A high viscosity cement paste and preparation method thereof

By adjusting the ratio of cement to water and introducing CO2 gas reaction, the problem of insufficient viscosity of traditional cement slurry is solved, and the preparation of high-viscosity cement slurry is realized, which is suitable for high-demand engineering fields.

CN116283154BActive Publication Date: 2024-11-22TONGJI UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310338189.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-11-22
Estimated Expiration
2043-03-31

AI Technical Summary

Technical Problem

The viscosity of traditional cement slurry is difficult to meet the construction requirements in the fields of spraying and 3D printing, and it cannot effectively improve the viscosity.

Method used

By adjusting the ratio of cement to water, and introducing high-purity CO2 gas during the stirring process, the reaction between cement and CO2 is promoted to generate CaCO3, thereby increasing the viscosity of the cement slurry.

Benefits of technology

It effectively improves the viscosity of cement slurry, meets the needs of high viscosity, simplifies the preparation process, and is suitable for fields such as spraying and 3D printing.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to a high-viscosity cement paste and a preparation method thereof, wherein the preparation method comprises the following steps: S1, mixing a part of the cement component with water, standing, and mixing again to obtain a cement mixture; S2, introducing CO2 into the cement mixture obtained in step S1, and then adding the remaining part of the cement component, and mixing to obtain cement paste. Compared with the prior art, the preparation method of the present invention is simple, effectively improves the viscosity of the cement paste, and is expected to be widely used in fields with special requirements for the viscosity of cement paste, such as spraying, 3D printing construction, etc.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cement-based materials, and in particular to a high-viscosity cement slurry and a preparation method thereof. Background Art

[0002] Cement-based materials are one of the most widely used man-made materials in the world today, especially in the engineering field. With the development of the times, more and more difficult projects have become a reality, and new technologies have begun to be applied in the engineering field, which puts higher requirements on engineering materials. In the fields of shotcrete, 3D printing construction, etc., there are special requirements for the viscosity of cement materials, and the viscosity of traditional cement slurry materials is difficult to meet the construction requirements. Therefore, there is an urgent need for a method for improving the viscosity of traditional cement slurry and the prepared cement slurry for application in production and life. Summary of the invention

[0003] The purpose of the present invention is to provide a high-viscosity cement slurry and a preparation method thereof in order to overcome the defects of the prior art such as low viscosity of the cement slurry.

[0004] The purpose of the present invention can be achieved by the following technical solutions:

[0005] The technical solution of the present invention is to provide a method for preparing high-viscosity cement slurry, comprising the following steps:

[0006] S1, mixing a part of the cement component with water, letting it stand, and mixing it again to obtain a cement mixture;

[0007] S2. CO2 is introduced into the cement mixture obtained in step S1, and then the remaining cement components are added, and the mixture is stirred and mixed to obtain cement paste.

[0008] Furthermore, the mass ratio of water to cement component is 0.2-0.8:1.

[0009] Furthermore, in step S1, 1 / 3-2 / 3 of the cement component is stirred and mixed with water.

[0010] Furthermore, in step S1, the standing time is 18-22 minutes.

[0011] Furthermore, in step S2, the purity of the introduced CO2 is 99.99%.

[0012] Furthermore, in step S2, the ratio of the amount of CO2 introduced to the total mixture of cement components and water is 1L:8-12g.

[0013] Furthermore, in step S2, the maximum flow rate when CO2 is introduced is 2.5 L / min.

[0014] Furthermore, in step S2, aggregates and admixtures may be added, and the aggregates may be selected from any one or more of sand, gravel or fiber.

[0015] Furthermore, the mass ratio of the aggregate, admixture, cement component and water is 0-x:0-y:1, where x and y are any natural numbers greater than 0.

[0016] Aggregates and admixtures are conventionally designed components and amounts in the art, and do not serve as components that affect the innovation of the present invention. When the mass ratio of aggregate to the total mixture of cement component and water is 0:1, it indicates that no aggregate is added to the total mixture of cement component and water; when the mass ratio of admixture to the total mixture of cement component and water is 0:1, it indicates that no admixture is added to the total mixture of cement component and water.

[0017] A second technical solution of the present invention is to provide a high-viscosity cement slurry based on the preparation method as described in one of the above technical solutions.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] (1) The present invention effectively improves the viscosity of cement paste by adjusting the ratio of cement material to water and introducing CO2 for reaction. The main components of cement are limestone, clay, and iron ore powder. CO2 can react with CaO in cement paste, as well as hydrated calcium silicate gel and calcium hydroxide generated by cement hydration reaction to generate CaCO3. As the water-cement ratio increases, the proportion of free water in cement paste increases, the fluidity of cement paste increases, and the viscosity decreases. As the water-cement ratio decreases, the proportion of free water in cement paste decreases, the fluidity of cement paste decreases, and the viscosity increases.

[0020] (2) The preparation method of the present invention is simple and effective, and is expected to be widely used in fields such as spraying and 3D printing construction that have special requirements on the viscosity of cement slurry. DETAILED DESCRIPTION

[0021] The present invention is described in detail below with reference to specific embodiments.

[0022] In the following examples and comparative examples, unless otherwise specified, raw materials or processing techniques are conventional commercially available raw materials or conventional processing techniques in the art.

[0023] Embodiment 1:

[0024] 400 g of PO32.5 cement and 160 g of water were used to prepare cement paste with a water-cement ratio of 0.4:1.

[0025] (1) First, mix 200g of cement with 160g of water and stir thoroughly to completely dissolve the cement.

[0026] (2) Let the above cement mixture stand for 20 minutes.

[0027] (3) The cement mixture was stirred again after standing. After stirring for 30 seconds, 99.99% pure CO2 was introduced to complete the reaction. The CO2 gas was introduced for 20 minutes at a flow rate of 2.5 L / min.

[0028] (4) Add the remaining 200 g of cement to the mixture in step (3) and stir thoroughly to obtain cement slurry.

[0029] Embodiment 2:

[0030] 350 g of PO32.5 cement and 210 g of water were used to prepare cement paste with a water-cement ratio of 0.6:1.

[0031] (1) First, mix 175g of cement with 210g of water and stir thoroughly to completely dissolve the cement powder.

[0032] (2) Let the above cement mixture stand for 20 minutes.

[0033] (3) The cement mixture was stirred again after standing. After stirring for 30 seconds, 99.99% pure CO2 was introduced to complete the reaction. The CO2 gas was introduced for 20 minutes at a flow rate of 2.5 L / min.

[0034] (4) Add the remaining 175 g of cement to the mixture in step (3) and stir thoroughly to obtain the desired cement slurry.

[0035] Comparative Example 1:

[0036] Compared with Example 1, most of the steps are the same except that the CO2 injection is omitted.

[0037] The specific steps are as follows:

[0038] 400 g of PO32.5 cement and 160 g of water were used to prepare cement paste with a water-cement ratio of 0.4:1.

[0039] (1) First, mix 200g of cement with 160g of water and stir thoroughly to completely dissolve the cement powder.

[0040] (2) Let the above cement mixture stand for 20 minutes.

[0041] (3) Stir the cement mixture again after it has been allowed to stand for 30 seconds and then allow it to stand for 20 minutes.

[0042] (4) Add the remaining 200 g of cement to the mixture in step (3) and stir thoroughly to obtain the desired cement slurry.

[0043] Comparative Example 2:

[0044] Compared with Example 2, most of the steps are the same except that the CO2 injection is omitted.

[0045] The specific steps are as follows:

[0046] 350 g of PO32.5 cement and 210 g of water were used to prepare cement paste with a water-cement ratio of 0.6:1.

[0047] (1) First, mix 175g of cement with 210g of water and stir thoroughly to completely dissolve the cement powder.

[0048] (2) Let the above cement mixture stand for 20 minutes.

[0049] (3) Stir the cement mixture again after it has been allowed to stand for 30 seconds and then allow it to stand for 20 minutes.

[0050] (4) Add the remaining 175 g of cement to the mixture in step (3) and stir thoroughly to obtain the desired cement slurry.

[0051] The viscosity of the cement pastes obtained in Example 1, Example 2, Comparative Example 1, and Comparative Example 2 was tested. The test instrument was an MCR rheometer from Anton Paar, and the test shear rate was 1000 s -1 , take 10g of cement paste sample. The test is carried out within 43-45 minutes after the cement and water are mixed.

[0052] The test results are shown in Table 1. In Example 1 and Comparative Example 1 with a water-cement ratio of 0.4, the viscosity of the cement slurry in Example 1 with CO2 introduced is 99.76% higher than that in Comparative Example 1 without CO2 introduced. In Example 2 and Comparative Example 2 with a water-cement ratio of 0.6, the viscosity of the cement slurry in Example 2 with CO2 introduced is 299.83% higher than that in Comparative Example 2 without CO2 introduced. It can be seen that the method of the present invention can effectively improve the viscosity of cement slurry.

[0053] Table 1 Cement paste viscosity test results

[0054] Example 1 Example 2 Comparative Example 1 Comparative Example 2 Viscosity (mPa·s) 399.67 168.93 200.05 42.25

[0055] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. A method for preparing a high-viscosity cement slurry, characterized in that: The steps include: S1, mixing a part of the cement component with water, letting it stand, and mixing it again to obtain a cement mixture; S2, introducing CO2 into the cement mixture obtained in step S1, then adding the remaining part of the cement components, stirring and mixing to obtain cement slurry; In step S2, the ratio of the amount of CO2 introduced to the total mixture of cement components and water is 1L:8-12g; The maximum flow rate when CO2 is introduced is 2.5L / min.

2. The method for preparing a high-viscosity cement slurry according to claim 1, characterized in that: The mass ratio of water to cement components is 0.2-0.8:

1.

3. The method for preparing a high-viscosity cement slurry according to claim 1, characterized in that: In step S1, 1 / 3-2 / 3 of the cement component is stirred and mixed with water.

4. The method for preparing a high-viscosity cement slurry according to claim 1, characterized in that: In step S1, the standing time is 18-22 minutes.

5. The method for preparing a high-viscosity cement slurry according to claim 1, characterized in that: In step S2, the purity of the introduced CO2 is 99.99%.

6. The method for preparing a high-viscosity cement slurry according to claim 1, characterized in that: In step S2, aggregates and admixtures may also be added, wherein the aggregates are selected from any one or more of sand, gravel or fiber.

7. The method for preparing a high-viscosity cement slurry according to claim 6, characterized in that: The mass ratio of the total mixture of aggregate, admixture, cement component and water is 0-x:0-y:1, where x and y are any natural numbers greater than 0.

8. A high viscosity cement paste, characterized in that: Based on the preparation method according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Method for improving efficiency of absorbing CO2 by newly-stirred concrete

    CN109368642A

  • Preparation method of carbon dioxide premixed cement-based composite material

    CN113816767A

  • Method for preparing cement-based material from carbonized steel slag slurry

    CN114538867A