A kind of sintered porous brick made of garbage pyrolysis gasification residue and its preparation and application
By mixing clay and coal gangue with pretreated waste pyrolytic gasified residues, extruding and calculating, porous bricks are prepared, which solves the problems of low garbage disposal rate in villages and towns and the unused pyrolytic gasified residues, and achieves efficient The preparation of sintered porous bricks with pyrolysis gasified residue in garbage has high compressive strength and low toxicity for heavy metal leaching.
Patent Information
- Application Number
- CN202310256109.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-16
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-03-16
AI Technical Summary
The garbage disposal rate in rural areas is low, and sustainable garbage disposal is difficult to achieve remote rural areas, and the pyrolytic gasified residue has not been effectively utilized.
Mix clay, coal gangue and pretreated garbage pyrolysis gasification residues, and then calcined after extrusion and molding to prepare porous bricks. The screening treatment is used to improve the uniformity of the particle size, and produce high compressive strength and good weathering resistance. Garbage pyrolysis gasification residue sintered porous bricks.
The efficient utilization of garbage pyrolysis gasification residue is achieved, and the prepared porous bricks have high compressive strength and low heavy metal leaching toxicity, which meets the performance requirements of the construction industry.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of porous brick preparation methods, and in particular to a garbage pyrolysis gasification residue sintered porous brick and the preparation and application thereof. Background Art
[0002] The treatment rate of domestic waste in villages and towns is 89.62%, and the harmless treatment rate is only 57.90%. At the same time, the rural villagers in mountainous and hilly terrains live relatively scattered, and road traffic is difficult. The centralized waste treatment method has high transportation costs and is difficult to operate sustainably. Small decentralized heat treatment equipment such as gasifiers, gasification incinerators, and pyrolysis incinerators have the advantages of intermittent operation, high volume reduction and reduction, and strong rural adaptability. While being widely used in remote rural areas, they produce a large amount of waste pyrolysis and gasification residues, and there is an urgent need to develop multi-path source utilization technology. Summary of the invention
[0003] In order to solve the above problems, the purpose of the present invention is to provide a sintered porous brick of garbage pyrolysis gasification residue and its preparation and application. The present invention first mixes clay, coal gangue and pre-treated garbage pyrolysis gasification residue to obtain a mixture; then extrudes the obtained mixture after post-treatment to obtain a brick blank; finally, the obtained brick blank is post-treated and calcined to obtain a sintered porous brick of garbage pyrolysis gasification residue. The present invention can reasonably utilize garbage pyrolysis gasification residue and coal gangue to turn waste into treasure, and the prepared sintered porous brick of garbage pyrolysis gasification residue has the advantages of high compressive strength, good weathering resistance, and no heavy metal leaching toxicity hazards, which meets the performance requirements of the construction industry for porous bricks.
[0004] In the present invention, after the garbage pyrolysis gasification residue is screened (the sieve hole diameter is 2 mm), the particles with a particle size of less than 1.18 mm in the garbage pyrolysis gasification residue account for more than 90%, and the smaller the particle size, the higher the strength of the finished brick; there is calcium aluminum feldspar in the residue, and during the high-temperature roasting stage, excessive quartz and calcium aluminum feldspar generate calcium feldspar with good crystallization performance, thereby increasing the strength of the porous brick. Therefore, the garbage pyrolysis gasification residue in the sintered porous bricks of the garbage pyrolysis gasification residue of the present invention can be as high as 40%.
[0005] The purpose of the present invention can be achieved by the following technical solutions:
[0006] The first object of the present invention is to provide a method for preparing sintered porous bricks from garbage pyrolysis and gasification residues, comprising the following steps:
[0007] (1) mixing clay, coal gangue and pre-treated garbage pyrolysis gasification residue to obtain a mixture;
[0008] (2) subjecting the mixture obtained in step (1) to post-treatment and extrusion molding to obtain a brick;
[0009] (3) The brick blanks obtained in step (2) are post-treated and then calcined to obtain sintered porous bricks made of garbage pyrolysis gasification residue.
[0010] In one embodiment of the present invention, in step (1), the pre-treated garbage pyrolysis and gasification residue is garbage pyrolysis and gasification residue that has been subjected to screening treatment.
[0011] In one embodiment of the present invention, during the screening process, the sieve hole diameter is 2 mm.
[0012] In one embodiment of the present invention, the mass percentages of clay, coal gangue and pre-treated garbage pyrolysis gasification residue are 45%-80%: 10%-15%: 10%-40%;
[0013] The sum of the mass percentages of clay, coal gangue and pre-treated garbage pyrolysis gasification residue is 100%.
[0014] In one embodiment of the present invention, the mass percentages of clay, coal gangue and pre-treated garbage pyrolysis gasification residue are 50%:10%:40%.
[0015] In one embodiment of the present invention, in step (2), the post-treatment is to further mix the mixture after aging.
[0016] In one embodiment of the present invention, the aging process lasts for 24 hours to 48 hours;
[0017] The matured mixture is mixed by two-stage double-roll stirring.
[0018] In one embodiment of the present invention, in step (2), during the extrusion molding process, water is added to ensure that the moisture content of the brick is 10%-20%.
[0019] In one embodiment of the present invention, in step (3), the post-treatment is a drying treatment, and the drying treatment takes 3 to 4 days.
[0020] In one embodiment of the present invention, in step (3), during the calcination process, the temperature is 950°C-1050°C.
[0021] The second object of the present invention is to provide a sintered porous brick made of garbage pyrolysis gasification residue prepared by the above method.
[0022] The third object of the present invention is to provide an application of the above-mentioned garbage pyrolysis gasification residue sintered porous bricks in the construction industry.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] (1) The present invention can reasonably utilize the garbage pyrolysis gasification residue and coal gangue, turning waste into treasure, and the prepared sintered porous bricks of garbage pyrolysis gasification residue have the advantages of high compressive strength, good weathering resistance, and no heavy metal leaching toxicity hazards, which meets the performance requirements of the construction industry for porous bricks;
[0025] (2) The average compressive strength of the sintered porous bricks prepared by the present invention is greater than 19 MPa, the standard compressive strength is greater than 14 MPa, the average boiling water absorption is not greater than 23%, the saturation coefficient is not greater than 0.88, and the heavy metal leaching toxicity is far lower than the limit value of the "Green Product Evaluation Wall Materials". DETAILED DESCRIPTION
[0026] The present invention provides a method for preparing sintered porous bricks from garbage pyrolysis and gasification residues, comprising the following steps:
[0027] (1) mixing clay, coal gangue and pre-treated garbage pyrolysis gasification residue to obtain a mixture;
[0028] (2) subjecting the mixture obtained in step (1) to post-treatment and extrusion molding to obtain a brick;
[0029] (3) The brick blanks obtained in step (2) are post-treated and then calcined to obtain sintered porous bricks made of garbage pyrolysis gasification residue.
[0030] In one embodiment of the present invention, in step (1), the pre-treated garbage pyrolysis and gasification residue is garbage pyrolysis and gasification residue that has been subjected to screening treatment.
[0031] In one embodiment of the present invention, during the screening process, the sieve hole diameter is 2 mm.
[0032] In one embodiment of the present invention, the mass percentages of clay, coal gangue and pre-treated garbage pyrolysis gasification residue are 45%-80%: 10%-15%: 10%-40%;
[0033] The sum of the mass percentages of clay, coal gangue and pre-treated garbage pyrolysis gasification residue is 100%.
[0034] In one embodiment of the present invention, the mass percentages of clay, coal gangue and pre-treated garbage pyrolysis gasification residue are 50%:10%:40%.
[0035] In one embodiment of the present invention, in step (2), the post-treatment is to further mix the mixture after aging.
[0036] In one embodiment of the present invention, the aging process lasts for 24 hours to 48 hours;
[0037] The matured mixture is mixed by two-stage double-roll stirring.
[0038] In one embodiment of the present invention, in step (2), during the extrusion molding process, water is added to ensure that the moisture content of the brick is 10%-20%.
[0039] In one embodiment of the present invention, in step (3), the post-treatment is a drying treatment, and the drying treatment takes 3 to 4 days.
[0040] In one embodiment of the present invention, in step (3), during the calcination process, the temperature is 950°C-1050°C.
[0041] The invention provides a sintered porous brick made of garbage pyrolysis and gasification residue prepared by the method.
[0042] The present invention provides an application of the above-mentioned garbage pyrolysis gasification residue sintered porous bricks in the construction industry.
[0043] The present invention is described in detail below with reference to specific embodiments.
[0044] In the following examples, unless otherwise specified, all reagents used are commercially available reagents, and all detection means and methods used are conventional detection means and methods in the art.
[0045] In the following embodiments, the pre-treated garbage pyrolysis gasification residues were screened using a vibrating screen machine with a mesh size of 2 mm, and the particles with a particle size of less than 1.18 mm accounted for more than 90%.
[0046] In the following examples, the calcination process is carried out by slowly raising the temperature to 950-1050°C and sintering at 950-1050°C for 2 hours.
[0047] There are five stages in the roasting process, which are as follows:
[0048] (1) Room temperature - 100℃: low temperature preheating stage of the brick. This stage is mainly to remove the natural moisture remaining in the brick. After drying and baking, the moisture content of the brick is generally less than 7%. However, the moisture inside the body can only be discharged from the pores of the brick due to heat vaporization. Maintain the temperature for 30 minutes. If the temperature rises too quickly, the water vapor will increase rapidly and burst the brick.
[0049] (2) 100-400℃: Medium temperature preheating stage. In this stage, chemically bound water is discharged, and the mechanical strength of the brick will gradually increase but will not shrink; at 400℃, the organic matter in the brick begins to burn with oxygen, and the fuel mixed in it also begins to burn without flame. The brick slowly turns red, heats up and shines by itself, and is kept warm for 45 minutes.
[0050] (3) 400-600℃: high temperature preheating stage. At the end of this stage, at about 550-600℃, the SiO2 in the brick will undergo a crystal transformation, and the volume effect will increase. At this time, if stress is not concentrated, the volume of the brick will expand violently. However, due to the slow transformation speed, the liquid phase will have a certain buffering effect to offset part of the solid expansion stress. At this time, choose to keep warm for 60 minutes to prevent large cracks.
[0051] (4) 600-800℃: High temperature calcination stage. This stage ensures uniform heating of the green body and sufficient internal reaction. Before the sintering temperature is reached, the mixed material particles will become semi-molten, and the pores between the unmelted particles will be filled with molten particles to interlock and bond with each other, increasing the density. This stage is set to keep warm for 60 minutes.
[0052] (5) 950-1050℃: high temperature sintering stage. In this stage, the temperature is kept for 2 hours, and the waste pyrolysis gasification residue is sintered into porous bricks, which are then cooled with the furnace.
[0053] Example 1
[0054] The present embodiment provides a sintered porous brick made of garbage pyrolysis and gasification residue and a preparation method thereof.
[0055] (1) The waste pyrolysis and gasification residue from the waste pyrolysis and gasification incineration plant in the Economic Development Zone of Langxi County, Anhui Province was sieved using a vibrating screen with a sieve hole of 2 mm to obtain the pretreated waste pyrolysis and gasification residue ();
[0056] (2) mixing clay, coal gangue and the pretreated garbage pyrolysis gasification residue obtained in step (1) in a weight percentage of 80%:10%:10% to obtain a mixture;
[0057] (3) The mixture obtained in step (2) is aged in an aging tank for 36 hours, then further mixed by two-stage double-roll stirring, and then sent to a vacuum brick extruder for extrusion molding (during the extrusion molding process, water is added to ensure that the moisture content of the brick is 15%) to obtain a brick;
[0058] (4) The bricks obtained in step (3) are placed in a cool and ventilated place for natural drying for 3 days, and sintered at 950° C. for 2 hours to obtain sintered porous bricks made of garbage pyrolysis gasification residue.
[0059] The average compressive strength of the sintered porous bricks made of garbage pyrolysis gasification residue prepared in this embodiment is 27.73 MPa, the standard value of compressive strength is 20.49 MPa, the average boiling water absorption rate is 16.75%, the saturation coefficient is 0.866, and the heavy metal leaching toxicity is lower than the limit value of "Green Product Evaluation Wall Materials".
[0060] The garbage pyrolysis gasification residue prepared in this embodiment can be further applied in the construction industry.
[0061] Example 2
[0062] The present embodiment provides a sintered porous brick made of garbage pyrolysis and gasification residue and a preparation method thereof.
[0063] (1) sieving the waste pyrolysis and gasification residue from the urban waste pyrolysis and gasification incineration plant in Heishui County, Sichuan Province using a vibrating screen with a sieve hole of 2 mm to obtain pretreated waste pyrolysis and gasification residue;
[0064] (2) mixing clay, coal gangue and the pretreated garbage pyrolysis gasification residue obtained in step (1) in a weight percentage of 60%:10%:30% to obtain a mixture;
[0065] (3) The mixture obtained in step (2) is aged in an aging tank for 36 hours, then further mixed by two-stage double-roll stirring, and then sent to a vacuum brick extruder for extrusion molding (during the extrusion molding process, water is added to ensure that the moisture content of the brick is 15%) to obtain a brick;
[0066] (4) The bricks obtained in step (3) are placed in a cool and ventilated place for natural drying for 3 days, and sintered at 950° C. for 2 hours to obtain sintered porous bricks made of garbage pyrolysis gasification residue.
[0067] The average compressive strength of the sintered porous bricks made of garbage pyrolysis gasification residue prepared in this embodiment is 20.84 MPa, the standard value of compressive strength is 16.17 MPa, the average boiling water absorption rate is 18.75%, the saturation coefficient is 0.861, and the heavy metal leaching toxicity is lower than the limit value of "Green Product Evaluation Wall Materials".
[0068] The garbage pyrolysis gasification residue prepared in this embodiment can be further applied in the construction industry.
[0069] Example 3
[0070] The present embodiment provides a sintered porous brick made of garbage pyrolysis and gasification residue and a preparation method thereof.
[0071] (1) sieving the waste pyrolysis and gasification residue from the urban waste pyrolysis and gasification incineration plant in Heishui County, Sichuan Province using a vibrating screen with a sieve hole of 2 mm to obtain pretreated waste pyrolysis and gasification residue;
[0072] (2) mixing clay, coal gangue and the pretreated garbage pyrolysis gasification residue obtained in step (1) in a weight percentage of 60%:10%:30% to obtain a mixture;
[0073] (3) The mixture obtained in step (2) is aged in an aging tank for 36 hours, then further mixed by two-stage double-roll stirring, and then sent to a vacuum brick extruder for extrusion molding (during the extrusion molding process, water is added to ensure that the moisture content of the brick is 15%) to obtain a brick;
[0074] (4) The bricks obtained in step (3) are placed in a cool and ventilated place for natural drying for 3 days, and sintered at 1000° C. for 2 hours to obtain sintered porous bricks made of garbage pyrolysis gasification residue.
[0075] The average compressive strength of the sintered porous bricks made of garbage pyrolysis gasification residue prepared in this embodiment is 22.14 MPa, the standard value of compressive strength is 17.72 MPa, the average boiling water absorption rate is 18.13%, the saturation coefficient is 0.847, and the heavy metal leaching toxicity is lower than the limit value of "Green Product Evaluation Wall Materials".
[0076] The garbage pyrolysis gasification residue prepared in this embodiment can be further applied in the construction industry.
[0077] Example 4
[0078] The present embodiment provides a sintered porous brick made of garbage pyrolysis and gasification residue and a preparation method thereof.
[0079] (1) sieving the waste pyrolysis and gasification residue from the urban waste pyrolysis and gasification incineration plant in Heishui County, Sichuan Province using a vibrating screen with a sieve hole of 2 mm to obtain pretreated waste pyrolysis and gasification residue;
[0080] (2) mixing clay, coal gangue and the pretreated garbage pyrolysis gasification residue obtained in step (1) in a weight percentage of 50%:10%:40% to obtain a mixture;
[0081] (3) The mixture obtained in step (2) is aged in an aging tank for 36 hours, then further mixed by two-stage double-roll stirring, and then sent to a vacuum brick extruder for extrusion molding (during the extrusion molding process, water is added to ensure that the moisture content of the brick is 15%) to obtain a brick;
[0082] (4) The bricks obtained in step (3) are placed in a cool and ventilated place for natural drying for 3 days, and sintered at 950° C. for 2 hours to obtain sintered porous bricks made of garbage pyrolysis gasification residue.
[0083] The average compressive strength of the sintered porous bricks made of garbage pyrolysis gasification residue prepared in this embodiment is 19.12 MPa, the standard compressive strength is 14.06 MPa, the average boiling water absorption is 18.92%, the saturation coefficient is 0.874, and the heavy metal leaching toxicity is lower than the limit value of "Green Product Evaluation Wall Materials".
[0084] The garbage pyrolysis gasification residue prepared in this embodiment can be further applied in the construction industry.
[0085] Comparative Example 1
[0086] This comparative example provides a sintered porous brick and a preparation method thereof.
[0087] (1) sieving the waste pyrolysis and gasification residue from the urban waste pyrolysis and gasification incineration plant in Heishui County, Sichuan Province using a vibrating screen with a sieve hole of 2 mm to obtain pretreated waste pyrolysis and gasification residue;
[0088] (2) mixing clay, coal gangue and the pretreated garbage pyrolysis gasification residue obtained in step (1) in weight percentages of 55%:10%:45% to obtain a mixture;
[0089] (3) The mixture obtained in step (2) is aged in an aging tank for 36 hours, then further mixed by two-stage double-roll stirring, and then sent to a vacuum brick extruder for extrusion molding (during the extrusion molding process, water is added to ensure that the moisture content of the brick is 15%) to obtain a brick;
[0090] (4) The bricks obtained in step (3) are placed in a cool and ventilated place for natural drying for 3 days, and sintered at 950° C. for 2 hours to obtain sintered porous bricks made of garbage pyrolysis gasification residue.
[0091] The average compressive strength of the sintered porous bricks made of garbage pyrolysis gasification residue prepared in this comparative example is 17.28 MPa, the standard value of compressive strength is 13.21 MPa, the average boiling water absorption rate is 19.01%, the saturation coefficient is 0.892 (does not meet the standard requirement of the saturation coefficient not exceeding 0.88), and the heavy metal leaching toxicity is lower than the limit value of the "Green Product Evaluation Wall Materials".
[0092] Comparative Example 2
[0093] This comparative example provides a sintered porous brick and a preparation method thereof.
[0094] (1) sieving the waste pyrolysis and gasification residue from the urban waste pyrolysis and gasification incineration plant in Heishui County, Sichuan Province using a vibrating screen with a sieve hole of 2 mm to obtain pretreated waste pyrolysis and gasification residue;
[0095] (2) mixing clay, coal gangue and the pretreated garbage pyrolysis gasification residue obtained in step (1) in a weight percentage of 40%:10%:50% to obtain a mixture;
[0096] (3) The mixture obtained in step (2) was aged in an aging tank for 36 hours, then further mixed by two-stage double-roll stirring, and then sent to a vacuum brick extruder for extrusion molding (during the extrusion molding process, water was added to ensure that the moisture content of the bricks was 15%), but the bricks could not be extruded.
[0097] Comparative Example 3
[0098] This comparative example provides a sintered porous brick and a preparation method thereof.
[0099] (1) sieving the waste pyrolysis and gasification residue from the urban waste pyrolysis and gasification incineration plant in Heishui County, Sichuan Province using a vibrating screen with a sieve hole of 2 mm to obtain pretreated waste pyrolysis and gasification residue;
[0100] (2) mixing clay, coal gangue and the pretreated garbage pyrolysis gasification residue obtained in step (1) in a weight percentage of 60%:10%:30% to obtain a mixture;
[0101] (3) The mixture obtained in step (2) is aged in an aging tank for 36 hours, then further mixed by two-stage double-roll stirring, and then sent to a vacuum brick extruder for extrusion molding (during the extrusion molding process, water is added to ensure that the moisture content of the brick is 15%) to obtain a brick;
[0102] (4) The bricks obtained in step (3) are placed in a cool and ventilated place for natural drying for 3 days, and sintered at 900° C. for 2 hours to obtain sintered porous bricks made of garbage pyrolysis gasification residue.
[0103] The average compressive strength of the sintered porous bricks made of garbage pyrolysis gasification residue prepared in this comparative example is 18.65 MPa, the standard value of compressive strength is 15.84 MPa, the average boiling water absorption rate is 19.36%, the saturation coefficient is 0.888 (does not meet the standard requirement that the saturation coefficient is not more than 0.88), and the heavy metal leaching toxicity is lower than the limit value of the "Green Product Evaluation Wall Materials".
[0104] Comparative Example 4
[0105] This comparative example provides a sintered porous brick and a preparation method thereof.
[0106] (1) sieving the waste pyrolysis and gasification residue from the urban waste pyrolysis and gasification incineration plant in Heishui County, Sichuan Province using a vibrating screen with a sieve hole of 2 mm to obtain pretreated waste pyrolysis and gasification residue;
[0107] (2) mixing clay, coal gangue and the pretreated garbage pyrolysis gasification residue obtained in step (1) in a weight percentage of 60%:10%:30% to obtain a mixture;
[0108] (3) The mixture obtained in step (2) is aged in an aging tank for 36 hours, then further mixed by two-stage double-roll stirring, and then sent to a vacuum brick extruder for extrusion molding (during the extrusion molding process, water is added to ensure that the moisture content of the brick is 15%) to obtain a brick;
[0109] (4) The bricks obtained in step (3) are placed in a cool and ventilated place for natural drying for 3 days, and sintered at 1100° C. for 2 hours to obtain sintered porous bricks made of garbage pyrolysis gasification residue.
[0110] The surface of the sintered porous bricks made of garbage pyrolysis gasification residue prepared in this comparative example is black and sticky, showing an "overburning" phenomenon.
[0111] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the explanation of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.
Claims
1. A method for preparing sintered porous bricks from garbage pyrolysis and gasification residue, characterized in that: The following steps are involved: (1) mixing clay, coal gangue and pre-treated garbage pyrolysis gasification residue to obtain a mixture; (2) post-treating the mixture obtained in step (1) and extruding it to obtain a brick; (3) post-treating the bricks obtained in step (2) and then calcining them to obtain sintered porous bricks made of the waste pyrolysis gasification residue; The mass percentages of clay, coal gangue and pre-treated garbage pyrolysis gasification residue are 50%:10%:40%, or 80%:10%:10%, or 60%:10%:30%. In step (1), the pre-treated waste pyrolysis and gasification residue is the waste pyrolysis and gasification residue that has been subjected to screening treatment; during the screening treatment, the sieve hole diameter is 2 mm; In step (2), the post-treatment is to perform aging treatment on the mixture and then mix it evenly; During the aging process, the time is 24h-48h; During the extrusion process, water is added to ensure that the moisture content of the brick is 10%-20%; In step (3), the roasting process has five stages, which are as follows: 1) Room temperature -100℃, keep warm for 30min; 2) 100-400℃, keep warm for 45 minutes; 3) 400-600℃, keep warm for 60min; 4) 600-800℃, keep warm for 60min; 5) 950-1050℃, keep warm for 2h; In step (3), the post-treatment is a drying treatment, and the drying treatment takes 3 to 4 days.
2. A sintered porous brick made from garbage pyrolysis and gasification residue prepared by the method of claim 1.