Preparation method of low-cost battery-grade iron phosphate and lithium iron phosphate
By using hydroxyethylene diphosphonic acid and microwave heating technology in the preparation of lithium iron phosphate battery materials, the problems of high cost and difficult removal of impurities in the existing technology have been solved, and high-quality and low-cost preparation of lithium iron phosphate materials has been achieved. , improving electrochemical performance and material density.
Patent Information
- Application Number
- CN202310151587.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-22
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-02-22
AI Technical Summary
In the existing lithium iron phosphate battery material preparation methods, it is difficult to achieve low cost and high quality at the same time, and impurities are difficult to remove, affecting the material performance.
Additives such as hydroxyethylene diphosphonic acid (HEDP) are used to react with impurity ions in low-quality phosphate and ferrous sulfate, and battery-grade iron phosphate is prepared through microwave heating technology, and then mixed and calcined with lithium and carbon sources. Lithium Iron Phosphate.
It effectively reduces the entry of impurity elements into the material lattice, improves product purity and electrochemical performance, reduces the amount of washing water, reduces production costs, and increases the material's packing density and usage range.
Smart Images

Figure CN116281915B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of preparation of lithium-ion battery positive electrode materials iron phosphate and lithium iron phosphate, and specifically relates to a preparation method of battery-grade precursor iron phosphate and battery material lithium iron phosphate. Background Art
[0002] As a key industry for national development, the new energy vehicle industry has achieved tremendous development in recent years. As a key component of electric vehicles, batteries have also become the direction for various companies to compete for layout. With the development of the electric vehicle market, higher and higher requirements are placed on the electrochemical performance and safety performance of batteries. Lithium iron phosphate batteries occupy most of the market for electric vehicle battery materials with their advantages of high energy density and high safety. As the market's requirements for material quality become higher and higher, the development of high-quality iron phosphate electrode materials will have a strong market development prospect. In addition, the country has reduced subsidies for new energy vehicles year by year in recent years. The development of lower-cost raw materials and preparation methods will reduce the cost of the entire industrial chain and further enhance product competitiveness.
[0003] There are many methods for preparing lithium iron phosphate, depending on the different synthetic raw materials, such as hydrothermal process route, ferrous oxalate process route, iron oxide process route and iron phosphate process route. Among the above methods, the preparation of lithium iron phosphate by iron phosphate process has gradually developed into the mainstream process due to its simple synthesis process, high raw material utilization rate, good repeatability, high activity of positive electrode materials and increasingly mature and stable production technology.
[0004] With the rise of the ammonium method for preparing ferric phosphate and its continuous upgrading and improvement, the prepared products have become more and more stable and have gradually become the mainstream process in the market. However, there is still room for improvement. The main materials required for its preparation method are ferrous sulfate and phosphate. The raw materials used in the existing preparation methods are mainly high-purity ferrous sulfate crystals, food phosphoric acid, etc. The impurity content of the ferric phosphate prepared by them is controllable, but the production cost is high. Some patents introduce the preparation of ferric phosphate directly by processing phosphate ore. Although this method can reduce costs to a certain extent, this method requires the use of concentrates, which is greatly affected by the quality of phosphate ore, and impurities are difficult to remove in the later stage; in addition, the reaction of product generation in the liquid phase reaction is a process of liquid phase nucleation followed by crystal nucleus growth. The particles generated by the entire reaction system are large, which is difficult to handle in the later stage. The products produced by these methods have extremely limited scope of use. Summary of the invention
[0005] The present invention is mainly based on the problem that low cost and high quality of the product cannot be met at the same time in the process of preparing iron phosphate, and provides a method for preparing battery-grade iron phosphate by using additives to stabilize impurity ions in low-quality phosphate and ferrous sulfate. The iron phosphate prepared by the method is used as a precursor, and is mixed with a lithium source and a carbon source and calcined to prepare battery-grade lithium iron phosphate.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides a method for preparing low-cost battery-grade iron phosphate and lithium iron phosphate, and the preparation method comprises the following steps:
[0007] (1) adding water to ferrous sulfate and stirring to dilute it as a base solution, adding an additive and an oxidant to a phosphate solution in sequence and mixing them evenly, adding the mixed solution to the base solution to form a phosphate mixed solution, heating the phosphate mixed solution to react, and filtering and washing the product after the reaction is completed;
[0008] (2) adding water and phosphoric acid to the washed filter cake for slurrying, heating the filter cake for crystallization reaction, and heating the filter cake for reaction to obtain a slurry;
[0009] (3) filtering, washing, drying, crushing and calcining the slurry obtained in step (2) to obtain battery-grade iron phosphate, i.e., anhydrous iron phosphate product.
[0010] The additive in the reaction process is one of aminotrimethylenephosphonic acid (ATMP): [CH2PO(OH)2]3N, ethylenediaminetetramethylenephosphonic acid (EDTMP), ethylenediaminetetraacetic acid (EDTA), and hydroxyethylidene diphosphonic acid (HEDP), and hydroxyethylidene diphosphonic acid (HEDP) is most preferred, and the addition amount is about 0.1wt%-3.0wt% of the mass of the whole system.
[0011] HEDP, as an additive, can dissociate in aqueous solution, and one molecule can dissociate into up to 5 positive and negative ions. HEDP has strong chelating properties for metals and can chelate with Mg, Ca, Zn, Co, Ni, Pb, Sn, Sb, etc. After chelating with metal ions, the chelating agent will stably exist in the solution system, thereby greatly reducing the entry of impurity element ions into the material lattice.
[0012] The phosphate includes one or more of monoammonium phosphate, potassium dihydrogen phosphate, sodium dihydrogen phosphate, ammonium dihydrogen phosphate and low-quality calcium dihydrogen phosphate; and the effective phosphorus content in the phosphate solution is greater than 10wt%, and the pH of the phosphate is 2.0-8.0. The technical scheme of the present invention can not only realize the reaction with high-quality phosphate raw materials, but also realize the reaction with low-quality phosphate raw materials. The high-quality phosphate raw material refers to a phosphate with a phosphate content greater than 30wt%, more preferably a phosphate with a phosphate content greater than 50wt%, more preferably a phosphate with a phosphate content greater than 80wt%, and more preferably a phosphate with a phosphate content greater than 90wt%.
[0013] In addition, the phosphates of the present application also include low-quality phosphates, i.e., products with an effective phosphorus content of 10-20 wt%. Due to the different preparation methods used for phosphates, the content of impurity elements will vary greatly, especially cheap phosphorus sources, such as agricultural monoammonium phosphate and phosphates prepared from low-quality acids, which contain high levels of metal impurity elements, as shown in Table 1.
[0014] Table 1 Comparison table of impurity content of low-quality phosphorus sources
[0015]
[0016]
[0017] The molar ratio of the ferrous sulfate, phosphate and oxidant in step (1) is 1:1-2:2-5; the concentration of the ferrous sulfate solution is 1.0-2.0 mol / L, and the oxidant includes any one of oxygen, ozone, perchloric acid or hydrogen peroxide.
[0018] In the step (1), the pH value of the phosphate mixed solution is adjusted to a range of 1.5-3.0 during the temperature reaction, and the pH adjuster is a phosphoric acid solution.
[0019] The oxidant includes one of oxygen, ozone, perchloric acid and hydrogen peroxide, and the molar ratio of the oxidant to the ferrous sulfate solution is 2-5:1. The oxidant is mainly a substance with strong oxidizing properties under acidic conditions, which can 2+ Completely oxidized to Fe 3+ .
[0020] According to the solubility product theory and the calculation of the equilibrium constants of phosphate ionization at each level, the precipitation of hydrated iron phosphate depends on the concentration of H2PO4 - Concentration and Fe 3+ concentration, the lower the pH, the more ionized H2PO4 - The lower the concentration, the more the generated hydrated iron phosphate will dissolve in the phosphoric acid, which can hardly promote the reaction. In this process, when the pH value is lower than 1.5, the yield of the product can only reach about 90%, which greatly wastes the raw materials and also makes the water treatment at the back end very difficult. When the pH is too high, Fe 3+ It will hydrolyze to generate a large amount of iron hydroxide wrapped inside the hydrated iron phosphate, which is difficult to convert through reaction. At the same time, some impurities are easy to react and precipitate at high pH, resulting in low product purity. Therefore, the maximum pH is often controlled below 2.5.
[0021] In the step (1), the phosphate mixed solution is reacted at 30-50° C., and during the reaction, the heating reaction method is selected from microwave heating, steam heating or thermal oil heating.
[0022] Microwave heating is used during the reaction process, the microwave operating frequency is controlled at 3.5 GHz ± 25 MHz, and the microwave power is controlled between 100 and 5000 W. In a preferred embodiment, the microwave power is controlled to be 3000-5000 W.
[0023] The microwave power source: a microwave magnetron is used as the power source, the frequency is: 3.5GHz±25MHz, the working power is controlled at 100~5000W, the whole device is equipped with multiple microwave power sources, which are distributed in the front, back, left and right positions of the reactor, covering the entire reaction area of the reactor. The microwave output power, working time, and system temperature are controlled by a microwave controller. The built-in program heating system and feedback adjustment system can control the reaction temperature deviation at about ±2℃.
[0024] Microwaves are a type of electromagnetic waves that are absorptive and penetrating. After absorbing microwaves, liquid molecules change direction as the positive and negative polarities of the microwave energy field continuously change, thereby increasing the degree of ionization and ion activity of the liquid molecules. The mutual friction and stirring between liquid molecules will produce microwave "thermal effect" and "non-thermal effect", affecting the crystallization process of the reaction products, accelerating the diffusion rate of the reaction products to the liquid phase, and increasing the contact probability between liquid molecules.
[0025] Microwave frequency plays a key role in the reaction. Under certain conditions, microwaves can accelerate the reaction rate and increase the conductivity of the liquid phase of the reaction system. The greater the microwave power, the more energy absorbed by water molecules, the more water molecules dissociate, the more significant the polarization of water molecules, and the conductivity increases accordingly. After water is treated with microwaves, the degree of association decreases, the number of single-molecule water increases, and the conductivity increases. Moreover, this characteristic can still be maintained for a period of time after the microwave field is removed and the temperature is lowered, becoming an ionic nano-water state, and its diffusion and penetration capabilities will be enhanced, which is conducive to the reaction.
[0026] After microwave treatment, the secondary and tertiary ionization of phosphoric acid is promoted, and the temperature of the reaction materials can be increased. It mainly increases the activity of molecules and the number of freely moving molecules through the action of microwaves, thereby promoting the ionization of phosphoric acid or the interaction of ions in the solution.
[0027] In addition, microwave heating reaction can also accelerate the deposition and precipitation of reaction crystals, and has the effect of refining and homogenizing crystals, but microwave action will not change the crystal system, lattice structure and crystal composition. Crystal size distribution and pore distribution will have a great influence on the packing density. During the nucleation and crystallization process, crystal growth and packing structure will change over time. Under the action of microwaves, the relative change rate of fractal dimension is low, the fractal has a high self-similarity, and its crystal packing structure basically does not change much. However, under the action of heating, the fractal dimension value of particle size decreases and the fractal dimension value of pores increases. The difference in fractal dimension between microwave and heating indicates that under heating conditions, due to the low consistency of the formed crystal size, the crystals are nested with each other, which easily forms a dense crystal packing structure and easily blocks the ion transmission channel. Under the action of microwaves, due to the homogenization of particles, the low porosity caused by the nesting of particles of different particle sizes is avoided. In addition, microwave action also causes the refinement of crystal particles, and the result of crystal refinement may lead to the formation of a denser crystal stacking, thereby improving the packing density of the material.
[0028] The filter cake washed in step (2) is added with water and phosphoric acid to form a slurry with a solid content of 7wt%-12wt%, and the slurry is stirred at 80-100°C for 1-3h at a stirring speed of 100-600r / min.
[0029] The reaction process of the present invention adopts a program feedback control method, the primary reaction temperature is controlled at 30-50°C, that is, the temperature rise reaction of step (1), and the secondary reaction temperature is controlled at 80-100°C, that is, the temperature rise crystallization reaction of step (2). The program heating time of the two reactions is controlled at about 20-30 minutes, and the feedback adjustment method is adopted in the insulation stage, and the reaction speed is 100-600r / min. The primary reaction time is controlled at 0.5-1h, and the secondary reaction time is to continue the insulation reaction for 1-3h after the slurry changes color.
[0030] The primary reaction temperature is controlled between 30 and 50°C. On the one hand, it avoids the slow reaction rate caused by too low temperature, which results in incomplete product reaction; on the other hand, it avoids the impurities generated by too high temperature from being wrapped in the product and difficult to wash out, and also reduces the amount of washing water. The secondary reaction controls the reaction time and temperature in order to fully transform the iron-containing impurity phase generated by the primary reaction.
[0031] The product after the reaction is completed is filtered and washed until the conductivity is sufficiently low, such as less than 10 mS / cm, or less than 5 mS / cm, or less than 1 mS / cm. The filtering and washing are conventional operations in the art. After washing, it is flash dried at 90-100° C. and calcined at 450-600° C. to obtain anhydrous iron phosphate.
[0032] Another technical solution of the present invention is to uniformly mix the obtained anhydrous iron phosphate, lithium carbonate and glucose in water, and then perform ball milling, sand milling, spray drying and calcination in sequence to obtain lithium iron phosphate.
[0033] The molar ratio of the iron source (anhydrous ferric phosphate): lithium source (lithium carbonate) is 1:1-1.2, the mass percentage of the carbon source (glucose): ferric phosphate and lithium carbonate is 10-30%, the solvent is water, the ground sample is spray dried, the wind speed is set to 10-30 m / s, the inlet temperature is set to 80-150° C., the outlet temperature is set to 60-100° C., the calcination gas uses high-purity nitrogen or argon, the heating rate is 5-10° C. / min, the calcination temperature is 600-800° C., and the calcination time is 4-6 hours.
[0034] Compared with the prior art, the present invention has the following beneficial effects:
[0035] 1. The additives used in the present invention can complex the impurity metal ions in the reaction solution and can exist stably in the solution, preventing them from being incorporated into the material lattice during the reaction process, thereby affecting the performance of the material. At the same time, the complexed metal ions will not participate in the reaction to generate precipitation during the reaction process, and can be easily filtered out and washed away directly during the washing process, thereby greatly reducing the amount of washing water used and improving the quality of the product;
[0036] 2. The present invention adopts a microwave heating reaction device, which uses high-power microwaves for heating, greatly improving the reaction rate and reducing the heating time. In addition, microwave heating can accelerate the deposition and precipitation of reaction crystals, and has the effect of refining and homogenizing crystals, but the microwave effect will not change the crystal system, lattice structure and crystal composition, so the product particles are small, the particle size distribution is uniform and the morphology is regular;
[0037] 3. The iron phosphate prepared as above is used as a precursor and mixed with a lithium source and a carbon source to prepare lithium iron phosphate, which has excellent electrochemical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] In order to more clearly illustrate the specific embodiment method of the present invention or the technical solution in the prior art, the following is a brief introduction to the drawings required for use in the specific implementation methods or the description of the prior art. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0039] Figure 1 The present invention provides a simplified process flow diagram of the ferric phosphate production process.
[0040] Figure 2 This is the XRD diagram of iron phosphate in Example 1 of the present invention.
[0041] Figure 3 It is the SEM picture of the iron phosphate of comparative example 1 and example 1 of the present invention.
[0042] Figure 4 The SEM images of lithium iron phosphate prepared using the iron phosphate of Comparative Example 1 and Example 1 as precursors.
[0043] Figure 5 The charge and discharge curves of lithium iron phosphate prepared using the iron phosphate of Comparative Example 1 and Example 1 as precursors. Specific embodiments
[0044] The technical scheme of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments, but it will be understood by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0045] like Figure 1 As shown, the present invention provides a method for preparing battery-grade iron phosphate, wherein the iron source in the preparation method is a ferrous sulfate solution of a byproduct of titanium dioxide after impurities are removed, and water is added to adjust the concentration to the required range. The phosphorus source is sequentially added to the additive and the oxidant and mixed evenly before use. Then, a continuous microwave heating reaction is carried out in a microwave reaction device, and the obtained product is filtered and washed after the reaction is completed; the washed filter cake is added with water and phosphoric acid for pulping, and the temperature is quickly raised to the reaction temperature through continuous microwave heating reaction, and the reaction is terminated after a period of insulation. Finally, the finished anhydrous iron phosphate is obtained after filtering, washing, drying, and calcining in sequence.
[0046] The process of preparing ferric phosphate by using the above-mentioned iron source and phosphorus source is as described in the following embodiment:
[0047] Example 1
[0048] A1: Take ferrous sulfate solution and add water to adjust the concentration to 1.2 mol / L. Take agricultural monoammonium solution with a molar ratio of iron source to phosphorus source of 1:1.2, adjust the pH to about 5 with ammonia water, collect the filtrate by filtration, add hydroxyethylidene diphosphonic acid (HEDP) with a mass fraction of 1.0wt% of the total mass of the reactants, stir to form a phosphate mixture, add hydrogen peroxide solution with a molar ratio of oxidant to iron source of 2:1;
[0049] A2: Turn on the microwave heater and control its power to 2.0 kW. Stir the phosphate mixture evenly and then add it to the reactor using a nozzle. Adjust the pH value of the reaction to about 2.0 by controlling the feeding rate of the phosphoric acid solution. Stir while adding the material at a stirring rate of 400 r / min. After the addition is completed, control the reaction temperature to 45°C and continue the reaction for 1.0 h.
[0050] A3: The slurry after the reaction is filtered and washed until the conductivity is lower than 8.0mS / cm. The washing water is treated by the water treatment system and then reused; then the filter cake is slurried with water and phosphoric acid, the solid content of the slurry is controlled at 9.0wt%, the reaction pH is controlled at about 1.8, and the temperature is continued to rise to 90°C for crystallization reaction, and then the reaction is terminated after constant temperature reaction for 90 minutes.
[0051] A4: Filter the slurry after the reaction is completed and wash it until the conductivity is lower than 1.0mS / cm. The washing water is treated by the MVR system and then reused;
[0052] A5: Take the clean filter cake and dry it in a flash dryer. The air inlet temperature is set to 150°C and the air outlet temperature is set to 110°C. The powder collected after the flash evaporation is ferric phosphate dihydrate.
[0053] A6: After the dry material is filled into the sagger, it is calcined. The calcination temperature is set to 600°C and the calcination time is set to 4.0h. After the calcination, nano anhydrous ferric phosphate can be obtained. The dehydration rate of the product after drying is about 19.3%.
[0054] Embodiment 2-5
[0055] In Examples 2-5, the type of additive in the A1 reaction step is changed, and the other conditions are consistent with those in Example 1, wherein the additive in Example 2 is ethylenediaminetetramethylenephosphonic acid (EDTMP), the additive in Example 3 is aminotrimethylenephosphonic acid (ATMP): [CH2PO(OH)2]3N, the additive in Example 4 is ethylenediaminetetraacetic acid (EDTA), and no additive is added in Example 5, thereby preparing a ferric phosphate product.
[0056] Embodiment 6-10
[0057] Examples 6-10 are for changing the mass content of the additive in the A2 reaction step, and the other conditions are consistent with Example 1, wherein the content of the additive hydroxyethylidene diphosphonic acid (HEDP) in Example 6 is 0.1%, the content of the additive hydroxyethylidene diphosphonic acid (HEDP) in Example 7 is 0.5%, the content of the additive hydroxyethylidene diphosphonic acid (HEDP) in Example 8 is 1.5%, the content of the additive hydroxyethylidene diphosphonic acid (HEDP) in Example 9 is 2.0%, and the content of the additive hydroxyethylidene diphosphonic acid (HEDP) in Example 10 is 3.0%, thereby preparing a ferric phosphate product.
[0058] Examples 11-15
[0059] Examples 11-15 are for changing the power of the microwave heating reaction in the A2 reaction step, and the other conditions are consistent with Example 1, wherein the power of the microwave heating reaction in Example 11 is 0.5 kW, the power of the microwave heating reaction in Example 12 is 1.0 kW, the power of the microwave heating reaction in Example 13 is 3.0 kW, the power of the microwave heating reaction in Example 14 is 4.0 kW, and the power of the microwave heating reaction in Example 15 is 5.0 kW, thereby preparing an iron phosphate product.
[0060] Examples 16-17
[0061] Examples 16-17 change the heating method in the A2 reaction step, and the other conditions are consistent with Example 1, wherein the heating method in Example 1 is replaced with steam heating, and the heating method in Example 2 is replaced with thermal oil heating, and the other conditions are consistent with Example 1, thereby preparing an iron phosphate product.
[0062] A method for preparing lithium iron phosphate
[0063] S1: Take the iron phosphate product, lithium carbonate and glucose in Example 1-17, according to the molar ratio of iron source: lithium source = 1:1.03, the carbon source: precursor with a mass percentage of 27% of iron phosphate and lithium carbonate, and the solvent is water, mix them evenly and grind them in a sand mill for 20 minutes;
[0064] S2: The ground sample was spray dried with the wind speed set to 20 m / s, the inlet temperature set to 120 °C, and the outlet temperature set to 80 °C to prepare a precursor mixed sample;
[0065] S3: Calcine the precursor mixed sample in an argon atmosphere furnace. Before heating, introduce inert gas to exhaust the air. Then increase the temperature to 680°C at a heating rate of 5°C / min. After calcining for 5 hours, the reaction is terminated. After cooling the sample to room temperature, it is crushed and sieved to obtain a lithium iron phosphate sample.
[0066] Main index test methods
[0067] In the iron-phosphorus ratio test method, the determination of iron content adopts chemical titration method, and the determination of phosphorus content adopts weight method; the element content test uses inductively coupled plasma emission spectrometer for analysis, and its working principle is to analyze the element to be tested according to the characteristic spectral lines emitted when the atoms of the element to be tested in the excited state return to the ground state, so as to qualitatively and quantitatively analyze the trace metal elements. The charge and discharge test is carried out by Xinwei electrochemical workstation. The specific method is to connect the battery to the tester, and set the current size required for the relevant experiment. In this paper, the charge and discharge current of 0.1C is used for testing (1C = 170mAh / g), and the voltage range setting is set on the microcomputer through the relevant software. This paper uses the voltage range of 2-3.75V for testing. The charging or discharging stage of the battery is controlled by the microcomputer program, and the charging and discharging is carried out in a constant current and constant voltage manner.
[0068] Table 2 Comparison of process conditions and indicators of the examples and comparative examples
[0069]
[0070]
Claims
1. A method for preparing battery-grade iron phosphate, characterized in that: The preparation method is as follows: (1) Add water to ferrous sulfate and stir to dilute it as a base solution, add an additive and an oxidant to the phosphate solution in sequence and mix them evenly, add the mixed solution to the base solution to form a phosphate mixed solution, turn on the microwave heater, control its power to 2.0 kW, 3.0 kW or 4.0 kW, stir the phosphate mixed solution evenly and then add it to the reactor through a nozzle, adjust the pH value of the reaction to 2.0 by controlling the feeding rate of the phosphoric acid solution, stir while adding, and the stirring speed is 400 r / min. After the addition is completed, the reaction temperature is controlled to 45°C, and the reaction is continued for 1.0 h; the product after the reaction is completed is filtered and washed, the additive is hydroxyethylidene diphosphonic acid HEDP, and the added mass fraction of hydroxyethylidene diphosphonic acid is 1.0 wt% of the total mass of the reactants; (2) adding water and phosphoric acid to the washed filter cake for slurrying, heating it for crystallization reaction, and obtaining slurry after the temperature reaction; (3) The slurry obtained in step (2) is filtered, washed, dried, crushed, and calcined to obtain battery-grade anhydrous iron phosphate.
2. The method for preparing battery-grade iron phosphate according to claim 1, characterized in that: The phosphate solution includes one or more of monoammonium phosphate, potassium dihydrogen phosphate, sodium dihydrogen phosphate, ammonium dihydrogen phosphate or calcium dihydrogen phosphate, and the effective phosphorus content in the phosphate solution is greater than 10 wt%, and the pH of the phosphate is between 2-8.
3. The method for preparing battery-grade iron phosphate according to claim 1, characterized in that: In the step (1), the molar ratio of ferrous sulfate, phosphate and oxidant is 1:1-2:2-5; the oxidant includes any one of oxygen, ozone, perchloric acid or hydrogen peroxide.
4. The method for preparing battery-grade iron phosphate according to claim 1, characterized in that: In the step (1), the pH regulator is a phosphoric acid solution.
5. The method for preparing battery-grade iron phosphate according to claim 4, characterized in that: Water and phosphoric acid are added to the washed filter cake to form a slurry with a solid content of 7.0 wt%-12 wt%, and the mixture is stirred at 80-100 °C for 1.0-3.0 h at a stirring speed of 100-600 r / min.
6. The method for preparing battery-grade iron phosphate according to claim 5, characterized in that: In step (3), the drying temperature is 90-100°C; and the calcination temperature is 450-600°C.
7. A method for preparing lithium iron phosphate, comprising mixing anhydrous iron phosphate prepared by the method according to any one of claims 1 to 6 with lithium carbonate and glucose in water, and then subjecting the mixture to ball milling, sand milling, spray drying and calcination to obtain lithium iron phosphate.
8. The method for preparing lithium iron phosphate according to claim 7, characterized in that: The molar ratio of anhydrous ferric phosphate: lithium carbonate is 1:1~1.2, the mass percentage of glucose: ferric phosphate and lithium carbonate is 10~30%, the ground sample is spray dried, the wind speed is set to 10~30 m / s, the inlet temperature is set to 80~150 ℃, the outlet temperature is set to 60~100 ℃, the calcination gas is high-purity nitrogen or argon, the heating rate is 5~10 ℃ / min, the calcination temperature is 600~800 ℃, and the calcination time is 4~6h.
Citation Information
Patent Citations
Pressure-controlling deaggregating synthetic method for lithium iron phosphate positive electrode material
CN105322167A
Method for synthesizing ferric phosphate by utilizing waste phosphate generated by precipitation of trace heavy metal
CN109809382A
Preparation method of battery-grade anhydrous iron phosphate
CN110482514A
Preparation method of low-cost lithium iron phosphate
CN110482515A
Nano lithium iron phosphate and preparation method thereof
CN111348637A