Preparation method and application of doped modified indium oxide-based composite material

The doped modified indium oxide-based composite material was prepared by a one-step hydrothermal method, and the use of iron titanate to modify indium oxide was solved, and the problem of low photocatalytic activity of indium oxide was achieved, which was effective in the utilization of solar energy and efficient degradation of environmental pollutants was achieved. .

CN116273017BActive Publication Date: 2024-11-15NANTONG VOCATIONAL COLLEGE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310297229.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-11-15
Estimated Expiration
2043-03-24

AI Technical Summary

Technical Problem

The application of indium oxide as a semiconductor material in the field of photocatalysis is limited by its wide band gap and easy recombination of photogenerated carriers, resulting in its low photocatalytic activity. No prior art has been found to use iron titanate to oxidize. Reports on the materials, preparation methods and applications of indium doping modification.

Method used

A one-step hydrothermal method is used to prepare doped modified indium oxide-based composite materials, modify indium oxide through iron titanate, expand its visible light absorption range, and accelerate the separation of photogenerated carriers through heterojunction structure to improve its light Catalytic properties.

Benefits of technology

The visible light response range of indium oxide is effectively expanded, the utilization efficiency of sunlight is improved, and the degradation rate of environmental pollutants such as methyl orange, rhodamine B, tetracycline is significantly improved, showing efficient photocatalytic performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116273017B_ABST
    Figure CN116273017B_ABST
Patent Text Reader

Abstract

The present invention provides a preparation method and application of a doped modified indium oxide-based composite material, and relates to the technical field of semiconductor photocatalytic materials. The composite material is prepared by a hydrothermal method using indium oxide as a main material and iron titanate as a modified material, and the preparation process is simple. The doped modified indium oxide-based composite material overcomes the defect that the indium oxide monomer only absorbs ultraviolet light, and its absorption range is extended to the visible light region, and solar energy can be used for driving more efficiently. The doped modified indium oxide-based composite material has good photodegradation performance for various antibiotics.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of semiconductor photocatalytic materials, and specifically relates to a preparation method and application of a doped and modified indium oxide-based composite material. Background Art

[0002] Semiconductor materials are a class of materials with semiconductor properties. The conductivity of semiconductors at room temperature is between conductors and insulators, and the resistivity is about 1mΩ·cm~1GΩ·cm. The main feature of semiconductors is the existence of a band gap, which refers to the energy difference between the guide band and the valence band. Interband excitation produces two types of carriers, free electrons and holes. The optical and electrical properties of semiconductors are related to the band gap. Semiconductor materials are divided into intrinsic semiconductors and impurity semiconductors according to the characteristics of carriers. Intrinsic semiconductors have equal numbers of free electrons and holes, and are free of impurities and defects. They are ideal semiconductors. Impurity semiconductors are doped with certain impurities, and impurity semiconductors can be divided into n-type semiconductors (structures with electrons as majority carriers) and p-type semiconductors (structures with holes as majority carriers). Since the application of germanium, silicon, etc., other semiconductors such as inorganic substances, organic substances, organic-inorganic composites and other types of materials have appeared one after another, and are widely used in chemical, pharmaceutical, electronic and military fields. Among them, inorganic metal oxides are particularly valued by scientists. They play an indispensable role in physics, chemistry, and materials science, and can be used to prepare battery materials, sensors, and catalysts.

[0003] Among many semiconductor materials, indium oxide (In2O3) is a typical n-type semiconductor material. It is in the form of light yellow powder, insoluble in water, but soluble in inorganic acid, with a density of 7.18 g / cm3 and a melting point of 2000°C. The band gap of indium oxide is relatively wide, with a direct band gap between 3.55 and 3.75 eV. Indium oxide has two phase structures: cubic iron manganese type and hexagonal corundum type. Indium oxide with a cubic structure is a stable structure, while indium oxide with a hexagonal structure is a metastable structure. It is usually a high-temperature and high-pressure phase. However, as a semiconductor material used in the field of photocatalysis, the band gap of single indium oxide is relatively wide, which limits its ability to respond to light. At the same time, the photogenerated carriers of indium oxide are easy to recombine, which seriously restricts its photocatalytic activity. Existing studies have conducted various modification studies on this issue. For example, Guo Yongfu's team from the School of Environmental Science and Engineering at Suzhou University of Science and Technology prepared In2O3 / CdS catalysts by in situ growing CdS on the In2O3 surface. The doping of CdS expands the absorption range of visible light, inhibits the recombination of photogenerated carriers, and enhances the photocatalytic performance of the catalyst.

[0004] Chinese patent CN202210891169.5 prepared Ag-modified In2O3 materials by solvent thermal and high temperature calcination. The synthesis method is simple and easy to operate, which is conducive to further industrialization. At the same time, using the precursor MIL-68 (In) as the template In2O3, the prepared Ag-modified In2O3 material can follow the rod-shaped structure of MIL-68 (In), which is conducive to CO2 adsorption, and the material has high catalytic activity and cyclic stability, and can achieve a good CO2 reduction effect at room temperature and pressure, and will not cause pollution in the process of using water as a proton source. Chinese patent CN201810323832.5 discloses a new type of In2O3 / BiOI composite semiconductor photocatalyst and its preparation method. The prepared composite semiconductor photocatalyst exhibits excellent photocatalytic degradation effect on rhodamine B, especially when the mass ratio of In2O3 is 5%, the degradation effect is the best, and the degradation of rhodamine B reaches 95.9% in 120 minutes.

[0005] However, to date, there has been no report on the materials, preparation methods and applications of indium oxide doped with iron titanate.

[0006] In view of the above background and research status, the present invention is proposed. Summary of the invention

[0007] The object of the present invention is to provide a method for preparing a doped modified indium oxide-based composite material, which is completed by only one hydrothermal step, has a simple preparation process and low cost. Indium oxide is modified by iron titanate having visible light absorption characteristics, and the absorption range of light by indium oxide monomer is expanded to absorb solar energy more efficiently. At the same time, the doped modified indium oxide-based composite material has good electron-hole separation and transfer efficiency.

[0008] Another object of the present invention is to provide a doped modified indium oxide-based composite material for use in fields such as removal of environmental pollutants.

[0009] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0010] In a first aspect, the present invention provides a method for preparing a doped modified indium oxide-based composite material, comprising the following steps: weighing an iron source and adding it to anhydrous ethanol to form a solution, slowly dropping a titanium source, and then adding an indium source, oxalic acid and sodium hydroxide, transferring the formed mixed solution into a hydrothermal kettle for reaction, washing and drying the obtained precipitate, and then calcining it in a muffle furnace to obtain the doped modified indium oxide-based composite material.

[0011] The valence state of iron in the iron source is +3, and the molar ratio of iron to titanium in the iron source and the titanium source is 1:1.

[0012] The iron source and indium source include but are not limited to one of nitrate, chloride and sulfate.

[0013] The titanium source includes but is not limited to one of tetrabutyl titanate and tetraisopropyl titanate.

[0014] In some embodiments, the ratio of the molar number of sodium hydroxide to the sum of the molar numbers of indium and iron elements is 1:(2-3), and the mass ratio of oxalic acid to sodium hydroxide is 1:2.

[0015] In some embodiments, the reaction temperature of the hydrothermal reactor is 160-200° C., and the reaction time is 20-40 hours.

[0016] In some embodiments, the calcination temperature of the muffle furnace is 400-600° C., and the calcination time is 1-2 hours.

[0017] In a second aspect, the present invention provides an application of a doped and modified indium oxide-based composite material prepared by the above-mentioned preparation method in the field of removing environmental pollutants.

[0018] The environmental pollutants include at least one of dyes such as methyl orange, rhodamine B, and antibiotics such as tetracycline.

[0019] As a preferred embodiment, a method for preparing a doped modified indium oxide-based composite material comprises the following steps: weighing an iron source and adding it to anhydrous ethanol to form a solution, slowly dropping a titanium source, and then adding an indium source, oxalic acid and sodium hydroxide, transferring the formed mixed solution into a hydrothermal kettle for reaction, washing and drying the obtained precipitate, and then calcining it in a muffle furnace to obtain a doped modified indium oxide-based composite material.

[0020] Wherein, in this step, the molar ratio of iron to titanium in the iron source and the titanium source is 1:1.

[0021] Wherein, in this step, the ratio of the molar number of sodium hydroxide to the sum of the molar numbers of indium and iron elements is 1:2, and the mass ratio of oxalic acid to sodium hydroxide is 1:2.

[0022] Wherein, in this step, the reaction temperature of the hydrothermal kettle is 180° C. and the reaction time is 30 hours.

[0023] Wherein, in this step, the calcination temperature of the muffle furnace is 500° C., and the calcination time is 1.5 hours.

[0024] The technical solution provided by the present invention has the following beneficial effects: the present invention adopts a one-step hydrothermal method to prepare a doped and modified indium oxide-based composite photocatalytic material, and the preparation process is simple; by doping and modifying indium oxide having only ultraviolet light absorption performance with iron titanate having visible light response performance, the visible light response range of indium oxide is effectively expanded, and the efficient use of sunlight is enhanced; at the same time, iron titanate and indium oxide form a heterojunction structure, which accelerates the separation of photogenerated carriers and exhibits extremely high visible light response performance, especially efficient removal of environmental pollutants such as methyl orange, rhodamine B, tetracycline, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is the XRD diagram of the sample obtained in Example 1 of the present invention. DETAILED DESCRIPTION

[0026] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] The present invention is further described below by way of examples. Unless otherwise specified, the materials in the examples are prepared according to existing methods or directly purchased from the market.

[0028] The reagents and raw materials used in the present invention are shown in Table 1 below:

[0029] Table 1 Reagents and raw materials used in the present invention

[0030]

[0031] Example 1

[0032] Accurately weigh 2.38 grams of ferric chloride, dissolve it in 50 milliliters of anhydrous ethanol to form a solution, slowly add 3 grams of tetrabutyl titanate, stir for 30 minutes, add 2.64 grams of indium nitrate, 0.175 grams of oxalic acid, and 0.35 grams of sodium hydroxide, continue to stir for 30 minutes, transfer to a 100-ml hydrothermal kettle, react at 160°C for 40 hours, wash the obtained precipitate with water and alcohol for 3 times each, vacuum dry it, place it in a crucible, and calcine it at 600°C in a muffle furnace for 1 hour to obtain an iron titanate-doped modified indium oxide composite material.

[0033] 100 mg of the prepared doped modified indium oxide composite material was placed in a beaker containing 100 ml of a 10 mg / L methyl orange solution, subjected to ultrasonic treatment for 2 minutes, dark adsorbed for 30 minutes, and then illuminated for 60 minutes with a 300-W xenon lamp at a distance of 20 cm from the liquid surface under stirring. After centrifugation, the solution after degradation was measured for its absorbance at 460 nm by a UV-visible spectrophotometer. The degradation rate of methyl orange was calculated to be 92.3%.

[0034] Example 2

[0035] Accurately weigh 2.38 grams of ferric chloride, dissolve it in 50 milliliters of anhydrous ethanol to form a solution, slowly add 3 grams of tetrabutyl titanate, stir for 30 minutes, add 2.64 grams of indium nitrate, 0.175 grams of oxalic acid, and 0.35 grams of sodium hydroxide, continue stirring for 30 minutes, transfer to a 100-ml hydrothermal kettle, react at 180°C for 30 hours, wash the obtained precipitate with water and alcohol for 3 times each, vacuum dry it, place it in a crucible, and calcine it at 500°C in a muffle furnace for 1.5 hours to obtain an iron titanate-doped modified indium oxide composite material.

[0036] 100 mg of the prepared doped modified indium oxide composite material was placed in a beaker containing 100 ml of a 10 mg / L rhodamine B solution, subjected to ultrasonic treatment for 2 minutes, dark adsorbed for 30 minutes, and then illuminated for 60 minutes with a 300-W xenon lamp light source at a distance of 20 cm from the liquid surface under stirring. After centrifugation, the degraded solution was measured for its absorbance at 554 nm by a UV-visible spectrophotometer, and the degradation rate of methyl orange was calculated to be 95.6%.

[0037] Example 3

[0038] Accurately weigh 2.38 grams of ferric chloride, dissolve it in 50 milliliters of anhydrous ethanol to form a solution, slowly add 3 grams of tetrabutyl titanate, stir for 30 minutes, add 2.64 grams of indium nitrate, 0.175 grams of oxalic acid, and 0.35 grams of sodium hydroxide, continue stirring for 30 minutes, transfer it into a 100-ml hydrothermal kettle, react at 200°C for 20 hours, wash the obtained precipitate with water and alcohol for 3 times each, vacuum dry it, place it in a crucible, and calcine it at 400°C in a muffle furnace for 1 hour to obtain an iron titanate-doped modified indium oxide composite material.

[0039] 100 mg of the prepared doped modified indium oxide composite material was placed in a beaker containing 100 ml of 10 mg / L tetracycline solution, ultrasonically treated for 2 minutes, dark adsorbed for 30 minutes, and then illuminated for 60 minutes with a 300-watt xenon lamp light source at a distance of 20 cm from the liquid surface under stirring. The degraded solution was centrifuged and its absorbance at 357 nm was measured by a UV-visible spectrophotometer. The degradation rate of methyl orange was calculated to be 86.4%.

[0040] Comparative Example 1

[0041] Accurately weigh 2.64 g of indium nitrate, 0.09 g of oxalic acid, and 0.175 g of sodium hydroxide, stir for 30 minutes, transfer to a 100 ml hydrothermal kettle, react at 160 ° C for 40 hours, wash the obtained precipitate with water and alcohol for 3 times each, vacuum dry it, place it in a crucible, and calcine it at 600 ° C in a muffle furnace for 1 hour to obtain unmodified indium oxide monomer material.

[0042] 100 mg of the prepared unmodified indium oxide monomer material was placed in a beaker containing 100 ml of a 10 mg / L methyl orange solution, subjected to ultrasonic treatment for 2 minutes, dark adsorbed for 30 minutes, and then illuminated for 60 minutes with a 300-W xenon lamp at a distance of 20 cm from the liquid surface under stirring. The degraded solution was centrifuged and its absorbance at 460 nm was measured by a UV-visible spectrophotometer. The degradation rate of methyl orange was calculated to be 37.8%.

[0043] It can be seen from Comparative Example 1 that the degradation effect of the prepared indium oxide monomer material on methyl orange is significantly lower than that of the doped and modified indium oxide composite material under the same conditions. This is mainly because the light absorption capacity of the indium oxide monomer is reduced, and the recombination probability of photogenerated electrons and holes is high, and sufficient photogenerated charges required for efficient photocatalytic reaction are not generated.

[0044] Characterization of doped modified indium oxide composites

[0045] The present invention uses a D8 Advance X-ray diffractometer from Bruker Spectroscopy Instruments of Germany to perform XRD analysis on the iron titanate / cerium oxide composite material prepared in Example 1 of the present invention, and the results are as follows: Figure 1 As shown, the test conditions are: Cu target Kα line, λ=0.15406nm, 2θ is 10°~70°, and the scanning speed is 5(°) / min. Figure 1 The diffraction peaks at 21.5°, 30.6°, 33.1°, 35.5°, 37.7° and 39.8° of 2θ correspond to the (211), (222), (321), (400), (411) and (420) crystal planes of indium oxide (PDF card 71-2195), respectively, with the space group la-3, a=b=c=10.117. The remaining diffraction peaks are all attributed to the (002), (200), (201), (110), (111), (112), (203), (004), (310), (400) and (113) crystal planes of iron titanate (PDF card 73-1631) with the space group Ccmm. All the fronts are sharp, indicating that the prepared samples have good crystal form and high purity.

[0046] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments can still be modified, or some or all of the technical features therein can be replaced by equivalents. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing an iron titanate-doped modified indium oxide-based heterojunction composite material, characterized in that: The method comprises the following steps: weighing an iron source and adding the solution to anhydrous ethanol to form a solution, slowly dropping a titanium source, then adding an indium source, oxalic acid and sodium hydroxide, transferring the formed mixed solution to a hydrothermal kettle for reaction, washing and drying the obtained precipitate, and then calcining the precipitate in a muffle furnace to obtain an iron titanate doped modified indium oxide-based heterojunction composite material, wherein the valence state of iron in the iron source is +3, the molar ratio of iron to titanium in the iron source and the titanium source is 1:1, the ratio of the molar number of the sodium hydroxide to the sum of the molar numbers of indium and iron elements is 1:(2-3), the mass ratio of oxalic acid to sodium hydroxide is 1:2, the reaction temperature of the hydrothermal kettle is 160-200°C, the reaction time is 20-40 hours, the calcination temperature of the muffle furnace is 400-600°C, and the calcination time is 1-2 hours.

2. The preparation method according to claim 1, characterized in that: The iron source and the indium source are one of nitrate, chloride and sulfate respectively.

3. The preparation method according to claim 1, characterized in that: The titanium source is one of tetrabutyl titanate and tetraisopropyl titanate.

4. Use of an iron titanate-doped modified indium oxide-based heterojunction composite material obtained by the preparation method described in any one of claims 1 to 3 in removing environmental pollutants.

5. The use according to claim 4, characterized in that: The environmental pollutant includes at least one of methyl orange, rhodamine B dye, or tetracycline antibiotics.