A high-insulation side glaze for zinc oxide resistor based on polytetrafluoroethylene
Through the sanding and sintering process of modified polytetrafluoroethylene powder, a high-insulating side glaze is formed, which solves the problem of insufficient insulation strength and temperature resistance of the zinc oxide resistor sheet side coating, and achieves excellent insulation and high temperature resistance. The lightning protection ability of the resistor sheet is enhanced.
Patent Information
- Application Number
- CN202211735804.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-31
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-12-31
AI Technical Summary
The insulation strength and temperature resistance of the side coating of existing zinc oxide resistors are insufficient, which can easily lead to flashover and thermal collapse, affecting the lightning protection performance of the equipment.
PTFE powder, nano-TiO2 and nano-SiO2 are sanded, dried and sintered in a specific ratio to form modified PTFE powder, which is then roll-coated on the side of the zinc oxide resistor with an acetone solution, and the curing temperature is controlled at 210 -230℃, forming high insulation side glaze.
Significantly improve the insulation performance and high temperature resistance of the zinc oxide resistor, avoid flashover and thermal collapse, enhance the moisture-proof effect, and meet the strict electrical performance test and action load test requirements.
Smart Images

Figure CN116230335B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of resistor sheets for lightning arresters, in particular to a high-insulation side glaze of a zinc oxide resistor sheet based on polytetrafluoroethylene. Background Art
[0002] Zinc oxide resistors have been widely used in power transmission and distribution lines, power stations, subways, light rails and other places due to their excellent nonlinear volt-ampere characteristics and ability to absorb impact energy. Their main function is to prevent equipment from being damaged by lightning and surge overvoltage. The existing side coatings of zinc oxide resistors are mainly epoxy resin powder and polyester materials, and the curing temperature is usually 140℃-180℃. On the one hand, due to insufficient side insulation strength, zinc oxide resistors are prone to side flashover, small hole breakdown and other discharge phenomena when subjected to large current impacts; on the other hand, due to insufficient heat resistance of the side coating, the resistors often melt due to excessively high temperatures during action load tests, causing thermal collapse of the arrester. The performance of the side coating has become a key factor affecting the development of zinc oxide resistors.
[0003] Polytetrafluoroethylene has the characteristics of acid and alkali resistance, high temperature resistance and ultra-high insulation, and can be used as an ideal coating material for resistors. However, since the commercial polytetrafluoroethylene solution is relatively dilute, the thickness of the coating on the side of the resistor is relatively thin, and it cannot achieve a good insulation effect. Therefore, modifying polytetrafluoroethylene through non-polar fillers and further increasing the viscosity of the solution will produce good results in the field of resistors. Summary of the invention
[0004] 1. Technical issues to be resolved
[0005] In view of the deficiencies in the prior art, the present invention provides a high-insulation side glaze for zinc oxide resistors based on polytetrafluoroethylene, which has high temperature resistance and high insulation performance.
[0006] (II) Technical solution
[0007] To achieve the above object, the present invention provides the following technical solution: the zinc oxide resistor side glaze is prepared from the following raw materials in weight ratio: polytetrafluoroethylene powder: 80%-90%; nano-TiO 2 :5%-10%; Nano-SiO 2 : 6%-12%, and its preparation process comprises the following steps:
[0008] 1) Sand grinding: weigh polytetrafluoroethylene powder, TiO 2 and SiO2, sand-milled to a certain particle size in anhydrous ethanol system;
[0009] 2) Drying to make polytetrafluoroethylene powder, TiO 2and SiO2 are uniformly dispersed in an ethanol solution, mixed evenly, dried and crushed to obtain modified polytetrafluoroethylene powder B;
[0010] 3) Sintering and curing: Powder B is mixed with acetone solution in a certain proportion to form a paste, which is then rolled onto the side of the sintered zinc oxide resistor. After curing at 220°C, grinding, and aluminum spraying, a zinc oxide resistor with excellent performance is obtained.
[0011] Preferably, the sand-grinding particle size of the raw material in step 1 has an average particle size of 0.3-0.5 μm.
[0012] Preferably, the coating thickness of the paste obtained in step 3 is 0.1-0.4 mm.
[0013] Preferably, in the curing process in step 3, the temperature curve of the insulating coating curing process mainly includes: a heating rate of 2-5°C / min, a holding temperature of 210-230°C, a holding time of 3-5h, and natural cooling to room temperature.
[0014] Preferably, after the zinc oxide resistor is coated with enamel, it must meet the requirements of repeated charge transfer test: no flashover after 20 times, and 4 / 10μs high current impact energy tolerance test: no flashover after 2 times
[0015] (III) Beneficial effects
[0016] Compared with the prior art, the present invention provides a high-insulation side glaze for zinc oxide resistor based on polytetrafluoroethylene, which has the following beneficial effects:
[0017] 1. The high-insulation side glaze of the polytetrafluoroethylene-based zinc oxide resistor has an excellent insulating property, which can prevent the resistor from flashing during rigorous electrical performance testing and operation.
[0018] 2. The high-insulation side glaze of the polytetrafluoroethylene-based zinc oxide resistor has an excellent high-temperature resistance coating, and the resistor does not experience thermal collapse during the action load test.
[0019] 3. The high-insulation side glaze of the zinc oxide resistor based on polytetrafluoroethylene adopts sand grinding technology. The modified polytetrafluoroethylene prepared has a small particle size, a smaller porosity than conventional glazes, and a better moisture-proof effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is the curing temperature curve of the present invention. DETAILED DESCRIPTION
[0021] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0022] The zinc oxide resistor side glaze is made of the following raw materials in weight ratio: polytetrafluoroethylene powder: 80%-90%; nano-TiO 2 :5%-10%; Nano-SiO 2 : 6%-12%, and its preparation process comprises the following steps:
[0023] 1) Sand grinding: weigh polytetrafluoroethylene powder, TiO 2 and SiO2, sand-milled in anhydrous ethanol system to a certain particle size, with an average particle size of 0.3-0.5 μm;
[0024] 2) Drying to make polytetrafluoroethylene powder, TiO 2 and SiO2 are uniformly dispersed in an ethanol solution, mixed evenly, dried and crushed to obtain modified polytetrafluoroethylene powder B;
[0025] 3) Sintering and curing, mix powder B and acetone solution in a certain proportion to form a paste, roll it on the side of the sintered zinc oxide resistor, the coating thickness of the paste is 0.1-0.4mm, and after curing at 220℃, grinding and aluminum spraying, a zinc oxide resistor with excellent performance is obtained. Curing process: The temperature curve of the insulating coating curing process mainly includes: heating rate 2-5℃ / min, insulation temperature 210-230℃, insulation time 3-5h, and natural cooling to room temperature.
[0026] Embodiment 1:
[0027] It includes the following components, weight percentages and processes:
[0028] Weigh polytetrafluoroethylene powder by weight: 82%, TiO 2 :8% and SiO2:10%, sand grinding was carried out in anhydrous ethanol system to make polytetrafluoroethylene powder, TiO 2 and SiO2 are uniformly dispersed in an ethanol solution. Then, the modified polytetrafluoroethylene powder B is obtained by drying and crushing at 100°C. The powder B is mixed with the acetone solution at a ratio of 1:0.5 to form a paste solution, which is then rolled on the side of the sintered zinc oxide resistor, cured at 210°C for 4 hours, ground, and sprayed with aluminum to obtain the finished zinc oxide resistor.
[0029] Embodiment 2:
[0030] It includes the following components, weight percentages and processes:
[0031] Weigh polytetrafluoroethylene powder by weight: 85.5%, TiO 2 :5% and SiO2:9.5%, sand grinding was carried out in anhydrous ethanol system to make polytetrafluoroethylene powder, TiO 2 and SiO2 are uniformly dispersed in an ethanol solution. Then, the modified polytetrafluoroethylene powder B is obtained by drying and crushing at 100°C. The powder B is mixed with the acetone solution at a ratio of 1:0.45 to form a paste solution, which is then rolled on the side of the sintered zinc oxide resistor, cured at 220°C for 4 hours, ground, and sprayed with aluminum to obtain the finished zinc oxide resistor.
[0032] Embodiment three:
[0033] It includes the following components, weight percentages and processes:
[0034] Weigh polytetrafluoroethylene powder by weight: 88%, TiO 2 :5% and SiO2:7%, sand grinding was carried out in anhydrous ethanol system to make polytetrafluoroethylene powder, TiO 2 and SiO2 are uniformly dispersed in an ethanol solution. Then, the modified polytetrafluoroethylene powder B is obtained by drying and crushing at 100°C. The powder B is mixed with the acetone solution at a ratio of 1:0.45 to form a paste solution, which is then rolled on the side of the sintered zinc oxide resistor, cured at 230°C for 4 hours, ground, and sprayed with aluminum to obtain the finished zinc oxide resistor.
[0035] Curing temperature curve Figure 1 ;
[0036] The polytetrafluoroethylene glaze prepared by the formula and process described in the above embodiments 1, 2, and 3 is coated on the side of the resistor, with a specification of D42×20mm. The test parameters are as follows:
[0037] Electrical testing: Electrical testing implementation standard: Energy industry standard of the People's Republic of China NB / T 42152-2018 "General Technical Requirements for Non-Linear Metal Oxide Resistors".
[0038]
[0039] 8 / 20μs lightning impulse repeated transfer charge test:
[0040]
[0041] 4 / 10μs high current impulse withstand test:
[0042]
[0043] The zinc oxide resistor of this embodiment has been proven to be effective after testing. Compared with conventional insulating glazes, the current carrying capacity is increased by 10%. The resistor has good side surface after impact, and the overall performance is greatly improved, which fully meets the expected requirements.
[0044] The beneficial effects of the present invention are as follows: the high-insulation side glaze of the zinc oxide resistor based on polytetrafluoroethylene has an excellent insulating property, which can prevent the resistor from flashing over when it is subjected to a strict electrical performance test and operation, and has excellent high temperature resistance, so that the resistor does not suffer from thermal collapse when performing an action load test. The modified polytetrafluoroethylene prepared by the sand grinding technology has a small particle size, a smaller porosity than conventional glazes, and a better moisture-proof effect.
[0045] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A high-insulation side glaze for zinc oxide resistor based on polytetrafluoroethylene, characterized in that: The zinc oxide resistor side glaze is prepared from the following raw materials in weight ratio: polytetrafluoroethylene powder: 80%-90%; nano-TiO2: 5%-10%; nano-SiO2: 6%-12%. The preparation process includes the following steps: 1) Sand grinding: weigh polytetrafluoroethylene powder, TiO2 and SiO2 according to the weight percentage of the above components, and sand grind them to a certain particle size in an anhydrous ethanol system; 2) drying to uniformly disperse the polytetrafluoroethylene powder, TiO2 and SiO2 in the ethanol solution, and after uniform mixing, drying and crushing to obtain modified polytetrafluoroethylene powder B; 3) Sintering and curing: Powder B is mixed with acetone solution in a certain proportion to form a paste, which is then rolled onto the side of the sintered zinc oxide resistor. After curing at 220°C, grinding, and aluminum spraying, a zinc oxide resistor with excellent performance is obtained.
2. The high-insulation side glaze of zinc oxide resistor based on polytetrafluoroethylene according to claim 1 is characterized in that: The sand-grinding particle size of the raw material in step 1 is: average particle size 0.3-0.5 μm.
3. The high-insulation side glaze of zinc oxide resistor based on polytetrafluoroethylene according to claim 1 is characterized in that: The coating thickness of the paste obtained in step 3 is 0.1-0.4 mm.
4. The high-insulation side glaze of zinc oxide resistor based on polytetrafluoroethylene according to claim 1 is characterized in that: The curing process in step 3: the temperature curve of the insulating coating curing process mainly includes: a heating rate of 2-5°C / min, a holding temperature of 210-230°C, a holding time of 3-5h, and a natural cooling to room temperature.
5. The high-insulation side glaze of zinc oxide resistor based on polytetrafluoroethylene according to claim 1, characterized in that: After the zinc oxide resistor is coated with enamel, it must meet the requirements of repeated charge transfer test: no flashover after 20 times, and 4 / 10μs high current impact energy tolerance test: no flashover after 2 times.
Citation Information
Patent Citations
Extra-high-voltage heat-resistant insulating material and preparation method thereof
CN105331047A
Voltage nonlinear resistor and its producing method
CN1290943A
Arc resistant insulating material and circuit breaker
JP2010044930A
Insolating nozzle for arc blow circuit breaker
US20040014868A1