A method for simultaneously removing arsenic and antimony from yellow phosphorus
By using a combination method of aqueous basic oxidant, dispersant and catalyst in yellow phosphorus, the removal temperature and energy consumption of arsenic and antimony in yellow phosphorus are reduced, and the problem of difficulty in separation of arsenic and antimony in yellow phosphorus in the prior art is solved. , realizes the production of high-purity yellow phosphorus.
Patent Information
- Application Number
- CN202310241160.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-14
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-03-14
Smart Images

Figure CN116216670B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of yellow phosphorus processing, and in particular to a method for simultaneously removing arsenic and antimony from yellow phosphorus. Background Art
[0002] Yellow phosphorus is an important phosphorus chemical raw material, especially high-purity phosphorus chemical products. High-purity yellow phosphorus is mainly used to produce food, pharmaceutical-grade phosphates, electronic-grade phosphorus derivatives or electronic-grade phosphoric acid, etc. It is widely used in the production of food additives, medicines, microelectronic integrated circuit etching cleaning agents, advanced lubricant additives, semiconductor diffusion additives, etc. These application fields have strict requirements on the impurity content in yellow phosphorus, among which the arsenic content and antimony content are required to be less than 20ppm, or even lower.
[0003] Although my country's industrial yellow phosphorus production capacity ranks first in the world, the quality of yellow phosphorus products is not graded. The main impurities are organic matter, arsenic, and iron, followed by antimony, zinc, copper, nickel, and lead. The total content of other impurities is at the 10-9 level; among them, organic matter is mainly polynuclear aromatic hydrocarbons, which have a strong affinity with yellow phosphorus. Arsenic mainly exists in the form of arsenic phosphide and easily forms eutectics with phosphorus. Although antimony, phosphorus, and arsenic belong to the same main group elements, they belong to different periods. The interlayer covalency of arsenic is stronger than that of antimony, and the distance between the layers is also farther than that of antimony, resulting in antimony's metallic properties being stronger than arsenic. Under acidic conditions, arsenic is more easily oxidized than antimony. Antimony is closely combined with phosphorus, and it is impossible to separate antimony and phosphorus by water extraction or filtration alone. It is one of the more difficult metals to remove.
[0004] In industrial yellow phosphorus, the arsenic content is generally 100-300ppm, and the antimony content is generally 100-300ppm. Moreover, with the depletion of phosphate ore, the arsenic and antimony contents in industrial yellow phosphorus tend to increase gradually, which has a great impact on the quality of yellow phosphorus. Since arsenic and antimony belong to the same main group elements as phosphorus and have many similar physical and chemical properties, in the process of electric furnace phosphorus production, arsenic and antimony are reduced while reducing phosphorus. Arsenic and antimony are condensed into the yellow phosphorus product at the same time, making it difficult to separate yellow phosphorus from arsenic and antimony.
[0005] There are chemical and physical methods for purifying yellow phosphorus. The main physical methods include vacuum distillation, activated carbon adsorption, electromagnetic purification, extraction purification, regional melting, microfiltration purification, etc., but the phosphorus yield of physical purification methods is generally low, generally only 60-80%, not more than 90%. The chemical method mainly purifies single impurities in yellow phosphorus. Wan Ronghui et al. mixed yellow phosphorus with a nitric acid solution with a concentration of 10%-12% (mass fraction) in patent CN101327917, and stirred the reaction at 70°C with sodium bromate as an oxidation enhancer. Arsenic was oxidized and hydrated to arsenous acid or arsenic acid and entered the water phase. After 3 hours, the dearsenified yellow phosphorus was removed, and its dearsenification rate was ≥96%, and the phosphorus yield was ≥92%. Lin Jun et al. introduced in a method for removing antimony from yellow phosphorus (CN103771365A) that an oxidizing antimony removal agent (5-30% nitric acid solution) is fully mixed and contacted with yellow phosphorus in a molten state in a ratio of 1:1-5, and the reaction is leached at 60-80°C for 10-60 minutes to make the antimony in the yellow phosphorus enter the liquid phase, and the phosphorus phase is separated from the liquid phase to achieve the purpose of removing antimony. The above methods are all carried out in an acidic environment of nitric acid, and nitrate ions are introduced, which affects the stability of product quality, and the reaction temperature of the purification process is high, and the reaction is more intense. CN112875661A discloses a method for producing electronic grade yellow phosphorus, which uses oxidants such as polyphosphoric acid and hydrogen peroxide to purify yellow phosphorus under a protective atmosphere to obtain electronic grade yellow phosphorus with higher purity, but its removal effect on arsenic and antimony is unknown.
[0006] In summary, the existing technology usually aims at removing a single impurity in yellow phosphorus, so it is urgent to develop a technology for simultaneously removing arsenic and antimony impurities in yellow phosphorus to simplify the purification process of yellow phosphorus. Summary of the invention
[0007] The purpose of the present invention is to provide a method for simultaneously removing arsenic and antimony from yellow phosphorus, so as to solve the problem of complicated processes for removing arsenic and antimony from yellow phosphorus.
[0008] In order to solve the above technical problems, the present invention adopts the following technical scheme: a method for simultaneously removing arsenic and antimony from yellow phosphorus, characterized in that: the yellow phosphorus liquefied by heating and the aqueous phase basic oxidant are fully stirred and mixed in a reactor under the condition of hot water liquid sealing, and a dispersant, an acidulant and a catalyst are added, and stirred at 55-65°C to allow the arsenic and antimony impurities in the yellow phosphorus to enter the aqueous phase after reaction, and then washed and allowed to stand for phase separation to obtain high-purity yellow phosphorus with low arsenic and antimony.
[0009] A further technical solution is that the method comprises the following specific steps:
[0010] (a) Material preheating, mixing and acidification: preheat the raw material yellow phosphorus to 50°C-70°C to fully liquefy, preheat the basic oxidant to 50-60°C and add it to the reactor to keep warm, then add the liquid yellow phosphorus to the reactor, add the acidifier, and stir and mix for 10-15 minutes to acidify;
[0011] (b) Dispersion: After heating the reaction system to 55-70°C, add a dispersant and stir for 5-10 minutes to fully disperse the yellow phosphorus;
[0012] (c) Catalytic oxidation: adding a catalyst for catalytic oxidation, heating the reaction system materials to 55-65° C., and stirring and mixing for 1-3 hours;
[0013] (d) Washing: After the reaction is completed, the reaction system is allowed to stand for 10 to 30 minutes. After the yellow phosphorus phase and the water phase are fully separated, the yellow phosphorus is transferred to a water washing tank and washed with hot pure water at 55 to 70° C. until the washing water is neutral.
[0014] (e) Separation and packaging: After washing, the washing system materials are allowed to stand for 10 to 30 minutes. After the yellow phosphorus phase and the water phase are fully separated, the yellow phosphorus is transported to the packaging system. After packaging, a high-purity yellow phosphorus product with low arsenic and antimony content is obtained.
[0015] A further technical solution is that the basic oxidant is hydrogen peroxide with a concentration of 5-15% and an added amount of 3-7 times the mass of yellow phosphorus.
[0016] A further technical solution is that the acidulant is at least one of phosphoric acid or polyphosphoric acid, the amount of the acidulant added is 0.1-1% of the mass of the basic oxidant, the phosphoric acid concentration is 82%-85%, and the mass concentration of phosphoric acid in polyphosphoric acid is 105%-116%.
[0017] A further technical solution is that the catalyst is one or more of hydroiodic acid, sodium iodide, sodium bromide, and elemental bromine, and the added amount of the catalyst is 0.01-0.1% of the mass of yellow phosphorus.
[0018] A further technical solution is that the dispersant is at least one of hexadecyltrimethylammonium bromide, sodium lignin sulfonate and polyethylene glycol, and the added amount of the dispersant is 0.05-0.1% of the mass of the basic oxidant.
[0019] A further technical solution is that the hot pure water is heated desalted water or deionized water.
[0020] A further technical solution is that the stirring linear speed is 0.2-2 m / s.
[0021] Reaction mechanism: Hydrogen peroxide is used as the basic oxidant, and a small amount of phosphoric acid or polyphosphoric acid is added as an acidifier, without introducing new impurity ions. Because yellow phosphorus itself is not compatible with water, in the ordinary yellow phosphorus purification process, the contact area between the yellow phosphorus phase and the water phase can only be increased by stirring, thereby increasing the reaction rate, but stirring alone still cannot achieve efficient mixing of the yellow phosphorus phase and the water phase. Before adding the catalyst, a dispersant that is conducive to the dispersion of yellow phosphorus is added. Under the action of stirring, the yellow phosphorus is dispersed in the water phase in the form of emulsion-like fine particles, which greatly increases the contact area between the yellow phosphorus and the water phase. After the catalyst is added, the reaction probability of arsenic and antimony in yellow phosphorus and the oxidant is increased, thereby increasing the reaction rate and the efficiency of arsenic removal and antimony removal. Through the action of the dispersant and the catalyst, the reaction temperature is reduced to 55-65°C, which is lower than the conventional 70-75°C, which not only reduces energy consumption, but also greatly reduces the loss of the basic oxidant hydrogen peroxide, and reduces the cost of arsenic removal and antimony removal.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] 1. The present invention adopts hydrogen peroxide as a basic oxidant, and adds a small amount of phosphoric acid or polyphosphoric acid as an acidulant, thereby avoiding the safety risk caused by the large amount of nitric acid used in the conventional method, and reducing the influence of nitrate ions on the system. In the de-arsenication and de-antimony purification process of yellow phosphorus, part of the phosphorus is inevitably oxidized into phosphoric acid, while using phosphoric acid or polyphosphoric acid as an acidulant will not introduce new impurity ions.
[0024] 2. The yellow phosphorus is dispersed in the water phase into emulsified fine particles through the dispersant, which greatly increases the contact area between the yellow phosphorus and the water phase, thereby increasing the reaction rate and the efficiency of arsenic and antimony removal, while reducing the reaction temperature, reducing the loss of the basic oxidant, and reducing the production cost.
[0025] 3. The low-temperature catalytic oxidation process provided by the present invention can simultaneously remove arsenic and antimony impurities in yellow phosphorus at a relatively low temperature and normal pressure. Compared with the traditional method, the temperature and reaction intensity of arsenic removal and antimony removal of yellow phosphorus are greatly reduced, the reaction safety is greatly improved, and the high-temperature decomposition loss of the basic oxidant hydrogen peroxide is reduced. At the same time, it also has the advantages of simple production process flow, high yellow phosphorus yield, low energy consumption, low cost, and high product purity. The low-arsenic and low-antimony yellow phosphorus produced can provide key raw material guarantees for downstream processing and production of high-purity phosphorus pentoxide, high-purity phosphoric acid and other products. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION
[0027] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In all embodiments, unless otherwise specified, all ratios are mass ratios.
[0028] The examples of the present invention are all carried out in the following reactor, which is a 2000-liter jacketed heating reactor equipped with an adjustable speed stirring device and a reaction liquid temperature measuring device. The temperature of the yellow phosphorus dearsenicization and deantimony reaction can be adjusted and controlled by the jacket hot water temperature.
[0029] Example 1
[0030] Under normal pressure, 800 kg of 8% hydrogen peroxide solution was prepared as a basic oxidant, heated to 50°C and added to the reactor for insulation. 200 kg of yellow phosphorus (arsenic content of 258 ppm, antimony content of 184 ppm) was heated to 65°C and completely liquefied and then poured into the reactor. 4.0 kg of polyphosphoric acid with a phosphoric acid concentration of 105% was added, and the mixture was stirred at a stirring speed of 1 m / s for 15 minutes for acidification.
[0031] The reaction system was heated to 55°C, 800g of hexadecyltrimethylammonium bromide was added, and stirring was continued for 15 minutes to fully disperse the yellow phosphorus. Then 200g of hydroiodic acid was added, the reaction system was heated to 55°C, and stirring was continued for 2.5 hours.
[0032] After the reaction is completed, the yellow phosphorus is allowed to stand for 30 minutes, and then the yellow phosphorus is transported to a water washing tank, washed with 65°C desalted water until the washing water is neutral, and then allowed to stand for another 30 minutes. After the yellow phosphorus phase and the water phase are fully separated, the yellow phosphorus is transported to the packaging system, and after packaging, a low-arsenic, low-antimony, high-purity yellow phosphorus product is obtained. 197.1 kg of yellow phosphorus is obtained, and the arsenic content in the yellow phosphorus is 0.7 ppm, and antimony is not detected (detection limit 0.2 ppm).
[0033] Example 2
[0034] Under normal pressure, 600 kg of a 12% hydrogen peroxide solution was prepared as a basic oxidant, heated to 55°C and added to the reactor for insulation. 200 kg of yellow phosphorus (arsenic content of 258 ppm, antimony content of 184 ppm) was heated to 70°C and completely liquefied and then pumped into the reactor. 6.0 kg of polyphosphoric acid with a phosphoric acid concentration of 105% was added, and the mixture was stirred at a stirring speed of 0.5 m / s for 10 minutes for acidification.
[0035] The reaction system was heated to 55°C, 600 g of hexadecyltrimethylammonium bromide was added, and stirring was continued for 15 minutes to fully disperse the yellow phosphorus. 150 g of hydroiodic acid was added, the reaction system was heated to 60°C, and stirring was continued for 1.0 hour.
[0036] After the reaction is completed, the yellow phosphorus is allowed to stand for 30 minutes, and then transported to a water washing tank, washed with 70°C desalted water until the washing water is neutral, and then allowed to stand for another 30 minutes. After the yellow phosphorus phase and the water phase are fully separated, the yellow phosphorus is transported to the packaging system, and a low-arsenic, low-antimony, high-purity yellow phosphorus product is obtained after packaging. 196.4 kg of yellow phosphorus is obtained, and the arsenic content in the yellow phosphorus is 0.5 ppm and the antimony content is 0.3 ppm.
[0037] Example 3
[0038] Under normal pressure, 600 kg of a 12% hydrogen peroxide solution was prepared as a basic oxidant, heated to 60°C and added to the reactor for heat preservation. 200 kg of yellow phosphorus (arsenic content of 258 ppm, antimony content of 184 ppm) was heated to 60°C and completely liquefied and then poured into the reactor. 6.0 kg of polyphosphoric acid with a phosphoric acid concentration of 116% was added, and the mixture was stirred at a stirring speed of 0.2 m / s for 15 minutes for acidification.
[0039] The reaction system was heated to 56°C, 600 g of sodium lignin sulfonate was added, and stirring was continued for 10 minutes to fully disperse the yellow phosphorus. 150 g of elemental bromine was added, the reaction system was heated to 61°C, and stirring was continued for 1.0 hour.
[0040] After the reaction is completed, the yellow phosphorus is allowed to stand for 30 minutes, and then transported to a water washing tank, washed with 70°C desalted water until the washing water is neutral, and then allowed to stand for another 30 minutes. After the yellow phosphorus phase and the water phase are fully separated, the yellow phosphorus is transported to the packaging system, and after packaging, a low-arsenic, low-antimony, high-purity yellow phosphorus product is obtained. 197.6 kg of yellow phosphorus is obtained, and the arsenic content in the yellow phosphorus is 0.3 ppm, and antimony is not detected (detection limit 0.2 ppm).
[0041] Example 4
[0042] Under normal pressure, 800 kg of 8% hydrogen peroxide solution was prepared as a basic oxidant, heated to 60°C and added to the reactor for insulation. 200 kg of yellow phosphorus (arsenic content of 258 ppm, antimony content of 184 ppm) was heated to 70°C for liquefaction and then poured into the reactor. 8.0 kg of 85% phosphoric acid was added and stirred at a stirring speed of 1.5 m / s for 15 minutes for acidification.
[0043] The reaction system was heated to 70°C, 400 g of sodium lignin sulfonate was added, and stirring was continued for 5 minutes to fully disperse the yellow phosphorus. 100 g of sodium bromide was added, the reaction system was heated to 65°C, and stirring was continued for 2.0 hours.
[0044] After the reaction is completed, the yellow phosphorus is allowed to stand for 30 minutes, and then transported to a water washing tank, washed with 65°C desalted water until the washing water is neutral, and then allowed to stand for another 30 minutes. After the yellow phosphorus phase and the water phase are fully separated, the yellow phosphorus is transported to the packaging system, and a low-arsenic, low-antimony, high-purity yellow phosphorus product is obtained after packaging. 192.3 kg of yellow phosphorus is obtained, and the arsenic content in the yellow phosphorus is 0.2 ppm, and antimony is not detected (detection limit 0.2 ppm).
[0045] Example 5
[0046] Under normal pressure, 600 kg of a 15% hydrogen peroxide solution was prepared as a basic oxidant, heated to 54°C and added to the reactor for insulation. 200 kg of yellow phosphorus (arsenic content of 258 ppm, antimony content of 184 ppm) was heated to 50°C for liquefaction and then poured into the reactor. 5.0 kg of 85% phosphoric acid was added and stirred at a stirring speed of 1.5 m / s for 10 minutes for acidification.
[0047] The reaction system was heated to 70°C, 400 g of sodium lignin sulfonate was added, and stirring was continued for 5 minutes to fully disperse the yellow phosphorus. 100 g of elemental bromine was added, the reaction system was heated to 65°C, and stirring was continued for 2.0 hours.
[0048] After the reaction is completed, the yellow phosphorus is allowed to stand for 20 minutes, and then the yellow phosphorus is transported to a water washing tank, washed with deionized water at 65°C until the washing water is neutral, and then allowed to stand for 20 minutes. After the yellow phosphorus phase and the water phase are fully separated, the yellow phosphorus is transported to the packaging system, and a low-arsenic, low-antimony, high-purity yellow phosphorus product is obtained after packaging. 195.8 kg of yellow phosphorus is obtained, and the arsenic content in the yellow phosphorus is 0.5 ppm and the antimony content is 0.3 ppm.
[0049] Example 6
[0050] Under normal pressure, 800 kg of a hydrogen peroxide solution with a mass concentration of 8% was prepared as a basic oxidant, heated to 57°C and added to the reactor for insulation. 200 kg of yellow phosphorus (arsenic content of 258 ppm, antimony content of 184 ppm) was heated to 60°C for liquefaction and then poured into the reactor. 6.0 kg of phosphoric acid with a mass concentration of 82% was added, and the mixture was stirred at a stirring speed of 1.5 m / s for 15 minutes for acidification.
[0051] The reaction system was heated to 60°C, 400 g of sodium lignin sulfonate was added, and stirring was continued for 15 minutes to fully disperse the yellow phosphorus. 20 g of sodium iodide was added, the reaction system was heated to 62°C, and stirring was continued for 3.0 hours.
[0052] After the reaction is completed, the yellow phosphorus is allowed to stand for 20 minutes, and then the yellow phosphorus is transported to a water washing tank, washed with deionized water at 65°C until the washing water is neutral, and then allowed to stand for another 20 minutes. After the yellow phosphorus phase and the water phase are fully separated, the yellow phosphorus is transported to the packaging system, and a low-arsenic, low-antimony, high-purity yellow phosphorus product is obtained after packaging. 198.4 kg of yellow phosphorus is obtained, and the arsenic content in the yellow phosphorus is 0.8 ppm and the antimony content is 0.3 ppm.
[0053] Example 7
[0054] Under normal pressure, 800 kg of a hydrogen peroxide solution with a mass concentration of 8% was prepared as a basic oxidant, heated to 60°C and added to the reactor for insulation. 200 kg of yellow phosphorus (arsenic content of 258 ppm, antimony content of 184 ppm) was heated to 63°C for liquefaction and then poured into the reactor. 6.0 kg of phosphoric acid with a mass concentration of 84% was added, and the mixture was stirred at a stirring speed of 1.5 m / s for 15 minutes for acidification.
[0055] The reaction system was heated to 67°C, 600 g of hexadecyltrimethylammonium bromide was added, and stirring was continued for 15 minutes to fully disperse the yellow phosphorus. 20 g of sodium iodide was added, the reaction system was heated to 60°C, and stirring was continued for 3.0 hours.
[0056] After the reaction is completed, the yellow phosphorus is allowed to stand for 30 minutes, and then the yellow phosphorus is transported to a water washing tank, washed with deionized water at 65°C until the washing water is neutral, and then allowed to stand for another 30 minutes. After the yellow phosphorus phase and the water phase are fully separated, the yellow phosphorus is transported to the packaging system, and a low-arsenic, low-antimony, high-purity yellow phosphorus product is obtained after packaging. 195.3 kg of yellow phosphorus is obtained, and the arsenic content in the yellow phosphorus is 0.2 ppm, and antimony is not detected (detection limit 0.2 ppm).
[0057] Example 8
[0058] Under normal pressure, 1400 kg of a 5% hydrogen peroxide solution was prepared as a basic oxidant, heated to 60°C and added to the reactor for insulation. 200 kg of yellow phosphorus (arsenic content of 258 ppm, antimony content of 184 ppm) was heated to 70°C for liquefaction and then poured into the reactor. 14.0 kg of 85% phosphoric acid was added and stirred at a stirring speed of 2.0 m / s for 15 minutes for acidification.
[0059] The reaction system was heated to 60°C, 700 g of hexadecyltrimethylammonium bromide was added, and stirring was continued for 15 minutes to fully disperse the yellow phosphorus. 50 g of sodium bromide was added, the reaction system was heated to 65°C, and stirring was continued for 3.0 hours.
[0060] After the reaction is completed, the yellow phosphorus is allowed to stand for 30 minutes, and then the yellow phosphorus is transported to a water washing tank, washed with deionized water at 65°C until the washing water is neutral, and then allowed to stand for another 30 minutes. After the yellow phosphorus phase and the water phase are fully separated, the yellow phosphorus is transported to the packaging system, and a low-arsenic, low-antimony, high-purity yellow phosphorus product is obtained after packaging. 195.7 kg of yellow phosphorus is obtained, and the arsenic content in the yellow phosphorus is 0.2 ppm, and antimony is not detected (detection limit 0.2 ppm).
[0061] Example 9
[0062] Under normal pressure, prepare 1400 kg of a 7% hydrogen peroxide solution as a basic oxidant, heat it to 56°C and add it to the reactor to keep warm. Heat 200 kg of yellow phosphorus (arsenic content of 258 ppm, antimony content of 184 ppm) to above 52°C for liquefaction and then pump it into the reactor. Add 1.4 kg of polyphosphoric acid with a phosphoric acid concentration of 105%, and stir for 15 minutes at a stirring speed of 2.0 m / s for acidification.
[0063] The reaction system was heated to 57°C, 700 g of sodium lignin sulfonate was added, and stirring was continued for 15 minutes to fully disperse the yellow phosphorus. 50 g of hydroiodic acid was added, the reaction system was heated to 62°C, and stirring was continued for 3.0 hours.
[0064] After the reaction is completed, the yellow phosphorus is allowed to stand for 10 minutes, and then the yellow phosphorus is transported to a water washing tank, washed with deionized water at 55°C until the washing water is neutral, and then allowed to stand for another 10 minutes. After the yellow phosphorus phase and the water phase are fully separated, the yellow phosphorus is transported to the packaging system, and a low-arsenic, low-antimony, high-purity yellow phosphorus product is obtained after packaging. 198.2 kg of yellow phosphorus is obtained, and the arsenic content in the yellow phosphorus is 1.0 ppm and the antimony content is 0.6 ppm.
[0065] Example 10
[0066] Under normal pressure, 1000 kg of a hydrogen peroxide solution with a mass concentration of 8% was prepared as a basic oxidant, heated to 55°C and added to the reactor for insulation. 200 kg of yellow phosphorus (arsenic content of 258 ppm, antimony content of 184 ppm) was heated to 53°C for liquefaction and then poured into the reactor. 10.0 kg of polyphosphoric acid with a phosphoric acid concentration of 105% was added, and the mixture was stirred at a stirring speed of 2.0 m / s for 15 minutes for acidification.
[0067] The reaction system was heated to 60°C, 1000 g of polyethylene glycol was added, and stirring was continued for 15 minutes to fully disperse the yellow phosphorus. 50 g of hydroiodic acid was added, the reaction system was heated to 63°C, and stirring was continued for 3.0 hours.
[0068] After the reaction is completed, the yellow phosphorus is allowed to stand for 10 minutes, and then the yellow phosphorus is transported to a water washing tank, washed with deionized water at 55°C until the washing water is neutral, and then allowed to stand for another 10 minutes. After the yellow phosphorus phase and the water phase are fully separated, the yellow phosphorus is transported to the packaging system, and a low-arsenic, low-antimony, high-purity yellow phosphorus product is obtained after packaging. 198.7 kg of yellow phosphorus is obtained, and the arsenic content in the yellow phosphorus is 0.9 ppm and the antimony content is 0.4 ppm.
[0069] Comparative Example 1
[0070] This comparative example provides a method for preparing low-arsenic and low-antimony yellow phosphorus, and the specific steps are basically the same as those in Example 1, except that no acidulant is added in this comparative example.
[0071] Comparative Example 2
[0072] This comparative example provides a method for preparing low-arsenic and low-antimony yellow phosphorus, and the specific steps are basically the same as those in Example 1, except that no dispersant is added in this comparative example.
[0073] Comparative Example 3
[0074] This comparative example provides a method for preparing low-arsenic and low-antimony yellow phosphorus, and the specific steps are basically the same as those in Example 1, except that an equal amount of nitric acid is added as an acidifying agent in this comparative example.
[0075] Test example
[0076] The yellow phosphorus prepared by the preparation methods of Examples 1 to 10 and Comparative Examples 1 to 3 was tested. The test results are shown in Table 1.
[0077] Table 1. Product comparison table
[0078]
[0079]
[0080] As can be seen from Table 1, the yellow phosphorus prepared in the embodiment of the present invention has a purity of 99.96% to 99.99%, an arsenic content of ≤1.0ppm, and an antimony content of less than 1.0ppm, or even undetectable. In Comparative Example 1, since no acidulant was used, it can be seen that the arsenic content and antimony content are greater than 20ppm; in Comparative Example 2, since no dispersant was used, it can be seen that the removal effect of arsenic content and antimony content is poor. At the same time, since no acidulant or dispersant was added in Comparative Examples 1 and 2, the yellow phosphorus was not dispersed and oxidized sufficiently, the removal effect of the most impurities was poor, and the arsenic and antimony contents were high; on the other hand, due to insufficient oxidation, the oxidation of yellow phosphorus was also reduced, resulting in the final yellow phosphorus yield being sometimes slightly higher. In Comparative Example 3, nitric acid was used as an acidulant. Compared with phosphoric acid, the arsenic content was only reduced to 12.4ppm and the antimony content was reduced to 9.2ppm. It can be seen that the acidulant, dispersant, and catalyst system used in the patent of the present invention have a significant effect on the removal of arsenic and antimony from yellow phosphorus.
[0081] The methods and products of the present invention have been described through preferred embodiments, and relevant technicians can obviously modify or appropriately change and combine the methods and products described herein without departing from the content, spirit and scope of the present invention to implement the technology of the present invention. It should be particularly pointed out that all similar substitutions and modifications are obvious to those skilled in the art, and they are all considered to be included in the spirit, scope and content of the present invention.
Claims
1. A method for simultaneously removing arsenic and antimony from yellow phosphorus, characterized in that: The heated liquefied yellow phosphorus and the aqueous phase basic oxidant are fully stirred and mixed in a reaction kettle under the condition of hot water liquid sealing, and a dispersant, an acidulant and a catalyst are added, and stirred at 55-65° C. to allow arsenic and antimony impurities in the yellow phosphorus to enter the aqueous phase after reaction, and then washed and allowed to stand for phase separation to obtain high-purity yellow phosphorus with low arsenic and low antimony content; The specific steps of the method are as follows: (a) Material preheating, mixing and acidification: preheat the raw material yellow phosphorus to 50-70°C to fully liquefy, preheat the basic oxidant to 50-60°C and add it to the reactor to keep warm, then add the liquid yellow phosphorus to the reactor, add the acidifier, and stir and mix for 10-15 minutes for acidification; (b) Dispersion: After heating the reaction system materials to 55-70°C, add a dispersant and stir for 5-10 minutes to fully disperse the yellow phosphorus; (c) Catalytic oxidation: adding a catalyst for catalytic oxidation, heating the reaction system materials to 55-65° C., and stirring and mixing for 1-3 hours; (d) Washing: After the reaction is completed, the reaction system is allowed to stand for 10 to 30 minutes. After the yellow phosphorus phase and the water phase are fully separated, the yellow phosphorus is transferred to a water washing tank and washed with hot pure water at 55 to 70° C. until the washing water becomes neutral. (e) Separation and packaging: After washing, the washing system materials are allowed to stand for 10 to 30 minutes. After the yellow phosphorus phase and the water phase are fully separated, the yellow phosphorus is transported to the packaging system. After packaging, a high-purity yellow phosphorus product with low arsenic and antimony content is obtained. The basic oxidant is hydrogen peroxide with a concentration of 5-15%, and the amount added is 3-7 times the mass of yellow phosphorus; the acidulant is at least one of phosphoric acid or polyphosphoric acid, and the amount added of the acidulant is 0.1-1% of the mass of the basic oxidant, the phosphoric acid concentration is 82%-85%, and the mass concentration of phosphoric acid in polyphosphoric acid is 105%-116%; the catalyst is one or more of hydroiodic acid, sodium iodide, sodium bromide, and elemental bromine, and the amount added of the catalyst is 0.01-0.1% of the mass of yellow phosphorus; the dispersant is at least one of hexadecyltrimethylammonium bromide, sodium lignin sulfonate, and polyethylene glycol, and the amount added of the dispersant is 0.05-0.1% of the mass of the basic oxidant.
2. The method for simultaneously removing arsenic and antimony from yellow phosphorus according to claim 1, characterized in that: The hot pure water is heated desalted water or deionized water.
3. The method for simultaneously removing arsenic and antimony from yellow phosphorus according to claim 1, characterized in that: The stirring linear speed is 0.2-2 m / s.
Citation Information
Cited By
Recycling method of iodine catalyst in low-arsenic low-antimony yellow phosphorus production
CN117699754A
A method for recycling iodine catalyst in the production of low-arsenic and low-antimony yellow phosphorus