Resistance-reducing and corrosion-inhibiting composition and preparation method thereof
By using porous materials in the resistance reducing agent, a coordinated combination of conductive agent and corrosion inhibitor is formed to form an efficient and stable resistance reduction and corrosion inhibitor, the problem of insufficient conductivity and corrosion resistance of traditional resistance reducing agents is solved, and the complexity is achieved High-efficiency resistance reduction and corrosion protection in the environment.
Patent Information
- Application Number
- CN202310276585.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-21
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-03-21
AI Technical Summary
Traditional resistance reducing agents have low conductivity, poor long-term performance, weak stability and poor corrosion resistance. They cannot effectively reduce grounding resistance and protect metal grounding bodies, especially in complex environments and highly corrosive geological conditions, which are difficult to ensure the power system. Safe and stable.
Porous materials (such as expanded perlite and zeolite) are used as loading materials, and cooperate with soluble salt-containing conductive agents, carbon-containing conductive agents, inorganic corrosion inhibitors and organic corrosion inhibitors to form good conductivity and long-term effectiveness , a resistance-resistance-resistance corrosion-resistance composition with high stability and excellent anti-corrosion effect, long-term storage of conductive agents through adsorption and slow release, reduce loss and loss, and store moisture in porous materials to maintain soil moisture content and permeability, forming a protective film Prevent corrosion.
It achieves a resistance reduction effect of good conductivity, improves the long-term effectiveness and stability of the composition, significantly reduces the grounding resistance, and provides effective anti-corrosion protection under different environmental conditions, avoiding conductive agent loss and metal corrosion.
Smart Images

Figure BDA0004136448050000141 
Figure BDA0004136448050000151
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of grounding resistance reduction materials, and in particular to a resistance reduction and corrosion inhibition composition and a preparation method thereof. Background Art
[0002] The power transmission and transformation system undertakes the important tasks of power transformation and transmission in the power system. It is the only channel connecting power plants and power users, and is one of the most important infrastructures in all countries. Setting up a grounding grid at a specific node in the power transmission and transformation system can effectively ensure the leakage safety and lightning protection effect of electrical equipment, thereby ensuring the safe and stable operation of the power system. The grounding grid is a general term for a mesh structure composed of multiple grounding bodies buried in the soil and grounding wires connecting power equipment to the grounding bodies. Among them, the grounding body can be made of metal materials such as copper, carbon steel, stainless steel, etc., or it can be a composite of non-metallic materials such as conductive polymers, conductive graphite, conductive coatings and metal materials.
[0003] Grounding resistance is the main evaluation index of grounding materials or grounding devices. Grounding resistance can be reduced by increasing the total area of the grounding grid or reducing the resistivity of the soil. Among them, increasing the total area of the grounding grid has problems such as high overall cost and difficulty in construction under complex environments. In order to solve the difficult problems of grounding projects under complex environmental conditions, especially grounding projects in high-resistance areas such as mountainous areas, islands, yellow sand, highly corrosive geological conditions, and narrow areas with limited area in urban areas, resistance reducing agents can usually be used to reduce the resistivity of the soil. However, traditional resistance reducing agents have problems such as low conductivity, poor long-term effectiveness, weak stability, and poor anti-corrosion effect, and cannot escort the safety of the power transmission and transformation system. Summary of the invention
[0004] Based on this, it is necessary to provide a resistance reducing and corrosion inhibiting composition and a preparation method thereof to solve the problems of low conductivity, poor long-term effectiveness, weak stability and poor anti-corrosion effect of traditional resistance reducing agents.
[0005] The above object of the present invention is achieved through the following technical solutions:
[0006] In a first aspect, the present invention provides a resistance-reducing and corrosion-inhibiting composition, comprising the following components in parts by weight:
[0007] 100 parts of porous material, 60 parts to 3000 parts of soluble salt conductive agent, 200 parts to 3000 parts of carbon-containing conductive agent, 5 parts to 50 parts of inorganic corrosion inhibitor and 5 parts to 50 parts of organic corrosion inhibitor;
[0008] Wherein, the porous material includes one or more of expanded perlite, zeolite and attapulgite.
[0009] In one embodiment, the porous material is expanded perlite.
[0010] In one embodiment, the expanded perlite satisfies one or more of the following conditions:
[0011] 1) The expansion ratio of the expanded perlite is 5 to 30 times;
[0012] 2) The particle size of the expanded perlite is 30 μm to 5 mm.
[0013] In one embodiment, the soluble salt conductive agent includes one or more of hydrochloride, nitrate, carbonate, bicarbonate and sulfate.
[0014] In one embodiment, the soluble salt conductive agent includes carbonate, bicarbonate and sulfate.
[0015] In one embodiment, the carbon-containing conductive agent includes carbon powder and / or graphite powder.
[0016] In one embodiment, the particle size of the carbon-containing conductive agent is 6.5 μm to 45 μm.
[0017] In one embodiment, the inorganic corrosion inhibitor includes one or more of nitrite, chromate, dichromate, molybdate, tungstate, phosphate, and silicate.
[0018] In one embodiment, the inorganic corrosion inhibitor is nitrite.
[0019] In one embodiment, the organic corrosion inhibitor includes one or more of amine corrosion inhibitors, phosphine corrosion inhibitors, triazole corrosion inhibitors, aldehyde corrosion inhibitors, carboxylate corrosion inhibitors and quaternary ammonium salt corrosion inhibitors.
[0020] In one embodiment, the organic corrosion inhibitor is one or more of benzotriazole, toluenetriazole, mercaptobenzotriazole, benzoate, gluconate and triethanolamine.
[0021] In a second aspect of the present invention, a resistance reducing and corrosion inhibiting composition is provided, which comprises the following steps:
[0022] Prepare the components according to the above-mentioned resistance-reducing and corrosion-inhibiting composition;
[0023] Under heating conditions, dissolving the soluble salt conductive agent, the inorganic corrosion inhibitor and the organic corrosion inhibitor in water to obtain a mixed solution;
[0024] adding the carbon-containing conductive agent into the mixed liquid to obtain a slurry;
[0025] The porous material is added into the slurry, and the mixture is dried to a moisture content of ≤5wt.%, to obtain the resistance-reducing and corrosion-inhibiting composition.
[0026] The present invention has the following beneficial effects:
[0027] The present invention utilizes a porous material with strong adsorption, good water absorption and good water retention as a loading material, and cooperates with effective components such as a soluble salt conductive agent, a carbon-containing conductive agent, an inorganic corrosion inhibitor and an organic corrosion inhibitor to obtain a resistance-reducing and corrosion-inhibiting composition with good conductivity, good long-term effectiveness, high stability and excellent anti-corrosion effect.
[0028] Compared with gelling substances such as silicates, aluminates, sulfoaluminates or bentonites in traditional resistance reducers, porous materials such as expanded perlite, zeolite and attapulgite have good adsorption properties, which can keep the conductive agent and corrosion inhibitor in the internal pores for a long time, and allow the effective components to play the conductive and anti-corrosion functions through sustained release, effectively reducing their loss under the action of groundwater or rainwater; at the same time, porous materials also have excellent water absorption and water retention. They can store water in the rainy season and release water in the dry season, which can not only keep the surrounding soil with high moisture content and high permeability, but also prevent the soluble salt conductive agent from failing due to lack of water, so that the soluble salt conductive agent can stably and permanently play its resistance reduction role.
[0029] At the same time, soluble salt conductive agents can be ionized in the moisture stored in the porous material, and reduce the resistivity of the surrounding soil through slow diffusion and penetration, and the resistance reduction area is relatively wide; carbon-containing conductive agents can increase the effective volume of the grounding body or reduce the contact resistance between the grounding body and the composition, further improving the stability and long-term effectiveness of the resistance reduction effect of the composition; inorganic corrosion inhibitors can form an oxide or precipitate protective film on the surface of the grounding body, and organic corrosion inhibitors can be adsorbed on the surface of the grounding body to form a dense adsorption film or complex protective film, which has a stable and reliable protective effect on metal grounding bodies of different materials, and effectively inhibits the corrosion of metal grounding bodies in different media. DETAILED DESCRIPTION
[0030] In order to make the above-mentioned purpose, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below.
[0031] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0032] Resistance reducers are usually good conductors composed of multiple components, and can be divided into chemical resistance reducers and physical resistance reducers. Among them, chemical resistance reducers use soluble salt electrolytes as conductive materials and are mixed with gelling substances that have a strong affinity for metals to form a low-resistance structure. Its resistance reduction mechanism is to reduce the resistivity of the soil through the penetration of free water and electrolyte. According to the resistance reduction mechanism of chemical resistance reducers, electrolytes can only ionize and play a resistance reduction role under wet conditions. The higher the electrolyte concentration, the better the resistance reduction effect, and the more serious its corrosion to metals; with the rise and fall of groundwater levels and the erosion of rainwater, electrolytes are easily lost, resulting in the gradual loss of resistance reduction effect; and in dry or cold environments, electrolytes precipitate crystals, the resistivity will increase and the resistance reduction effect will be lost. Physical resistance reducing agents usually use non-electrolyte solid powders such as charcoal, graphite, metal or metal oxide as conductive materials, and strong acid and weak alkali salts as gelling materials. Their conductive properties are not affected by soil moisture content and ambient temperature, and their anti-corrosion effect is better than that of chemical resistance reducing agents. However, since their conductive materials cannot penetrate into the surrounding soil, they cannot improve the conductive properties of the soil around the resistance reducing agent, and the resistance reducing effect area is very limited; if the cross-sectional area of the physical resistance reducing agent is not large enough, the grounding resistance will be significantly affected by the moisture content of the surrounding soil, resulting in insufficient stability and long-term resistance reducing effect; if the water absorption expansion coefficient of the physical resistance reducing agent is different from that of the grounding body, it cannot be tightly combined with the grounding body when the temperature and humidity change, resulting in the grounding body being exposed to the air and rusting, and the resistivity rises significantly. At the same time, both chemical resistance reducing agents and physical resistance reducing agents prevent water and oxygen erosion in the air by having a higher density than the soil, thereby alleviating the corrosion of metal grounding bodies such as copper, carbon steel or stainless steel. They do not have a protective effect on metal grounding bodies, resulting in serious corrosion problems for metal grounding bodies. It can be seen that traditional resistance reducing agents have the problems of low conductivity, poor long-term effectiveness, weak stability and poor anti-corrosion performance. Based on this, the first aspect of the present invention provides a resistance reducing and corrosion inhibiting composition, comprising the following components in parts by weight:
[0033] 100 parts of porous material, 60 parts to 3000 parts of soluble salt conductive agent, 200 parts to 3000 parts of carbon-containing conductive agent, 5 parts to 50 parts of inorganic corrosion inhibitor and 5 parts to 50 parts of organic corrosion inhibitor;
[0034] Wherein, the porous material includes one or more of expanded perlite, zeolite and attapulgite.
[0035] The present invention utilizes a porous material with strong adsorption, good water absorption and good water retention as a loading material, and cooperates with effective components such as a soluble salt conductive agent, a carbon-containing conductive agent, an inorganic corrosion inhibitor and an organic corrosion inhibitor to obtain a resistance-reducing and corrosion-inhibiting composition with good conductivity, good long-term effectiveness, high stability and excellent anti-corrosion effect.
[0036] Compared with gelling substances such as silicates, aluminates, sulfoaluminates or bentonites in traditional resistance reducers, porous materials such as expanded perlite, zeolite and attapulgite have good adsorption properties, which can keep the conductive agent and corrosion inhibitor in the internal pores for a long time, and allow the effective components to play the conductive and anti-corrosion functions through sustained release, effectively reducing their loss under the action of groundwater or rainwater; at the same time, porous materials also have excellent water absorption and water retention. They can store water in the rainy season and release water in the dry season, which can not only keep the surrounding soil with high moisture content and high permeability, but also prevent the soluble salt conductive agent from failing due to lack of water, so that the soluble salt conductive agent can stably and permanently play its resistance reduction role.
[0037] At the same time, soluble salt conductive agents can be ionized in the moisture stored in the porous material, and reduce the resistivity of the surrounding soil through slow diffusion and penetration, and the resistance reduction area is relatively wide; carbon-containing conductive agents can increase the effective volume of the grounding body or reduce the contact resistance between the grounding body and the composition, further improving the stability and long-term effectiveness of the resistance reduction effect of the composition; inorganic corrosion inhibitors can form an oxide or precipitate protective film on the surface of the grounding body, and organic corrosion inhibitors can be adsorbed on the surface of the grounding body to form a dense adsorption film or complex protective film, which has a stable and reliable protective effect on metal grounding bodies of different materials, and effectively inhibits the corrosion of metal grounding bodies in different media.
[0038] In some preferred embodiments, the resistance reducing and corrosion inhibiting composition comprises the following components in parts by weight:
[0039] 100 parts of porous material, 110 parts to 1500 parts of soluble salt conductive agent, 500 parts to 2000 parts of carbon-containing conductive agent, 10 parts to 40 parts of inorganic corrosion inhibitor and 10 parts to 40 parts of organic corrosion inhibitor.
[0040] In some embodiments, the porous material is expanded perlite.
[0041] Expanded perlite is a non-metallic mineral product obtained by the volume expansion of perlite sand under high temperature conditions. It has countless irregular closed pores and a well-developed honeycomb structure. It performs very well in terms of adsorption, water absorption, moisture retention, storage, thermal insulation and sterility. Applying it to geological conditions with poor water retention can prevent water loss, increase soil moisture retention rate, and enable soluble salt conductive agents to fully exert their resistance reduction effect. At the same time, it can also greatly reduce the loss of effective components through adsorption and storage, thereby improving the long-term effect and stability of the composition.
[0042] In some embodiments, the expanded perlite satisfies one or more of the following conditions:
[0043] 1) The expansion ratio of the expanded perlite is 5 to 30 times;
[0044] 2) The particle size of the expanded perlite is 30 μm to 5 mm.
[0045] It can be understood that the particle size is the equivalent circle diameter.
[0046] The expansion ratio and particle size of expanded perlite will affect its adsorption performance. If the expansion ratio is too low, the porosity will be low and the adsorption effect will be insufficient. If the expansion ratio is too high, the pores will be too large and the adsorption effect will not be ideal. If the particle size is too small, it will be difficult to form a lasting adsorption. If the particle size is too large, the adsorption effect will be reduced. Therefore, when the expansion ratio of expanded perlite is 5 to 30 times and the particle size is 30μm to 5mm, it can form a lasting and stable adsorption effect on other effective components, greatly reducing the loss of effective components.
[0047] In some embodiments, the soluble salt conductive agent includes one or more of hydrochloride, nitrate, carbonate, bicarbonate and sulfate.
[0048] Among them, hydrochloride, nitrate, and sulfate are strong acid salts, and carbonate and bicarbonate are weak acid salts. Reasonable matching of the above soluble salt conductive agents can not only make the composition have good conductivity, but also increase the pH of the composition, reduce the hydrogen ion concentration, and inhibit hydrogen evolution corrosion of metal grounding bodies. In addition, nitrates, carbonates, and bicarbonates all have a certain corrosion inhibition effect and can form a passivation film or precipitation film on the surface of metal materials, thereby inhibiting the corrosion of metals in the medium.
[0049] In some embodiments, the soluble salt conductive agent includes carbonates, bicarbonates and sulfates.
[0050] The soluble salt conductive agent contains two weak acid salts and one strong acid salt. While exerting a good resistance reduction effect, it can greatly improve the alkalinity of the composition and avoid the occurrence of hydrogen evolution corrosion. In addition, carbonates and bicarbonates can react with calcium ions, magnesium ions, etc. in the soil to form a precipitate protective film, further slowing down the corrosion of the metal grounding body.
[0051] In some preferred embodiments, the soluble salt conductive agent includes 20 to 1000 parts of the carbonate, 20 to 1000 parts of the bicarbonate and 20 to 1000 parts of the sulfate.
[0052] In some preferred embodiments, the soluble salt conductive agent includes 30 to 500 parts of the carbonate, 30 to 500 parts of the bicarbonate and 50 to 500 parts of the sulfate.
[0053] In some specific embodiments, the soluble salt conductive agent includes sodium carbonate, sodium bicarbonate and sodium sulfate.
[0054] In some embodiments, the carbon-containing conductive agent includes carbon powder and / or graphite powder.
[0055] Carbon powder and graphite powder are both non-electrolyte solid materials with high conductivity. Compared with metal powder and metal oxide powder, they have the advantages of not easy to corrode and stable conductivity; compared with carbon materials such as graphene, carbon nanotubes and carbon fibers, they have the advantages of low raw material cost and good economy.
[0056] In some preferred embodiments, the carbon-containing conductive agent is graphite powder.
[0057] In some embodiments, the particle size of the carbon-containing conductive agent is 6.5 μm to 45 μm.
[0058] It can be understood that the particle size is the equivalent circle diameter.
[0059] If the particle size of the carbon-containing conductive agent is too large, it will affect the adsorption performance of the porous material; if the particle size of the carbon-containing conductive agent is too small, its thickening effect is too strong, so that the different components in the composition cannot be mixed evenly, and the porous material cannot completely adsorb other components. Selecting a carbon-containing conductive agent with an appropriate particle size can improve the compatibility with other components, so that the composition can obtain the best adsorption and water absorption.
[0060] In some embodiments, the inorganic corrosion inhibitor includes one or more of nitrite, chromate, dichromate, molybdate, tungstate, phosphate, and silicate.
[0061] Among them, nitrites, chromates, dichromates, molybdates, tungstates, etc. can form a high-density, strong-adhesion oxide passivation layer on the surface of metal materials, thereby inhibiting the corrosion of metal materials; phosphates and silicates can react with calcium ions, iron ions, etc. to form a sediment protective film, the thickness of which will continue to increase with time and tightly adhere to the surface of the grounding body, and can also effectively prevent erosion by water and oxygen in the air.
[0062] In some embodiments, the inorganic corrosion inhibitor is nitrite.
[0063] Nitrite has strong oxidizing properties and can form an oxide passivation layer on the surface of the grounding body. Its density and adhesion are better than the sediment protective film, and its anti-corrosion effect is stronger. It does not contain any toxic substances such as heavy metals and will not cause pollution to the soil or groundwater.
[0064] In some embodiments, the organic corrosion inhibitor includes one or more of an amine corrosion inhibitor, a phosphine corrosion inhibitor, a triazole corrosion inhibitor, an aldehyde corrosion inhibitor, a carboxylate corrosion inhibitor, and a quaternary ammonium salt corrosion inhibitor.
[0065] The above-mentioned organic corrosion inhibitors contain non-metallic elements with unshared electron pairs, such as oxygen, nitrogen, sulfur, and phosphorus. They can cover the surface of the metal grounding electrode with a firm adsorption film through physical adsorption such as electrostatic attraction and van der Waals force, or chemical adsorption combined with metal coordination. They can also further react with metal ions to form an insoluble precipitate protective film, thereby having a good anti-corrosion effect on different metal materials.
[0066] In some embodiments, the organic corrosion inhibitor is one or more of benzotriazole, toluenetriazole, mercaptobenzotriazole, benzoate, gluconate and triethanolamine.
[0067] Among them, triethanolamine is an amine corrosion inhibitor, which can cover the surface of iron through electrostatic adsorption to inhibit hydrogen evolution corrosion, and has a good corrosion inhibition effect on iron in acidic media; benzoates and gluconates can coordinate with metals to form a strong chemical adsorption film; benzotriazole, methylbenzotriazole, and mercaptobenzotriazole can form a complex precipitation film, which has a good slow-release protection effect on metals such as copper, silver, zinc, cadmium, aluminum, and tin.
[0068] In some preferred embodiments, the organic corrosion inhibitor is benzotriazole.
[0069] Benzotriazole is an organic heterocyclic compound with lower toxicity than inorganic corrosion inhibitors such as nitrates and chromates. It has a large solubility in acid and alkali solutions and can react with metallic copper at the solid-liquid interface to form a stable and insoluble chain polymer complex. It has a unique and excellent corrosion inhibition and protection effect on copper and copper alloys, and can effectively inhibit the discoloration corrosion of copper-based grounding bodies.
[0070] In a second aspect of the present invention, a method for preparing a resistance-reducing and corrosion-inhibiting composition is provided, which comprises the following steps:
[0071] Prepare the components according to the above-mentioned resistance-reducing and corrosion-inhibiting composition;
[0072] Under heating conditions, dissolving the soluble salt conductive agent, the inorganic corrosion inhibitor and the organic corrosion inhibitor in water to obtain a mixed solution;
[0073] adding the carbon-containing conductive agent into the mixed liquid to obtain a slurry;
[0074] The porous material is added into the slurry, and the mixture is dried to a moisture content of ≤5wt.%, to obtain the resistance-reducing and corrosion-inhibiting composition.
[0075] By heating, soluble salt conductive agents, inorganic corrosion inhibitors and organic corrosion inhibitors can be quickly dissolved in water and added to form a uniform and stable mixed liquid; the carbon-containing conductive agent is insoluble in water and can thicken the mixed liquid to obtain a slurry with moderate viscosity; finally, the slurry is fully adsorbed by porous materials and dried to remove excess water to obtain a stable and long-lasting resistance-reducing and corrosion-inhibiting composition.
[0076] In some preferred embodiments, the heating condition has a temperature of 80°C to 90°C.
[0077] Heating at 80°C to 90°C can speed up the dissolution rate, prevent the water from volatilizing too quickly and reducing the water content of the product, and will not affect the anti-corrosion protection effect of the organic corrosion inhibitor.
[0078] In some preferred embodiments, the drying temperature is 105°C to 150°C.
[0079] The present invention is further described in detail below in conjunction with specific examples. The raw materials used in the following examples are all commercially available products unless otherwise specified; among them, the expansion ratio of expanded perlite is 25 times, and the particle size is 20 μm; the purity of sodium carbonate, sodium bicarbonate, sodium sulfate, and sodium nitrite are all ≥99%, and the purity of benzotriazole is ≥99.5%; the purity of graphite powder is ≥99%, and the fineness is 800 mesh (i.e., the particle size is 18 μm).
[0080] Example 1
[0081] Please refer to Table 1. According to the mass percentage, 100 parts of expanded perlite, 20 parts of sodium carbonate, 20 parts of sodium bicarbonate, 20 parts of sodium sulfate, 200 parts of graphite powder, 5 parts of sodium nitrite, 50 parts of benzotriazole and 60 parts of water were weighed. Water was added to the stirring kettle, heated to 80°C, and sodium carbonate, sodium bicarbonate, sodium sulfate, sodium nitrite and benzotriazole were added in sequence under stirring, and stirred for 30 minutes to completely dissolve the above components to obtain a mixed solution; graphite powder was added to the mixed solution, stirred for 15 minutes to mix evenly, and slurry was obtained; expanded perlite was added to the slurry, stirred for 15 minutes to allow the expanded perlite to completely absorb the effective components in the slurry, and ventilated and dried at 105°C until the moisture content dropped to below 5% (i.e., the composition contained a maximum of 22 parts of water), and a resistance-reducing and corrosion-inhibiting composition was obtained.
[0082] Example 2
[0083] Please refer to Table 1. According to the mass percentage, 100 parts of expanded perlite, 1000 parts of sodium carbonate, 20 parts of sodium bicarbonate, 1000 parts of sodium sulfate, 2000 parts of graphite powder, 50 parts of sodium nitrite, 5 parts of benzotriazole and 500 parts of water were weighed. Water was added to the stirring kettle, heated to 90°C, and sodium carbonate, sodium bicarbonate, sodium sulfate, sodium nitrite and benzotriazole were added in sequence under stirring, and stirred for 50 minutes to completely dissolve the above components to obtain a mixed solution; graphite powder was added to the mixed solution, stirred for 20 minutes to mix evenly, and slurry was obtained; expanded perlite was added to the slurry, stirred for 20 minutes to allow the expanded perlite to completely absorb the effective components in the slurry, and ventilated and dried at 150°C until the moisture content dropped to below 5% (i.e., the composition contained a maximum of 220 parts of water), and a resistance-reducing and corrosion-inhibiting composition was obtained.
[0084] Example 3
[0085] Please refer to Table 1. According to the mass percentage, 100 parts of expanded perlite, 20 parts of sodium carbonate, 1000 parts of sodium bicarbonate, 50 parts of sodium sulfate, 500 parts of graphite powder, 10 parts of sodium nitrite, 40 parts of benzotriazole and 200 parts of water were weighed. Water was added to a stirred kettle and heated to 85°C. Sodium carbonate, sodium bicarbonate, sodium sulfate, sodium nitrite and benzotriazole were added in sequence under stirring, and stirred for 40 minutes to completely dissolve the above components to obtain a mixed solution; graphite powder was added to the mixed solution and stirred for 18 minutes to mix evenly to obtain a slurry; expanded perlite was added to the slurry and stirred for 18 minutes to allow the expanded perlite to completely absorb the effective components in the slurry, and then ventilated and dried at 130°C until the moisture content dropped to below 5% (i.e., the composition contained at most 91 parts of water) to obtain a resistance-reducing and corrosion-inhibiting composition.
[0086] Example 4
[0087] Please refer to Table 1. According to the mass percentage, 100 parts of expanded perlite, 500 parts of sodium carbonate, 500 parts of sodium bicarbonate, 500 parts of sodium sulfate, 3000 parts of graphite powder, 40 parts of sodium nitrite, 10 parts of benzotriazole and 800 parts of water were weighed. Water was added to the stirring kettle, heated to 90°C, and sodium carbonate, sodium bicarbonate, sodium sulfate, sodium nitrite and benzotriazole were added in sequence under stirring, and stirred for 50 minutes to completely dissolve the above components to obtain a mixed solution; graphite powder was added to the mixed solution, stirred for 20 minutes to mix evenly, and slurry was obtained; expanded perlite was added to the slurry, stirred for 20 minutes to allow the expanded perlite to completely absorb the effective components in the slurry, and ventilated and dried at 150°C until the moisture content dropped to below 5% (i.e., the composition contained a maximum of 245 parts of water), and a resistance-reducing and corrosion-inhibiting composition was obtained.
[0088] Example 5
[0089] Please refer to Table 1. According to the mass percentage, 100 parts of expanded perlite, 300 parts of sodium carbonate, 300 parts of sodium bicarbonate, 300 parts of sodium sulfate, 1200 parts of graphite powder, 20 parts of sodium nitrite, 30 parts of benzotriazole and 600 parts of water were weighed. Water was added to the stirring kettle, heated to 85°C, and sodium carbonate, sodium bicarbonate, sodium sulfate, sodium nitrite and benzotriazole were added in sequence under stirring, and stirred for 40 minutes to completely dissolve the above components to obtain a mixed solution; graphite powder was added to the mixed solution, stirred for 18 minutes to mix evenly, and a slurry was obtained; expanded perlite was added to the slurry, stirred for 18 minutes to allow the expanded perlite to completely absorb the effective components in the slurry, and ventilated and dried at 130°C until the moisture content dropped to below 5% (i.e., the composition contained a maximum of 118 parts of water), and a resistance-reducing and corrosion-inhibiting composition was obtained.
[0090] Example 6
[0091] Please refer to Table 1. According to the mass percentage, 100 parts of expanded perlite, 200 parts of sodium carbonate, 200 parts of sodium bicarbonate, 400 parts of sodium sulfate, 1800 parts of graphite powder, 30 parts of sodium nitrite, 20 parts of benzotriazole and 700 parts of water were weighed. Water was added to the stirring kettle, heated to 85°C, and sodium carbonate, sodium bicarbonate, sodium sulfate, sodium nitrite and benzotriazole were added in sequence under stirring, and stirred for 40 minutes to completely dissolve the above components to obtain a mixed solution; graphite powder was added to the mixed solution, stirred for 18 minutes to mix evenly, and a slurry was obtained; expanded perlite was added to the slurry, stirred for 18 minutes to allow the expanded perlite to completely absorb the effective components in the slurry, and ventilated and dried at 130°C until the moisture content dropped to below 5% (i.e., the composition contained a maximum of 145 parts of water), and a resistance-reducing and corrosion-inhibiting composition was obtained.
[0092] Example 7
[0093] Please refer to Table 1. According to the mass percentage, 100 parts of expanded perlite, 600 parts of sodium carbonate, 100 parts of sodium bicarbonate, 600 parts of sodium sulfate, 1000 parts of graphite powder, 25 parts of sodium nitrite, 25 parts of benzotriazole and 600 parts of water were weighed. Water was added to the stirring kettle, heated to 85°C, and sodium carbonate, sodium bicarbonate, sodium sulfate, sodium nitrite and benzotriazole were added in sequence under stirring, and stirred for 40 minutes to completely dissolve the above components to obtain a mixed solution; graphite powder was added to the mixed solution, stirred for 18 minutes to mix evenly, and slurry was obtained; expanded perlite was added to the slurry, stirred for 18 minutes to allow the expanded perlite to completely absorb the effective components in the slurry, and ventilated and dried at 130°C until the moisture content dropped to below 5% (i.e., the composition contained a maximum of 129 parts of water), and a resistance-reducing and corrosion-inhibiting composition was obtained.
[0094] Example 8
[0095] Please refer to Table 1. According to the mass percentage, 100 parts of expanded perlite, 100 parts of sodium carbonate, 600 parts of sodium bicarbonate, 100 parts of sodium sulfate, 1500 parts of graphite powder, 25 parts of sodium nitrite, 25 parts of benzotriazole and 600 parts of water were weighed. Water was added to the stirring kettle, heated to 85°C, and sodium carbonate, sodium bicarbonate, sodium sulfate, sodium nitrite and benzotriazole were added in sequence under stirring, and stirred for 40 minutes to completely dissolve the above components to obtain a mixed solution; graphite powder was added to the mixed solution, stirred for 18 minutes to mix evenly, and a slurry was obtained; expanded perlite was added to the slurry, stirred for 18 minutes to allow the expanded perlite to completely absorb the effective components in the slurry, and ventilated and dried at 130°C until the moisture content dropped to below 5% (i.e., the composition contained a maximum of 129 parts of water), and a resistance-reducing and corrosion-inhibiting composition was obtained.
[0096] Comparative Example 1
[0097] The resistance-reducing and corrosion-inhibiting composition of this comparative example is the xx-5 type anti-corrosion and resistance-reducing agent produced by Beijing Langming Technology Co., Ltd.
[0098] Comparative Example 2
[0099] The resistance-reducing and corrosion-inhibiting composition of this comparative example is basically the same as that of Example 8, except that: in this comparative example, no porous material is added, and bentonite with a layered structure is used as a gelling material to fix the effective components.
[0100] Please refer to Table 1. According to the mass percentage, 100 parts of bentonite, 100 parts of sodium carbonate, 600 parts of sodium bicarbonate, 100 parts of sodium sulfate, 1500 parts of graphite powder, 25 parts of sodium nitrite, 25 parts of benzotriazole and 600 parts of water were weighed. Water was added to the stirring kettle, heated to 85°C, and sodium carbonate, sodium bicarbonate, sodium sulfate, sodium nitrite and benzotriazole were added in sequence under stirring, and stirred for 40 minutes to completely dissolve the above components to obtain a mixed solution; graphite powder was added to the mixed solution, and stirred for 18 minutes to mix evenly to obtain a slurry; expanded perlite was added to the slurry, and stirred for 18 minutes to allow the expanded perlite to completely absorb the effective components in the slurry, and then ventilated and dried at 130°C until the moisture content dropped to below 5% (i.e., the composition contained a maximum of 129 parts of water), to obtain a resistance-reducing and corrosion-inhibiting composition.
[0101] According to "DL / T 380-2010 Technical Requirements for Grounding Resistance Reduction Materials", the nominal resistivity, resistivity change after the impulse current withstand test, resistivity change after the power frequency current withstand test, resistivity after the stability experiment, and average corrosion rate after the corrosion test of the resistance reduction and corrosion inhibition compositions in Examples 1 to 8 and Comparative Examples 1 to 2 were tested, and the results are shown in Table 1.
[0102] Among them, the nominal resistivity refers to the resistivity of the grounding resistance reduction material at room temperature (25℃±10℃); the stability test is a combination of water loss test, hot and cold cycle test and water immersion test; the average corrosion rate is calculated based on the weight loss of the metal due to corrosion, indicating the corrosion depth per unit time, in millimeters / year (mm / a) or micrometers / year (μm / a). According to the provisions of "DL / T 380-2010 Technical Conditions for Grounding Resistance Reduction Materials", the resistance reduction material should meet the following requirements: nominal resistivity ≤5Ω·m, resistivity change after impulse current withstand test ≤20%, resistivity change after power frequency current withstand test ≤20%, resistivity after stability test ≤6Ω·m, average corrosion rate ≤0.03mm / a or ≤30μm / a.
[0103] Table 1. Component contents and test results of the resistance-reducing and corrosion-inhibiting compositions in Examples 1 to 8 and Comparative Examples 1 to 2
[0104]
[0105]
[0106] As can be seen from Table 1, in Examples 1 to 8, the nominal resistivity of the resistance-reducing and corrosion-inhibiting composition is lower, and the lowest can reach 1Ω·m, indicating that its conductivity is better and the resistance-reducing effect is more prominent; after the impulse current tolerance test and the power frequency current tolerance test, the resistivity change of the resistance-reducing and corrosion-inhibiting composition is only 6% at most, which is far lower than the 20% specified in the regulations, and the resistivity does not change after the stability test, indicating that it has excellent long-term effectiveness and stability; after the corrosion test, the average corrosion rate of the resistance-reducing and corrosion-inhibiting composition is only 0.3μm / a at most, and the corrosion protection effect is very outstanding. Therefore, according to the component contents in Examples 1 to 8, a resistance-reducing and corrosion-inhibiting composition with good conductivity, good long-term effectiveness, high stability and good corrosion inhibition effect can be prepared.
[0107] Although the various properties of the xx-5 type anti-corrosion and resistance-reducing agent in Comparative Example 1 meet the requirements for ground resistance-reducing materials, the various properties are significantly inferior to the resistance-reducing and corrosion-inhibiting compositions in Examples 1 to 8, especially the resistivity change and the average corrosion rate are greatly increased, indicating that its long-term effectiveness and corrosion inhibition effect are far inferior to the resistance-reducing and corrosion-inhibiting compositions in Examples 1 to 8.
[0108] The resistance-reducing and corrosion-inhibiting composition of comparative example 2 replaces the expanded perlite in Example 8 with an equal mass of bentonite, and its nominal resistivity is the same as that of Example 8, and it also has good conductivity and resistance-reducing effect. However, after the impulse current tolerance test and the power frequency current tolerance test, the resistivity change of the resistance-reducing and corrosion-inhibiting composition of comparative example 2 is at least doubled compared with the resistance-reducing and corrosion-inhibiting composition of Example 8, and the resistivity after the stability test is as high as 28Ω·m, far exceeding the prescribed 6Ω·m, and the long-term effect and stability are very poor. At the same time, the average corrosion rate of the resistance-reducing and corrosion-inhibiting composition of comparative example 2 after the corrosion test is 5μm / a, and the corrosion inhibition effect is far inferior to that of the resistance-reducing and corrosion-inhibiting composition of Example 8. It can be seen that although the layered bentonite has good water absorption and is conducive to improving the conductivity of the composition, it does not have a porous structure that absorbs and seals the effective components, resulting in serious loss of the conductive agent and the corrosion inhibitor, making the resistance-reducing and corrosion-inhibiting composition of comparative example 2 weak in long-term effect, poor in stability, and unsatisfactory in anti-corrosion effect.
[0109] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0110] The above-mentioned embodiments only express several implementation methods of the present invention, and the description is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be based on the attached claims, and the description can be used to interpret the content of the claims.
Claims
1. A resistance-reducing and corrosion-inhibiting composition, It is characterized in that The composition comprises the following components in parts by weight: 100 parts of porous material, 60 parts to 3000 parts of soluble salt conductive agent, 200 parts to 3000 parts of carbon-containing conductive agent, 5 parts to 50 parts of inorganic corrosion inhibitor and 5 parts to 50 parts of organic corrosion inhibitor; Wherein, the porous material is expanded perlite, the expansion ratio of the expanded perlite is 5 to 30 times, and the particle size of the expanded perlite is 30 μm to 5 mm; The soluble salt conductive agent includes 20 to 1000 parts of carbonate, 20 to 1000 parts of bicarbonate and 20 to 1000 parts of sulfate; The inorganic corrosion inhibitor is nitrite; The organic corrosion inhibitor is benzotriazole; The preparation method of the resistance-reducing and corrosion-inhibiting composition comprises the following steps: Under heating conditions, dissolving the soluble salt conductive agent, the inorganic corrosion inhibitor and the organic corrosion inhibitor in water to obtain a mixed solution; adding the carbon-containing conductive agent into the mixed liquid to obtain a slurry; The porous material is added into the slurry, and the mixture is dried to a moisture content of ≤5wt.%, to obtain the resistance-reducing and corrosion-inhibiting composition.
2. The resistance-reducing and corrosion-inhibiting composition according to claim 1, It is characterized in that The soluble salt conductive agent includes 30 to 500 parts of the carbonate, 30 to 500 parts of the bicarbonate and 50 to 500 parts of the sulfate.
3. The resistance-reducing and corrosion-inhibiting composition according to any one of claims 1 to 2, It is characterized in that The soluble salt conductive agent includes sodium carbonate, sodium bicarbonate and sodium sulfate.
4. The resistance-reducing and corrosion-inhibiting composition according to any one of claims 1 to 2, It is characterized in that The carbon-containing conductive agent includes carbon powder and / or graphite powder.
5. The resistance-reducing and corrosion-inhibiting composition according to claim 4, It is characterized in that The particle size of the carbon-containing conductive agent is 6.5 μm to 45 μm.
6. The resistance-reducing and corrosion-inhibiting composition according to any one of claims 1 to 2, It is characterized in that The resistance-reducing and corrosion-inhibiting composition comprises the following components in parts by mass: 100 parts of porous material, 110 to 1500 parts of soluble salt conductive agent, 500 to 2000 parts of carbon-containing conductive agent, 10 to 40 parts of inorganic corrosion inhibitor and 10 to 40 parts of organic corrosion inhibitor.
7. The resistance-reducing and corrosion-inhibiting composition according to claim 6, It is characterized in that The resistance-reducing and corrosion-inhibiting composition comprises the following components in parts by mass: 100 parts of expanded perlite, 300 parts of sodium carbonate, 300 parts of sodium bicarbonate, 300 parts of sodium sulfate, 1200 parts of graphite powder, 20 parts of sodium nitrite and 30 parts of benzotriazole.
8. The resistance-reducing and corrosion-inhibiting composition according to claim 6, It is characterized in that The resistance-reducing and corrosion-inhibiting composition comprises the following components in parts by mass: 100 parts of expanded perlite, 200 parts of sodium carbonate, 200 parts of sodium bicarbonate, 400 parts of sodium sulfate, 1800 parts of graphite powder, 30 parts of sodium nitrite and 20 parts of benzotriazole.
9. The resistance-reducing and corrosion-inhibiting composition according to claim 6, It is characterized in that The resistance-reducing and corrosion-inhibiting composition comprises the following components in parts by mass: 100 parts of expanded perlite, 600 parts of sodium carbonate, 100 parts of sodium bicarbonate, 600 parts of sodium sulfate, 1000 parts of graphite powder, 25 parts of sodium nitrite and 25 parts of benzotriazole.
10. The resistance-reducing and corrosion-inhibiting composition according to claim 6, It is characterized in that The resistance-reducing and corrosion-inhibiting composition comprises the following components in parts by mass: 100 parts of expanded perlite, 100 parts of sodium carbonate, 600 parts of sodium bicarbonate, 100 parts of sodium sulfate, 1500 parts of graphite powder, 25 parts of sodium nitrite and 25 parts of benzotriazole.
11. A method for preparing a resistance-reducing and corrosion-inhibiting composition, It is characterized in that The following steps are involved: Prepare the components according to the resistance reducing and corrosion inhibiting composition according to any one of claims 1 to 10; Under heating conditions, dissolving the soluble salt conductive agent, the inorganic corrosion inhibitor and the organic corrosion inhibitor in water to obtain a mixed solution; adding the carbon-containing conductive agent into the mixed liquid to obtain a slurry; The porous material is added into the slurry, and the mixture is dried to a moisture content of ≤5wt.%, to obtain the resistance-reducing and corrosion-inhibiting composition.