, degreasing is performed; specifically, the target blank is heated to 700°C at a heating rate of 0.5°C / min; the degreasing time is 70 hours;
[0202] Step 3: heating from 700°C to a first sintering temperature of 1300°C at a first heating rate of 1°C / min, and keeping the temperature for 10 hours in a gas environment with an ozone content of 5-8% in the air; heating to a second sintering temperature of 1420°C at a second heating rate of 8°C / min, and keeping the temperature for 30 minutes in a gas environment with an ozone content of 10-15% in the air; then cooling to a first sintering temperature of 1300°C at a first cooling rate of 3°C / min, and filling with water vapor at a flow rate of 0.1-1L / min during the cooling process, and keeping the temperature for 10 hours in a gas environment with an ozone content of 10-15% in the air;
[0203] Rapidly heat up to the second sintering temperature of 1480°C at a heating rate of 8°C / min, and keep the temperature for 30 minutes in a gas environment with an ozone content of 10-15% in the air; then cool down to the first sintering temperature of 1300°C at a cooling rate of 3°C / min, and fill with water vapor at a flow rate of 0.1-1L / min during the cooling process, and keep the temperature for 10 hours in a gas environment with an ozone content of 10-15% in the air;
[0204] Step 4: In a gas environment where the ozone content in air is 10-15%, cooling to room temperature at a second cooling rate of 1°C / min to obtain a target sintered body;
[0205] Step 5: After machining the obtained target sintered body, bind it to the metal back plate using indium binding.
[0206] Embodiment 17
[0207] An oxide target material comprises an oxide of element A, an oxide of element R and an oxide of element M;
[0208] The element A is indium (In);
[0209] The element R is praseodymium (Pr);
[0210] The element M is titanium (Ti);
[0211] In the above oxide target, the atomic molar ratios of elements A, R and M in the oxide target are x, z and m respectively, wherein x=0.93, z=0.05 and m=0.02.
[0212] In the method for preparing oxide targets, indium oxide (In2O3), praseodymium oxide (Pr6O 11 ) and titanium oxide (TiO2) powders were weighed according to the atomic molar ratio of In:Pr:Ti=0.93:0.05:0.02, and the total weight of the powders was 3 kg. The rest was the same as the preparation method in Example 16.
[0213] Embodiment 18
[0214] An oxide target material comprises an oxide of element A, an oxide of element B, an oxide of element R and an oxide of element M;
[0215] The element A is indium (In);
[0216] The element B is gallium (Ga);
[0217] The element R is terbium (Tb);
[0218] The element M is silicon (Si);
[0219] In the above oxide target, the atomic molar ratios of elements A, B, R and M in the oxide target are x, y, z and m respectively, wherein x=0.81, y=0.17, z=0.008, and m=0.012.
[0220] In the preparation method of the oxide target material, indium oxide (In2O3), gallium oxide (Ga2O3), terbium oxide (Tb4O7) and silicon oxide (SiO2) powders are weighed according to the atomic molar ratio of In:Ga:Tb:Si=0.81:0.17:0.008:0.012. The total weight of the powder is 3 kg, and the rest is the same as the preparation method of Example 16.
[0221] Embodiment 19
[0222] An oxide target material comprises an oxide of element A, an oxide of element B, an oxide of element R and an oxide of element M;
[0223] The element A is indium (In);
[0224] The element B is gallium (Ga);
[0225] The element R is terbium (Tb);
[0226] The element M is tantalum (Ta);
[0227] In the above oxide target, the atomic molar ratios of elements A, B, R and M in the oxide target are x, y, z and m respectively, wherein x=0.74, y=0.24, z=0.006, and m=0.014.
[0228] In the preparation method of the oxide target material, indium oxide (In2O3), gallium oxide (Ga2O3), terbium oxide (Tb4O7) and tantalum oxide (Ta2O5) powders are weighed according to the atomic molar ratio of In:Ga:Tb:Ta=0.74:0.24:0.006:0.014. The total weight of the powder is 3 kg, and the rest is the same as the preparation method of Example 16.
[0229] Embodiment 20
[0230] An oxide target material comprises an oxide of element A, an oxide of element B, an oxide of element R and an oxide of element M;
[0231] The element A is indium (In);
[0232] The element B is zinc (Zn);
[0233] The element R is praseodymium (Pr);
[0234] The element M is scandium (Sc);
[0235] In the above oxide target, the atomic molar ratios of elements A, B, R and M in the oxide target are x, y, z and m respectively, wherein x=0.65, y=0.32, z=0.015, m=0.015.
[0236] In the method for preparing oxide targets, indium oxide (In2O3), zinc oxide (ZnO), praseodymium oxide (Pr6O 11 ) and scandium oxide (Sc2O3) powders were weighed according to the atomic molar ratio of In:Zn:Pr:Sc=0.65:0.32:0.015:0.015, and the total weight of the powders was 3 kg. The rest was the same as the preparation method in Example 16.
[0237] Embodiment 21
[0238] An oxide target material comprises an oxide of element A, an oxide of element B, an oxide of element R and an oxide of element M;
[0239] The element A is indium (In);
[0240] The element B is zinc (Zn);
[0241] The element R is praseodymium (Pr);
[0242] The element M is titanium (Ti);
[0243] In the above oxide target, the atomic molar ratios of elements A, B, R and M in the oxide target are x, y, z and m respectively, wherein x=0.65, y=0.32, z=0.012 and m=0.018.
[0244] In the method for preparing oxide targets, indium oxide (In2O3), zinc oxide (ZnO), praseodymium oxide (Pr6O 11 ) and titanium oxide (TiO2) powders were weighed according to the atomic molar ratio of In:Zn:Pr:Ti=0.65:0.32:0.012:0.018. The total weight of the powders was 3 kg. The rest was the same as the preparation method in Example 16.
[0245] Embodiment 22
[0246] An oxide target material comprises an oxide of element A, an oxide of element B, an oxide of element R and an oxide of element M;
[0247] The element A is indium (In);
[0248] The element B is zinc (Zn);
[0249] The element R is terbium (Tb);
[0250] The element M is silicon (Si);
[0251] In the above oxide target, the atomic molar ratios of elements A, B, R and M in the oxide target are x, y, z and m respectively, wherein x=0.76, y=0.23, z=0.005, m=0.005.
[0252] In the preparation method of the oxide target material, indium oxide (In2O3), zinc oxide (ZnO), terbium oxide (Tb4O7) and silicon oxide (SiO2) powders are weighed according to the atomic molar ratio of In:Zn:Tb:Si=0.76:0.23:0.005:0.005, and the total weight of the powder is 3 kg. The rest is the same as the preparation method of Example 16.
[0253] Embodiment 23
[0254] An oxide target material comprises an oxide of element A, an oxide of element B, an oxide of element R and an oxide of element M;
[0255] The element A is indium (In);
[0256] The element B is zinc (Zn);
[0257] The element R is terbium (Tb);
[0258] The element M is tantalum (Ta);
[0259] In the above oxide target, the atomic molar ratios of elements A, B, R and M in the oxide target are x, y, z and m respectively, wherein x=0.8, y=0.18, z=0.008, and m=0.012.
[0260] In the preparation method of the oxide target material, indium oxide (In2O3), zinc oxide (ZnO), terbium oxide (Tb4O7) and tantalum oxide (Ta2O5) powders are weighed according to the atomic molar ratio of In:Zn:Tb:Ta=0.8:0.18:0.008:0.012. The total weight of the powder is 3 kg, and the rest is the same as the preparation method of Example 16.
[0261] Embodiment 24
[0262] An oxide target material comprises an oxide of element A, an oxide of element B, an oxide of element R and an oxide of element M;
[0263] The element A is indium (In);
[0264] The element B is gallium (Ga) and zinc (Zn), and the molar ratio of gallium to zinc is 1:1;
[0265] The element R is praseodymium (Pr);
[0266] The element M is scandium (Sc);
[0267] In the above oxide target, the atomic molar ratios of elements A, B, R and M in the oxide target are x, y, z and m respectively, wherein x=0.62, y=0.36, z=0.015 and m=0.005.
[0268] In the method for preparing oxide targets, indium oxide (In2O3), gallium oxide (Ga2O3), zinc oxide (ZnO), praseodymium oxide (Pr6O 11 ) and scandium oxide (Sc2O3) powders were weighed according to the atomic molar ratio of In:Ga:Zn:Pr:Sc=0.62:0.18:0.18:0.015:0.005. The total weight of the powders was 3 kg, and the rest was the same as the preparation method in Example 16.
[0269] Embodiment 25
[0270] An oxide target material comprises an oxide of element A, an oxide of element B, an oxide of element R and an oxide of element M;
[0271] The element A is indium (In);
[0272] The element B is gallium (Ga) and zinc (Zn), and the molar ratio of gallium to zinc is 1:1;
[0273] The element R is terbium (Tb);
[0274] The element M is titanium (Ti);
[0275] In the above oxide target, the atomic molar ratios of elements A, B, R and M in the oxide target are x, y, z and m respectively, wherein x=0.65, y=0.32, z=0.02 and m=0.01.
[0276] In the preparation method of the oxide target material, indium oxide (In2O3), gallium oxide (Ga2O3), zinc oxide (ZnO), terbium oxide (Tb4O7) and titanium oxide (TiO2) powders are weighed according to the atomic molar ratio of In:Ga:Zn:Tb:Ti=0.65:0.16:0.16:0.02:0.01. The total weight of the powder is 3 kg, and the rest is the same as the preparation method of Example 16.
[0277] Embodiment 26
[0278] An oxide target material comprises an oxide of element A, an oxide of element B, an oxide of element R and an oxide of element M;
[0279] The element A is indium (In);
[0280] The element B is gallium (Ga) and zinc (Zn), and the molar ratio of gallium to zinc is 1:6;
[0281] The element R is praseodymium (Pr);
[0282] The element M is silicon (Si);
[0283] In the above oxide target, the atomic molar ratios of elements A, B, R and M in the oxide target are x, y, z and m, respectively, where x=0.76, y=0.21, z=0.016, and m=0.014.
[0284] In the method for preparing oxide targets, indium oxide (In2O3), gallium oxide (Ga2O3), zinc oxide (ZnO), praseodymium oxide (Pr6O 11 ) and silicon oxide (SiO2) powders are weighed according to the atomic molar ratio of In:Ga:Zn:Pr:Si=0.76:0.03:0.18:0.016:0.014. The total weight of the powder is 3 kg. The rest is the same as the preparation method in Example 16.
[0285] Embodiment 27
[0286] An oxide target material comprises an oxide of element A, an oxide of element B, an oxide of element R and an oxide of element M;
[0287] The element A is indium (In);
[0288] The element B is gallium (Ga) and zinc (Zn), and the molar ratio of gallium to zinc is 1:4;
[0289] The element R is terbium (Tb);
[0290] The element M is tantalum (Ta);
[0291] In the above oxide target, the atomic molar ratios of elements A, B, R and M in the oxide target are x, y, z and m respectively, wherein x=0.76, y=0.22, z=0.008, and m=0.012.
[0292] In the preparation method of the oxide target material, indium oxide (In2O3), gallium oxide (Ga2O3), zinc oxide (ZnO), terbium oxide (Tb4O7) and tantalum oxide (Ta2O5) powders are weighed according to the atomic molar ratio of In:Ga:Zn:Tb:Ta=0.76:0.044:0.176:0.008:0.012. The total weight of the powder is 3 kg, and the rest is the same as the preparation method of Example 16.
[0293] Embodiment 28
[0294] An oxide target material comprises an oxide of element A, an oxide of element B, an oxide of element R and an oxide of element M;
[0295] The element A is indium (In);
[0296] The element B is gallium (Ga) and zinc (Zn), and the molar ratio of gallium to zinc is 1:3;
[0297] The element R is terbium (Tb);
[0298] The element M is antimony (Sb);
[0299] In the above oxide target, the atomic molar ratios of elements A, B, R and M in the oxide target are x, y, z and m respectively, wherein x=0.85, y=0.12, z=0.015, m=0.015.
[0300] In the preparation method of the oxide target material, indium oxide (In2O3), gallium oxide (Ga2O3), zinc oxide (ZnO), terbium oxide (Tb4O7) and antimony oxide (Sb2O3) powders are weighed according to the atomic molar ratio of In:Ga:Zn:Tb:Sb=0.85:0.03:0.09:0.015:0.015. The total weight of the powder is 3 kg, and the rest is the same as the preparation method of Example 16.
[0301] Embodiment 29
[0302] An oxide target material comprises an oxide of element A, an oxide of element B, an oxide of element R and an oxide of element M;
[0303] The element A is indium (In);
[0304] The element B is gallium (Ga) and zinc (Zn), and the molar ratio of gallium to zinc is 1:2;
[0305] The element R is praseodymium (Pr);
[0306] The element M is antimony (Sb);
[0307] In the above oxide target, the atomic molar ratios of elements A, B, R and M in the oxide target are x, y, z and m respectively, wherein x=0.76, y=0.21, z=0.012, and m=0.018.
[0308] In the method for preparing oxide targets, indium oxide (In2O3), gallium oxide (Ga2O3), zinc oxide (ZnO), praseodymium oxide (Pr6O 11) and antimony oxide (Sb2O3) powders were weighed according to the atomic molar ratio of In:Ga:Zn:Pr:Sb=0.76:0.07:0.14:0.012:0.018. The total weight of the powders was 3 kg, and the rest was the same as the preparation method in Example 16.
[0309] Embodiment 30
[0310] An oxide target material comprises an oxide of element A, an oxide of element B, an oxide of element R and an oxide of element M;
[0311] The element A is indium (In);
[0312] The element B is gallium (Ga) and zinc (Zn), and the molar ratio of gallium to zinc is 1:6;
[0313] The element R is terbium (Tb);
[0314] The element M is antimony (Sb);
[0315] In the above oxide target, the atomic molar ratios of elements A, B, R and M in the oxide target are x, y, z and m respectively, wherein x=0.76, y=0.21, z=0.012, and m=0.018.
[0316] In the preparation method of the oxide target material, indium oxide (In2O3), gallium oxide (Ga2O3), zinc oxide (ZnO), terbium oxide (Tb4O7) and antimony oxide (Sb2O3) powders are weighed according to the atomic molar ratio of In:Ga:Zn:Tb:Sb=0.76:0.03:0.18:0.012:0.018. The total weight of the powder is 3 kg, and the rest is the same as the preparation method of Example 16.
[0317] Comparative Example 1
[0318] Compared with Example 2, the atomic molar ratio of the metal elements In:Ga:Zn:Pr=0.64:0.11:0.22:0.015 in the oxide target is kept unchanged in this comparative example, but no oxide of M is added in this comparative example, and other parameters and preparation process are consistent with Example 2.
[0319] Comparative Example 2
[0320] The difference between this comparative example and Example 2 is that the atomic molar ratios of elements A, B, R and M in the oxide target are x, y, z and m, respectively, where x = 0.64, y = 0.33, z = 0.015, and m = 0.03. Other parameters and preparation process are consistent with Example 2.
[0321] Comparative Example 3
[0322] The difference between this comparative example and Example 2 is that the atomic molar ratios of elements A, B, R and M in the oxide target are x, y, z and m, respectively, where x = 0.64, y = 0.33, z = 0.015, and m = 0.05. Other parameters and preparation process are consistent with Example 2.
[0323] Comparative Example 4
[0324] The difference between this comparative example and Example 11 is that there is no process of the second sintering temperature in this comparative example, and only the first sintering temperature is maintained, that is, the specific method of step 3 in this comparative example is:
[0325] Step 3: Heat the temperature from 700°C to a first sintering temperature of 1250°C at a first heating rate of 1°C / min, and keep the temperature for 10 hours in a gas environment with an oxygen content of 20-30% in air; and continue to keep the temperature for 30 hours at the first sintering temperature of 1250°C in a gas environment with an oxygen content of 40-50% in air.
[0326] Other parameters and preparation process are the same as those in Example 11.
[0327] Comparative Example 5
[0328] The difference between Comparative Example 5 and Example 11 is that the insulation time of each first sintering temperature in Comparative Example 5 is only 5 hours, and the total insulation time of the first sintering temperature is 20 hours, that is, the specific method of step 3 in this comparative example is:
[0329] Step 3: heating from 700°C to a first sintering temperature of 1250°C at a first heating rate of 1°C / min, and keeping the temperature for 5 hours in a gas environment with an oxygen content of 20-30% in air; heating to a second sintering temperature of 1420°C at a second heating rate of 8°C / min, and keeping the temperature for 30 minutes in a gas environment with an oxygen content of 40-50% in air; then cooling to a first sintering temperature of 1250°C at a first cooling rate of 3°C / min, and keeping the temperature for 5 hours in a gas environment with an oxygen content of 40-50% in air;
[0330] Rapidly heat up to the second sintering temperature of 1460°C at a heating rate of 8°C / min, and keep warm for 30 minutes in a gas environment with an oxygen content of 40-50% in air; then cool down to the first sintering temperature of 1250°C at a cooling rate of 3°C / min, and keep warm for 5 hours in a gas environment with an oxygen content of 40-50% in air;
[0331] The temperature was rapidly increased to the second sintering temperature of 1500°C at a heating rate of 8°C / min, and kept warm for 30 minutes in a gas environment with an oxygen content of 60-70% in air; then the temperature was reduced to the first sintering temperature of 1250°C at a cooling rate of 3°C / min, and kept warm for 5 hours in a gas environment with an oxygen content of 40-50% in air.
[0332] Other parameters and preparation process are the same as those in Example 11.
[0333] Comparative Example 6
[0334] The difference between Comparative Example 6 and Example 11 is that each holding time of the second sintering temperature is 5 hours, and the total holding time of the second sintering temperature is 15 hours, that is, the specific method of step 3 in this comparative example is:
[0335] Step 3: heating from 700°C to a first sintering temperature of 1250°C at a first heating rate of 1°C / min, and keeping the temperature for 10 hours in a gas environment with an oxygen content of 20-30% in air; heating to a second sintering temperature of 1420°C at a second heating rate of 8°C / min, and keeping the temperature for 5 hours in a gas environment with an oxygen content of 40-50% in air; then cooling to a first sintering temperature of 1250°C at a first cooling rate of 3°C / min, and keeping the temperature for 10 hours in a gas environment with an oxygen content of 40-50% in air;
[0336] Rapidly heat up to the second sintering temperature of 1460°C at a heating rate of 8°C / min, and keep warm for 5 hours in a gas environment with an oxygen content of 60-70% in air; then cool down to the first sintering temperature of 1250°C at a cooling rate of 3°C / min, and keep warm for 10 hours in a gas environment with an oxygen content of 60-70% in air;
[0337] The temperature was rapidly increased to the second sintering temperature of 1500°C at a heating rate of 8°C / min, and kept warm for 5 hours in a gas environment with an oxygen content of 60-70% in air; then the temperature was reduced to the first sintering temperature of 1250°C at a cooling rate of 3°C / min, and kept warm for 10 hours in a gas environment with an oxygen content of 60-70% in air.
[0338] Other parameters and preparation process are the same as those in Example 11.
[0339] Comparative Example 7
[0340] The difference between Comparative Example 7 and Example 11 is that the sintering process is not repeated in this comparative example, the total holding time of the first sintering temperature is 20 hours, and the holding time of the second sintering temperature is 0.5 hours. That is, the specific method of step 3 of this comparative example is:
[0341] Step 3: Heat the temperature from 700°C to a first sintering temperature of 1250°C at a first heating rate of 1°C / min, and keep the temperature for 10 hours in a gas environment with an oxygen content of 20-30% in air; heat the temperature to a second sintering temperature of 1420°C at a second heating rate of 8°C / min, and keep the temperature for 30 minutes in a gas environment with an oxygen content of 40-50% in air; then cool the temperature to a first sintering temperature of 1250°C at a first cooling rate of 3°C / min, and keep the temperature for 10 hours in a gas environment with an oxygen content of 40-50% in air.
[0342] Other parameters and preparation process are the same as those in Example 11.
[0343] Target performance test
[0344] Conventional characterization methods were used, including testing the resistivity of the target block with a four-probe device, testing the target material grain size with a crystal phase microscope by wet chemical polishing, testing the target material relative density by a water displacement method, and testing the element distribution by a scanning electron microscope. The resistivity, grain size, relative density, and element distribution of the oxide targets prepared in Examples 1 to 30 and Comparative Examples 1 to 7 were tested respectively, and the test results are shown in Table 1.
[0345] Table 1
[0346]
[0347]
[0348] It can be seen from Table 1 that the oxide targets prepared in Examples 1 to 30 of the present invention all have lower resistivity, extremely small grain size, higher relative density and uniform element distribution.
[0349] From the comparison between Comparative Example 1 and Example 2, it can be seen that the relative density of the oxide target prepared without adding M oxide is reduced, the grain size is significantly increased, and the target element distribution is uneven.
[0350] From the comparison between Comparative Examples 2 to 3 and Example 2, it can be seen that when the added oxide of M is too high, the resistivity of the oxide target increases to a certain extent, the grain size is smaller, but the relative density decreases to a certain extent.
[0351] By comparing Comparative Example 4 with Example 11, it can be seen that the resistivity of the oxide target prepared by the sintering procedure that only maintains the first sintering temperature is significantly increased (105.1 mΩ·cm), the density is greatly reduced to only 82.2%, and the elements are also unevenly distributed; indicating that the oxide target is not fully sintered and cannot meet the requirements of actual applications.
[0352] By comparing Comparative Example 5 with Example 11, it can be seen that when the holding time of the first sintering temperature is insufficient, the resistivity of the prepared oxide target increases (65.2 mΩ·cm), the relative density decreases (92.5%), and the elements are also unevenly distributed; indicating that the target is not fully sintered and cannot meet the requirements of actual application.
[0353] By comparing Comparative Example 6 with Example 11, it can be seen that when the second sintering temperature is maintained for too long, the resistivity of the prepared oxide target is comparable (5.5 mΩ·cm), the relative density is high (99.4%), but the element distribution is uneven, and the grain size of the target is significantly increased to 15.4 μm, indicating that the target is over-sintered and cannot meet the requirements of actual applications.
[0354] Comparison between Comparative Example 7 and Example 11 shows that the resistivity of the oxide target prepared without repeated sintering increases (45.6 mΩ·cm) and the relative density decreases (90.1%), indicating that the target is not fully sintered and cannot meet the requirements of practical applications.
[0355] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. An oxide target material, characterized in that: The raw materials are oxides of element A, element B, element R and element M; The element A is indium; The element B is one or a combination of two or more of gallium and zinc; The element R is one or a combination of two or more of cerium, praseodymium, dysprosium and terbium; The element M is one or a combination of two or more of scandium, silicon, titanium, germanium, and antimony; The atomic molar ratios of elements A, B, R and M in the oxide target are x, y, z and m respectively, wherein 0.6≤x≤0.9994, 0.08≤y≤0.3994, 0.0005≤z≤0.05, 0.001≤m≤0.02, x+y+z+m=1; The resistivity of the oxide target is less than 10 mΩ·cm, and the relative density of the oxide target is more than 98.5%; The oxide target is prepared by the following method: Step 1, pressing the powder into a target blank; Step 2, drying the target blank and then degreasing it; Step 3, the degreased target blank is further heated to the first sintering temperature at a first heating rate in a gas environment, and then is further heated to the second sintering temperature at a second heating rate, and finally is cooled to the first sintering temperature at a first cooling rate and continues to sinter; the first heating rate is 0.1-5°C / min, and the first sintering temperature is 1200-1400°C; the second heating rate is 5-10°C / min, and the second sintering temperature is 1410-1600°C; the sintering process is repeated multiple times; each holding time at the first sintering temperature is 10-250 hours; each holding time at the second sintering temperature is 10-60 minutes; Step 4: After sintering, the temperature is lowered at a second cooling rate to room temperature in a gas environment to obtain a target material sintered body; Step 5: Processing and binding the target sintered body.
2. The oxide target according to claim 1, characterized in that 0.76≤x≤0.9994, 0.005≤m≤0.
015.
3. The oxide target according to claim 1, characterized in that The maximum particle size of the oxide target grains is less than 8 μm.
4. The oxide target according to claim 1, characterized in that The degreasing treatment in step 2 is to first raise the temperature of the target blank to 600-800° C. at a heating rate of 0.2-1° C. / min; the degreasing time is 50-100 hours.
Citation Information
Patent Citations
Oxide semiconductor thin film and thin film transistor prepared from same
CN107146816A
Method for preparing high-compact ITO target material through two-step sintering
CN106977179A
Indium tin tantalum ytterbium oxide powder and preparation method and application thereof