A method for preparing a self-healing marine antifouling coating of organic silicon
By introducing the reaction of bisaminopropyl-terminated polydimethylsiloxane with isophorone diisocyanate, combining amide bonds and hydrogen bonds, forming a polyurethane material with self-healing ability, solving the protection of traditional silicone coatings The problem of degradation of capacity has achieved high-strength and self-healing coating performance, which is suitable for marine pollution prevention fields.
Patent Information
- Application Number
- CN202310392396.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-13
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-04-13
AI Technical Summary
Traditional silicone coatings are susceptible to physical damage and corrosion during use, resulting in a decrease in protection ability, and the self-healing time is too long and unstable, making it difficult to achieve effective self-healing in the coating.
By introducing diaminopropyl-terminated polydimethylsiloxane reacts with isophorone diisocyanate under nitrogen protection, combining amide bonds and hydrogen bonds, forming a polyurethane material with self-healing ability and curing in an oven To improve the mechanical properties of the coating.
The prepared silicone coating has high strength, low surface energy and self-healing ability. It is suitable as a marine anti-fouling and anti-corrosion coating, which significantly improves the durability and protective performance of the coating.
Smart Images

Figure CN116254043B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of novel polymer marine antifouling, and in particular to a method for preparing a marine antifouling coating material with relatively high strength and self-healing ability. Background Art
[0002] The main chain of polydimethylsiloxane (PDMS) is an organic silicon material composed of Si-O. The bond angle of Si-O bond is large and easy to rotate, which makes PDMS have good segment movement ability, also known as segment flexibility; PDMS has good high temperature resistance, weather resistance, corrosion resistance, low surface energy, water resistance and chemical inertness, and is often used as a self-cleaning coating. Commonly used PDMS has active functional groups such as hydroxyl, carboxyl, and amino groups, and is modified by reacting active functional groups with other substances to improve its hardness and adhesion to the substrate. Traditional silicone coatings are susceptible to physical damage such as scratches and tears during use. As the use time increases, the damaged parts are corroded by corrosive media day and night, and finally corrode the metal substrate. In addition, the Si-O bond energy is large and there are no other atoms around the O atom to block it, so it is easy to rotate. The flexibility of the siloxane molecular chain is stronger than that of the alkane chain, and PDMS has a very low modulus; for the coating, the low modulus of the coating means that the coating has low hardness, that is, it cannot resist even tiny scratches. Therefore, modified PDMS coatings are the development trend of silicone coatings.
[0003] Isophorone diisocyanate (IPDI) is a commonly used raw material for synthesizing polyurethane. Generally, IPDI and PDMS with -NH2 are used to synthesize self-healing organosilicon-modified polyurethane. The self-healing time of the self-healing organosilicon-modified polyurethane is too long and it is likely to be damaged twice during the self-healing process. It will be damaged three times during the secondary self-healing. In this way, the organosilicon-modified polyurethane coating will completely lose its protective ability. In this regard, how to achieve self-healing has become a focus of researchers. There are many studies reporting that polymers with three-dimensional structures cross-linked by double dynamic bonds can achieve the effect of self-healing, but few studies have realized self-healing on coatings. Inspired by this, PDMS is modified to introduce a dynamic covalent bond, and then synthesized with IPDI to obtain a polyurethane material with self-healing ability. However, while giving the material self-healing ability, the mechanical properties of the coating will also decrease. By introducing amide bonds, hydrogen bonds and disulfide bonds, the mechanical strength of the coating is improved while ensuring the self-healing ability. Summary of the invention
[0004] In view of the deficiencies of the prior art, the present invention provides an organic silicon coating with high strength, self-healing ability and low surface energy and a preparation method to solve the above problems.
[0005] The technical solution of the present invention is:
[0006] According to the present invention, a method for preparing a high-strength marine antifouling coating with self-healing ability comprises the following specific steps:
[0007] (1) The bisaminopropyl-terminated polydimethylsiloxane is vacuum dried at 110° C., cooled to room temperature for later use after vacuum drying, and the dried bisaminopropyl-terminated polydimethylsiloxane is dissolved in anhydrous xylene;
[0008] (2) reacting the polydimethylsiloxane containing bisaminopropyl end-capping obtained in step (1) with terephthalaldehyde (TA) at 80° C. for 12 h under nitrogen protection to obtain H2N-PDMS-TA-H2N prepolymer, and removing the solvent and unreacted monomers by rotary evaporation after the reaction to obtain a light yellow transparent viscous product;
[0009] (3) dissolving the prepolymer obtained in step (2) in a tetrahydrofuran / isopropanol mixed solvent, and similarly dissolving isophorone diisocyanate in a tetrahydrofuran / isopropanol mixed solvent, and adding the mixture to the prepolymer solution, reacting at room temperature for 3 h under nitrogen protection to ensure sufficient reaction;
[0010] (4) dissolving the product obtained in step (3) in a mixed solvent of tetrahydrofuran / isopropanol, and similarly dissolving 2'2-diaminodiphenyl disulfide in a mixed solvent of tetrahydrofuran / isopropanol, and mixing the two solutions;
[0011] (5) reacting the mixed solution in step (4) at room temperature for 3 h under nitrogen protection to obtain the product TA-PDMS-PU;
[0012] (6) The product TA-PDMS-PU obtained in step (5) is subjected to rotary evaporation to remove the tetrahydrofuran / isopropanol mixed solvent, and is placed in an oven for curing for 48 hours to obtain the coating.
[0013] According to the present invention, preferably, the solvent in step (1) is xylene, which can be obtained through commercial channels.
[0014] According to the present invention, preferably, the chain extender in step (2) is terephthalaldehyde.
[0015] According to the present invention, preferably, the reaction temperature in step (2) is 80°C.
[0016] According to the present invention, preferably, the reaction time in step (2) is 12 h.
[0017] According to the present invention, preferably, the isocyanate in step (3) is isophorone diisocyanate.
[0018] According to the present invention, preferably, the volume ratio of the solvent tetrahydrofuran to isopropanol in steps (3) and (4) is 1:1.
[0019] According to the present invention, preferably, the reaction time in steps (3) and (5) is 3 hours.
[0020] According to the present invention, preferably, the chain extender in step (4) is 2'2-diaminodiphenyl disulfide.
[0021] The technical advantages of the present invention are as follows:
[0022] (1) The preparation process of the present invention is simple and controllable. By introducing amide bonds and urea bonds, the content of hydrogen bonds in the coating is increased, thereby increasing the strength of the generated polymer.
[0023] (2) The organic silicon coating material prepared by the present invention has the advantages of low surface energy, high strength, and self-healing ability, and is very suitable for use as a marine antifouling and anticorrosion coating. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 The water contact angle test result of the organosilicon coating material prepared in Example 1 of the present invention is shown in FIG.
[0025] The water contact angle on the coating surface was measured using a contact angle meter. A 4μL deionized water droplet was used for the test, and the photo was taken and measured within 5 to 10 seconds after the droplet fell on the coating surface. The contact angle of deionized water on the coating surface was measured using the angle measurement method, and the average value was taken to calculate the surface free energy of the material using the Owens method.
[0026] Figure 2 The tensile strength test result of the organosilicon coating material prepared in Example 1 of the present invention is shown in FIG.
[0027] The tensile strength of the coating was tested using a universal tensile testing machine at a tensile speed of 100 mm min -1 Take 5 sets of 50*4mm parallel samples and test the tensile strength of the coating when it breaks.
[0028] Figure 3 The self-cleaning test results of the organosilicon coating material prepared in Example 1 of the present invention are shown.
[0029] Tilt the coated glass plate by 15°, drop 1 ml of deionized water and CuCl2 solution on the glass plate and slide it down to see if there are any droplets left.
[0030] Figure 4 The adhesion test results of the organosilicon coating material prepared in Example 1 of the present invention are shown.
[0031] Use an adhesion tester to test the bonding strength of the coating on different substrates.
[0032] Figure 5 The self-healing test results of the organosilicon coating material prepared in Example 1 of the present invention are shown.
[0033] A 2-cm-long cross scratch was made on the coating surface using a scalpel, and the coated carbon steel sheet was placed in an oven at 50 °C for 4 h. DETAILED DESCRIPTION
[0034] The present invention will be further described below with reference to specific embodiments and drawings, but is not limited thereto.
[0035] Meanwhile, the experimental methods described in the following examples are conventional methods unless otherwise specified, and the reagents and materials are commercially available unless otherwise specified.
[0036] Embodiment 1:
[0037] 8mmol bisaminopropyl-terminated polydimethylsiloxane (Mn~1000) was vacuum dried at 110°C and completely dissolved in dry xylene, added into a 250ml three-necked flask equipped with a constant pressure separatory funnel and a spherical condenser and introduced with nitrogen, 4mmol terephthalaldehyde was dissolved in 20ml dry xylene and transferred to a constant pressure separatory funnel, the xylene solution mixed with terephthalaldehyde was slowly dripped into the xylene solution of bisaminopropyl-terminated polydimethylsiloxane, the reaction was stirred at a constant temperature of 80°C for 12h, the reaction was cooled to room temperature after the reaction was completed, the solvent xylene and unreacted substances were removed by rotary evaporation at 65°C to obtain a light yellow transparent viscous product, and the H2N-PDMS-TA-H2N prepolymer was synthesized.
[0038] In a three-necked flask, 4 mmol of H2N-PDMS-TA-H2N prepolymer was dissolved in tetrahydrofuran / isopropanol (V THF :V 异丙醇 =1:1) mixed solvent to prepare a 1g / ml solution. Similarly, 8mmol of isophorone diisocyanate was dissolved in tetrahydrofuran / isopropanol (V THF :V 异丙醇 =1:1) mixed solvent to prepare a solution of the same concentration, transfer it to a constant pressure separatory funnel, slowly drop isophorone diisocyanate into the H2N-PDMS-TA-H2N prepolymer solution, react at room temperature for 3h under nitrogen atmosphere, then dissolve 4mmol 2'2-diaminodiphenyl disulfide in 10ml tetrahydrofuran / isopropanol (V THF :V 异丙醇=1:1) mixed solvent, the reaction system was added, and the reaction was carried out at room temperature for 3 hours under a nitrogen atmosphere. After the reaction, the solvent and unreacted monomers were removed by rotary evaporation at 40°C to obtain a yellow transparent viscous product, which was named TA-PDMS-PU-1. The final product TA-PDMS-PU-1 was transferred to a polytetrafluoroethylene mold and dried in an oven at 40°C for 48 hours to obtain the coating material.
[0039] The water contact angle test results of the organic silicon coating material prepared in this embodiment are as follows: Figure 1 As shown in Figure 2, the water contact angle of the coating material is 97.6° and the surface free energy is 27.818 mJ / m 2 .
[0040] The tensile strength test results of the organosilicon coating material prepared in this embodiment are as follows: Figure 2 As shown, the tensile strength of the coating material is 4.5 MPa.
[0041] The self-cleaning test results of the organic silicon coating material prepared in this embodiment are as follows: Figure 3 As shown, the coating material has good self-cleaning performance.
[0042] The adhesion test results of the glass and carbon steel sheet of the organic silicon coating material prepared in this embodiment are as follows: Figure 4 As shown, the coating material has a relatively high adhesion force of 1.21 MPa on the Q235 carbon steel sheet and 1.9 MPa on the glass.
[0043] The self-healing test results of the organic silicon coating material prepared in this embodiment are as follows: Figure 5 As shown, the coating material has self-healing ability.
[0044] Embodiment 2:
[0045] 8mmol bisaminopropyl-terminated polydimethylsiloxane (Mn~1000) was vacuum dried at 110°C and completely dissolved in dry xylene, added into a 250ml three-necked flask equipped with a constant pressure separatory funnel and a spherical condenser and introduced with nitrogen, 4mmol terephthalaldehyde was dissolved in 20ml dry xylene and transferred to a constant pressure separatory funnel, the xylene solution mixed with terephthalaldehyde was slowly dripped into the xylene solution of bisaminopropyl-terminated polydimethylsiloxane, the reaction was stirred at a constant temperature of 80°C for 12h, the reaction was cooled to room temperature after the reaction was completed, the solvent xylene and unreacted substances were removed by rotary evaporation at 65°C to obtain a light yellow transparent viscous product, and the H2N-PDMS-TA-H2N prepolymer was synthesized.
[0046] In a three-necked flask, 4 mmol of H2N-PDMS-TA-H2N prepolymer was dissolved in tetrahydrofuran / isopropanol (V THF:V 异丙醇 =1:1) mixed solvent to prepare a 1g / ml solution. Similarly, 8mmol of isophorone diisocyanate was dissolved in tetrahydrofuran / isopropanol (V THF :V 异丙醇 =1:1) mixed solvent to prepare a solution of the same concentration, transfer it to a constant pressure separatory funnel, slowly drop isophorone diisocyanate into the H2N-PDMS-TA-H2N prepolymer solution, react at room temperature for 3h under nitrogen atmosphere, then dissolve 2mmol 2'2-diaminodiphenyl disulfide in 10ml tetrahydrofuran / isopropanol (V THF :V 异丙醇 =1:1) mixed solvent was added into the reaction system, and the reaction was carried out at room temperature for 3 hours under a nitrogen atmosphere. After the reaction, the solvent and unreacted monomers were removed by rotary evaporation at 40°C to obtain a yellow transparent viscous product, which was named TA-PDMS-PU-0.5. The final product TA-PDMS-PU-0.5 was transferred into a polytetrafluoroethylene mold and dried in an oven at 40°C for 48 hours to obtain the coating material.
[0047] The water contact angle test results of the organic silicon coating material prepared in this embodiment are as follows: Figure 1 As shown, the water contact angle of the coating material is 96.24° and the surface free energy is 28.104 mJ / m 2 .
[0048] The tensile strength test results of the organosilicon coating material prepared in this embodiment are as follows: Figure 2 As shown, the tensile strength of the coating material is 2.4 MPa.
[0049] The self-cleaning test results of the organic silicon coating material prepared in this embodiment are as follows: Figure 3 As shown, the coating material has good self-cleaning performance.
[0050] The test results of the adhesion test of the glass and carbon steel sheet of the organic silicon coating material prepared in this embodiment are as follows: Figure 4 As shown, the adhesion of the coating material on the Q235 carbon steel sheet is 1.19 MPa, and the adhesion on the glass is 1.64 MPa.
[0051] The self-healing test results of the organic silicon coating material prepared in this embodiment are as follows: Figure 5 As shown, the coating material has self-healing ability.
[0052] Embodiment 3:
[0053] 8mmol of bis-aminopropyl-terminated polydimethylsiloxane (Mn-1000) was dried under vacuum at 110°C and completely dissolved in dry xylene. The mixture was added into a 250ml three-necked flask equipped with a constant pressure separatory funnel and a spherical condenser and nitrogen was introduced. 4mmol of terephthalaldehyde was dissolved in 20ml of dry xylene and transferred to a constant pressure separatory funnel. The xylene solution mixed with terephthalaldehyde was slowly dripped into the xylene solution of bis-aminopropyl-terminated polydimethylsiloxane. The mixture was stirred at a constant temperature of 80°C for 12h. After the reaction was completed, the mixture was cooled to room temperature. The solvent xylene and unreacted substances were removed by rotary evaporation at 80°C to obtain a yellow transparent viscous product to synthesize H2N-PDMS-TA-H2N prepolymer.
[0054] In a three-necked flask, 4 mmol of H2N-PDMS-TA-H2N prepolymer was dissolved in tetrahydrofuran / isopropanol (V THF :V 异丙醇 =1:1) mixed solvent to prepare a 1g / ml solution. Similarly, 8mmol of isophorone diisocyanate was dissolved in tetrahydrofuran / isopropanol (V THF :V 异丙醇 =1:1) mixed solvent to prepare a solution of the same concentration, transferred to a constant pressure separatory funnel, slowly added isophorone diisocyanate dropwise to the H2N-PDMS-TA-H2N prepolymer solution, reacted at room temperature for 3 hours under a nitrogen atmosphere, named TA-PDMS-PU, and the final product TA-PDMS-PU was transferred to a polytetrafluoroethylene mold and dried in an oven at 40°C for 48 hours to obtain the coating material.
[0055] The water contact angle test results of the organic silicon coating material prepared in this embodiment are as follows: Figure 1 As shown, the water contact angle of the coating material is 96.75° and the surface free energy is 27.997 mJ / m 2 .
[0056] The tensile strength test results of the organosilicon coating material prepared in this embodiment are as follows: Figure 2 As shown, the tensile strength of the coating material is 0.4 MPa.
[0057] The self-cleaning test results of the organic silicon coating material prepared in this embodiment are as follows: Figure 3 As shown, the coating material has good self-cleaning performance.
[0058] The test results of the adhesion test of the glass and carbon steel sheet of the organic silicon coating material prepared in this embodiment are as follows: Figure 4 As shown, the adhesion of the coating material on the Q235 carbon steel sheet is 2.1 MPa, and the adhesion on the glass is 1.71 MPa.
[0059] The self-healing test results of the organic silicon coating material prepared in this embodiment are as follows: Figure 5 As shown, the coating material has self-healing ability.
Claims
1. A method for preparing a high-strength marine antifouling coating with self-healing ability, comprising the following steps: (1) The bisaminopropyl-terminated polydimethylsiloxane is vacuum dried at 110° C., cooled to room temperature for later use after vacuum drying, and the dried bisaminopropyl-terminated polydimethylsiloxane is dissolved in anhydrous xylene; (2) reacting the polydimethylsiloxane containing bisaminopropyl end-capping obtained in step (1) with terephthalaldehyde at 80° C. for 12 h under nitrogen protection to obtain H2N-PDMS-TA-H2N prepolymer; (3) dissolving the prepolymer obtained in step (2) in a tetrahydrofuran / isopropanol mixed solvent, and similarly dissolving isophorone diisocyanate in a tetrahydrofuran / isopropanol mixed solvent, and adding the mixture to the prepolymer solution, reacting at room temperature for 3 h under nitrogen protection to ensure sufficient reaction; (4) dissolving the product obtained in step (3) in a mixed solvent of tetrahydrofuran / isopropanol, and similarly dissolving 2'2-diaminodiphenyl disulfide in a mixed solvent of tetrahydrofuran / isopropanol, and mixing the two solutions; (5) reacting the mixed solution in step (4) at room temperature for 3 h under nitrogen protection to obtain the product TA-PDMS-PU; (6) removing the tetrahydrofuran / isopropanol mixed solvent from the product TA-PDMS-PU obtained in step (5) by rotary evaporation, and curing in an oven for 48 hours to obtain the coating; TA in step (2) is terephthalaldehyde; The volume ratio of the solvent tetrahydrofuran to isopropanol described in steps (3) and (4) is 1:1.
Citation Information
Cited By
A polyimide super-slip surface with self-repairing properties and its preparation method and application