Method for preparing phenolic lignin by transesterification reaction of lignin and dihydrocoumarin

Through the transesterification reaction of lignin and dihydrocoumarin, phenolic lignin with high solubility, antioxidant and ultraviolet resistance was prepared, which solved the problems of high temperature, high pressure and high cost in the existing technology, and realized the Possibility of industrialization implementation and widespread application.

CN116284839BActive Publication Date: 2024-12-03GUIZHOU UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310056619.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-16
Publication Date
2024-12-03
Estimated Expiration
2043-01-16

AI Technical Summary

Technical Problem

The existing lignin phenolization methods have problems such as high temperature and high pressure conditions that are not conducive to industrial production, mild reaction conditions but high cost, and the application range of phenolic lignin is limited.

Method used

The phenolic lignin is prepared by transesterification reaction with dihydrocoumarin, and the lignin is dissolved and activated by organic alkali and organic solvent system, and the transesterification reaction under mild conditions is carried out. The process is simple and cheap, and it uses low-grade fats. Purification by alcohol or water.

Benefits of technology

It reduces the preparation cost of phenolic lignin, improves its solubility, antioxidant and ultraviolet resistance, expands the functionalization and high-value utilization of lignin, and is suitable for biomedicine, environmental protection and packaging materials and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116284839B_ABST
    Figure CN116284839B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing phenolic lignin by transesterification reaction of lignin and dihydrocoumarin, comprising the following steps: (1) mixing lignin, an organic base, dihydrocoumarin and an organic solvent, reacting in a reactor at a temperature of 80-140°C for 0.5-24 hours to obtain a crude phenolic lignin solution; (2) adding C1-C4 lower aliphatic alcohol or water to the phenolic lignin solution, filtering the mixed solution, washing and purifying the filtered solid mixture with C1-C4 lower aliphatic alcohol or water, and drying to obtain phenolic lignin. The reaction conditions of the preparation process of the present invention are mild, and the process is simple, with the characteristics of low cost, which is conducive to industrial implementation; at the same time, the phenolic lignin obtained by the process of the present invention has a novel structure, which is of great significance for expanding the functionalization and high-value utilization of lignin; in addition, the phenolic lignin of the present invention also has the characteristics of better solubility, antioxidant and ultraviolet resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing phenolic lignin, in particular to a method for preparing phenolic lignin through transesterification reaction of lignin and dihydrocoumarin. Background Art

[0002] Lignin is the second largest bio-based resource after cellulose, but it is far from being fully utilized. In the black liquor of papermaking and pulping, which is mainly composed of cellulose, lignin is mostly discharged as a waste. According to incomplete statistics, the annual output of lignin is 50 million tons, but only 2% of the lignin is actually used, and more lignin is only used as combustion to provide heat.

[0003] Lignin has a large and complex polymer network structure, including methoxyl groups, phenolic hydroxyl groups, alcoholic hydroxyl groups, and terminal aldehyde groups on some side chains. Unfortunately, due to its aromaticity and highly complex three-dimensional structure, lignin is usually brittle, and has poor compatibility, low dispersion, and poor processability when used directly as a polymer or composite component. It is generally believed that chemical modification of lignin using its structural characteristics can significantly improve the above-mentioned deficiencies, thereby expanding its scope of application. For example, lignin can be modified by alkylation, alkoxylation, nitration, and esterification of hydroxyl, methoxyl, carbonyl, and carboxyl groups without destroying its inherent structure. Materials with great application potential have been obtained in the fields of cosmetics, energy catalysis, surfactants, and enhancers. Among them, the phenolization of lignin has been widely studied in the functionalization of lignin.

[0004] Phenolic lignin can be divided into three main pathways:

[0005] 1. After dissolving lignin in DMF, adding Lewis acid can break the methyl group in the methoxy group on lignin to form phenolic hydroxyl groups to obtain phenolic lignin. The most common of these is halogen acid (ACS Sustainable Chemistry Engineering, 5, 5424).

[0006] 2. In the patent with publication number CN111286041A, alkaline lignin is dissolved under acidic conditions (pH 4.0 or 6.0), and 2,2'-azobis-3-ethylbenzothiazoline-6-sulfonic acid and fungal laccase of Coriolus versicolor are added to obtain phenolic lignin. Secondly, phenol monooxygenase can also phenolate lignin.

[0007] 3. In the patent with publication number CN104004479A, alkali lignin is subjected to electrophilic substitution with α or γ-carbon cations at a relatively low pH value after phenol is dehydrated under strongly acidic conditions, and then grafted onto lignin to form phenolized lignin.

[0008] Among the above strategies for phenolization of lignin, strategies 1 and 3 require high temperature and high pressure, which are not conducive to industrial production and safety. Although the reaction conditions of strategy 2 are relatively mild, the process of extracting enzymes is more complicated and the cost is relatively high. Summary of the invention

[0009] The object of the present invention is to provide a method for preparing phenolic lignin by transesterification reaction of lignin and dihydrocoumarin. The reaction conditions of the preparation process of the present invention are mild, the process is simple, and the cost is low, which is conducive to industrial implementation; at the same time, the phenolic lignin prepared by the process of the present invention has a novel structure, which is of great significance for expanding the functionalization and high-value utilization of lignin; in addition, the phenolic lignin of the present invention also has the characteristics of better solubility, antioxidant and UV resistance.

[0010] The technical solution of the present invention is a method for preparing phenolic lignin by transesterification reaction of lignin and dihydrocoumarin, comprising the following steps:

[0011] (1) mixing lignin, an organic base, dihydrocoumarin and an organic solvent, and reacting them in a reactor at a temperature of 80-140° C. for 0.5-24 hours to obtain a phenolic lignin solution;

[0012] (2) Adding C1-C4 lower aliphatic alcohol or water to the phenolized lignin solution, filtering the mixed solution, washing and purifying the filtered solid mixture with C1-C4 lower aliphatic alcohol or water, and drying to obtain phenolized lignin.

[0013] The preparation method of the aforementioned phenolic lignin, wherein the lignin is one or any combination of alkali lignin, enzymatic lignin, lignin sulfonate, steam explosion lignin or lignin separated from agricultural and forestry lignocellulose waste, and its basic structural unit is as follows:

[0014]

[0015] In the above-mentioned method for preparing phenolic lignin, the mass concentration of lignin in the mixture in step (1) is 1-20wt%, the mass concentration of organic base is 0.5-30wt%, and the rest is organic solvent.

[0016] In the aforementioned method for preparing phenolic lignin, the organic base has the following structural characteristics:

[0017]

[0018] Wherein: R is independently hydrogen, methyl or ethyl; R1 is independently hydrogen or an alkyl group with 1 to 6 carbon atoms; R2, R3, R4 and R5 are independently hydrogen, methyl or ethyl.

[0019] In the above-mentioned method for preparing phenolic lignin, the organic solvent is one or a mixture of two or more of dimethyl sulfoxide, N-methylpyrrolidone, tetramethylguanidine, N,N-dimethylimidazolidinone, N,N-dimethylformamide, N,N-dimethylacetamide, N,N-diethylacetamide, 2-pyrrolidone, 2-azolopyridine, ε-caprolactam, N,N-dimethylpropylene urea, cyclopentane or pentanediol sulfone.

[0020] The above-mentioned method for preparing phenolic lignin has a temperature of 110° C. and a reaction time of 12 hours.

[0021] In the above-mentioned method for preparing phenolic lignin, the molar ratio of dihydrocoumarin to lignin hydroxyl group is 0.5-10:1.

[0022] In the above-mentioned method for preparing phenolic lignin, when adding C1-C4 lower aliphatic alcohol or water to the phenolic lignin solution in step (3), the volume ratio of C1-C4 lower aliphatic alcohol or water to the phenolic lignin solution is 0.5-10:1.

[0023] The above-mentioned method for preparing phenolic lignin, wherein the phenolic lignin has the following structural characteristics:

[0024]

[0025] Beneficial effects of the present invention

[0026] 1. The present invention is based on a system of organic solvents and organic bases to dissolve and activate lignin. At the same time, the organic base is used to open the ring of dihydrocoumarin and prepare phenolic lignin through transesterification reaction. The reaction conditions of the entire process are mild and the process steps are simple, which is very conducive to industrial promotion and implementation.

[0027] 2. The present invention is prepared based on an organic solvent and an organic base system, the reaction reagents are cheap and readily available, the preparation process is simple, and the reaction conditions are mild, thus greatly reducing the preparation cost of phenolic lignin.

[0028] 3. The present invention utilizes lignin and dihydrocoumarin to carry out transesterification reaction to prepare phenolic lignin. The obtained phenolic lignin has a novel structure and is of great significance for expanding the functionalization and high-value utilization of lignin.

[0029] 4. The present invention prepares phenolic lignin by subjecting lignin to a transesterification reaction. Compared with the original lignin, the solubility, antioxidant and UV resistance of the phenolic lignin are greatly improved. At the same time, the phenolic lignin has a lower glass transition temperature, so that it has better processing and dispersion properties in subsequent applications. These characteristics make the product of the present invention have better application prospects in industrial fields such as biomedicine, environmental protection, coatings and packaging materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 is the ATR spectrum of the phenolic lignin of the present invention;

[0031] Figure 2 The phenolic lignin of the present invention 1 H NMR spectrum;

[0032] Figure 3 The phenolic lignin of the present invention 13 C NMR spectrum;

[0033] Figure 4 is a two-dimensional spectrum of phenolic lignin of the present invention;

[0034] Figure 5 The phenolic lignin of the present invention 31 P NMR spectrum

[0035] Figure 6 is the TGA spectrum of the phenolic lignin of the present invention;

[0036] Figure 7 is the DSC spectrum of the phenolic lignin of the present invention;

[0037] Figure 8 is the anti-ultraviolet spectrum of the phenolic lignin of the present invention;

[0038] Fig. 9 is the antioxidant spectrum of the phenolic lignin of the present invention; DETAILED DESCRIPTION

[0039] The present invention will be further described below in conjunction with the embodiments, but they are not intended to limit the present invention.

[0040] Embodiments of the present invention

[0041] It is necessary to explain the phenolic hydroxyl content. 31 The results of P NMR test showed that the phenolic hydroxyl content of the unmodified lignin was 1.732 mmol / g. The unit of phenolic hydroxyl content in this paper is mmol / g.

[0042] The calculation formula of free radical scavenging rate (DPPH Scavenging acitivity) is as follows:

[0043]

[0044] Among them Abs sample , Abs blank and Abs control Represent the absorbance of sample, blank sample and control sample respectively.

[0045] Embodiment 1:

[0046] A method for preparing phenolic lignin by transesterification reaction of lignin and dihydrocoumarin, the steps are as follows:

[0047] (1) mixing alkali lignin, 1,8-diazabicyclo[5.4.0]-7-undecene, dihydrocoumarin and tetramethylguanidine, wherein the mass concentration of alkali lignin is 10wt%, the mass concentration of 1,8-diazabicyclo[5.4.0]-7-undecene is 15wt%, and the rest is tetramethylguanidine, and the molar ratio of dihydrocoumarin to the hydroxyl group on the alkali lignin is 2:1, and the mixture is kept in a nitrogen atmosphere for reaction in a reactor at a temperature of 110° C. for 12 hours to obtain a phenolized lignin solution;

[0048] (2) Add 5 times the amount of C1-C4 lower fatty alcohol to the phenolized lignin solution, filter the mixed solution, wash and purify the filtered solid mixture with C1-C4 lower fatty alcohol, and dry to obtain phenolized lignin.

[0049] Embodiment 2:

[0050] A method for preparing phenolic lignin by transesterification reaction of lignin and dihydrocoumarin, the steps are as follows:

[0051] (1) lignin sulfonate, 1,8-diazabicyclo[5.4.0]-7-undecene, dihydrocoumarin and N,N-diethylacetamide are mixed, wherein the mass concentration of lignin sulfonate is 1wt%, the mass concentration of 1,8-diazabicyclo[5.4.0]-7-undecene is 0.5wt%, and the rest is N,N-diethylacetamide, and the molar ratio of dihydrocoumarin to the hydroxyl group on lignin sulfonate is 0.5:1, and the mixture is kept in a N2 atmosphere for reaction in a reactor at a temperature of 80°C for 24 hours to obtain a phenolized lignin solution;

[0052] (2) Add 0.5 times the amount of C1-C4 lower fatty alcohol to the phenolized lignin solution, filter the mixed solution, wash and purify the filtered solid mixture with C1-C4 lower fatty alcohol, and dry to obtain phenolized lignin.

[0053] Embodiment 3:

[0054] A method for preparing phenolic lignin by transesterification reaction of lignin and dihydrocoumarin, the steps are as follows:

[0055] (1) mixing enzymatic lignin, 1,8-diazabicyclo[5.4.0]-7-undecene, dihydrocoumarin and ε-caprolactam, wherein the mass concentration of the enzymatic lignin is 20wt%, the mass concentration of 1,8-diazabicyclo[5.4.0]-7-undecene is 30wt%, and the rest is ε-caprolactam, and the molar ratio of dihydrocoumarin to the hydroxyl group on the enzymatic lignin is 3:1, and the mixture is kept in a N2 atmosphere for reaction in a reactor at a temperature of 140°C for 0.5 hour to obtain a phenolic lignin solution;

[0056] (2) Add 10 times the amount of C1-C4 water to the phenolated lignin solution, filter the mixed solution, wash and purify the filtered solid mixture with water, and dry it to obtain phenolated lignin.

[0057] Embodiment 4:

[0058] According to the steps of Example 1, 2g of each type of lignin was weighed, and added to the reactor with 0.3164g of 1,8-diazabicyclo[5.4.0]-7-undecene (DBU), 10g of N,N-dimethylformamide (DMF) and 1.0267g of dihydrocoumarin, respectively. The reactor was covered, and N2 was charged and discharged for three cycles, and the air was excluded. Finally, it was stirred for 6 hours in a 0Mpa N2 atmosphere at 120°C. After the reaction, a black homogeneous solution was obtained. 100mL of pure water was used as an anti-solvent to precipitate the solid product, which was washed and filtered 3 times, and the product was obtained after freeze-drying. The products obtained from different lignins in this example were tested, and the relevant results are shown in the following table:

[0059] Table 1 Research on lignin from different sources

[0060] serial number Lignin Phenolic hydroxyl content 1 Alkali lignin 2.78 2 Enzymatic hydrolysis of lignin 3.01 3 Lignin sulfonate 2.56 4 Steam explosion lignin 2.17

[0061] This example fully demonstrates that phenolic lignin products can be prepared from lignin from different sources, which fully demonstrates that this patent is universal with respect to lignin types.

[0062] Embodiment 5:

[0063] According to the steps of Example 1, 2g of enzymatic lignin was weighed, and an organic base of 1,8-diazabicyclo [5.4.0] -7-undecene (DBU), triethylamine (TEA) or 1,5-diazabicyclo [4.3.0] non-5-ene (DBN) was taken, and an organic solvent of dimethyl sulfoxide (DMSO), N,N-dimethylformamide (DMF) or N-methylpyrrolidone (NMP) was taken, and the enzymatic lignin, one of the organic bases and one of the organic solvents were mixed and added to the reactor, and the reactor was covered, and N2 was charged and discharged for three cycles, and the air was excluded. Finally, in a 0Mpa N2 atmosphere, 120°C conditions, stirred for 6 hours to obtain a homogeneous phenolic lignin solution. 100mL of pure water was used as an anti-solvent to precipitate the solid product, washed and filtered 3 times, and freeze-dried to obtain the product. The products obtained with different organic bases and organic solvents in this embodiment were tested, and the relevant results are shown in the following table:

[0064] Table 2 Study on different organic bases and organic solvents for a certain lignin content

[0065]

[0066]

[0067] This example fully demonstrates that phenolic lignin can be prepared with different lignin concentrations, different strong organic bases and their contents, and different organic solvents.

[0068] Embodiment 6:

[0069] According to the steps of Example 1, 2g of enzymatic lignin was weighed and added to the reactor with 0.3164g of 1,8-diazabicyclo[5.4.0]-7-undecene (DBU), 1.0267g of dihydrocoumarin, and 10g of N,N-dimethylformamide (DMF), respectively. The reactor was covered and N2 was charged and discharged for three cycles, and the air was excluded. Finally, the N2 atmosphere was maintained at 80-140°C and stirred for 1-24 hours to obtain a homogeneous phenolic lignin solution. The solid product was precipitated with 100mL of pure water, washed and filtered 3 times, and the product was obtained after freeze-drying. The products obtained at different reaction times and reaction temperatures in this embodiment were tested, and the relevant results are shown in the following table:

[0070] Table 3 Studies on the effects of different reaction times and reaction temperatures

[0071]

[0072]

[0073] This example fully demonstrates that phenolic lignin can be prepared at different reaction times and reaction temperatures.

[0074] Embodiment 7:

[0075] According to the steps of Example 1, 2g of enzymatic lignin was weighed and added to the reactor with 0.3164g of 1,8-diazabicyclo[5.4.0]-7-undecene (DBU) and 10g of N,N-dimethylformamide (DMF), respectively. The reactor was covered and N2 was charged and discharged for three cycles, and the air was excluded. Finally, the N2 atmosphere was maintained at 120°C and stirred for 6 hours to obtain a phenolic lignin solution. The solid product was precipitated using 100mL of different anti-solvents, washed and filtered 3 times, and the product was obtained after freeze-drying. The products obtained by different anti-solvents in this example were tested, and the relevant results are shown in the following table:

[0076] Table 4 Study on the effect of different anti-solvents

[0077] serial number Antisolvent Phenolic hydroxyl content Yield(%) 1 water 3.02 98 2 Methanol 2.34 70 3 Ethanol 2.27 65 4 Isopropyl alcohol 2.48 80 5 Tert-Butanol 2.44 80

[0078] This example fully demonstrates that phenolic lignin can be precipitated with different anti-solvents, and the reproduction rate of the product is relatively high, indicating that different anti-solvents have good effects.

[0079] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical solutions and inventive concepts of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for preparing phenolic lignin by transesterification of lignin and dihydrocoumarin, characterized in that: The steps include: (1) mixing lignin, an organic base, dihydrocoumarin and an organic solvent, and reacting them in a reactor at a temperature of 80-140° C. for 0.5-24 hours to obtain a phenolized lignin reaction crude liquid; (2) adding C1-C4 lower aliphatic alcohol or water to the crude phenolic lignin reaction solution, filtering the mixed solution, washing and purifying the filtered solid mixture with C1-C4 lower aliphatic alcohol or water, and drying to obtain phenolic lignin; The lignin is one or any combination of alkali lignin, enzymatic lignin, lignin sulfonate, steam explosion lignin or lignin separated from agricultural and forestry lignocellulose waste, and its structural formula is as follows: The mass concentration of lignin in the mixture of step (1) is 1-20wt%, the mass concentration of organic base is 0.5-30wt%, and the rest is organic solvent; The organic base has the following structural characteristics: Wherein: R is independently hydrogen, methyl or ethyl; R1 is independently hydrogen or an alkyl group having 1 to 6 carbon atoms; R2, R3, R4 and R5 are independently hydrogen, methyl or ethyl; The phenolic lignin has the following structural characteristics:

2. The method for preparing phenolic lignin by transesterification reaction of lignin and dihydrocoumarin according to claim 1, characterized in that: The organic solvent is one or a mixture of two or more of dimethyl sulfoxide, N-methylpyrrolidone, tetramethylguanidine, N,N-dimethylimidazolidinone, N,N-dimethylformamide, N,N-dimethylacetamide, N,N-diethylacetamide, 2-pyrrolidone, 2-azolopyridine, ε-caprolactam, N,N-dimethylpropylene urea, cyclopentane or pentaerythrityl sulfone.

3. The method for preparing phenolic lignin by transesterification reaction of lignin and dihydrocoumarin according to claim 1, characterized in that: The molar ratio of the dihydrocoumarin to the hydroxyl group on the lignin in the lignin solution is 0.5-3:

1.

4. The method for preparing phenolic lignin by transesterification of lignin and dihydrocoumarin according to claim 1, characterized in that: The reaction temperature of step (1) is 110° C. and the reaction time is 12 hours.

5. The method for preparing phenolic lignin by transesterification reaction of lignin and dihydrocoumarin according to claim 1, characterized in that: When adding C1-C4 lower aliphatic alcohol or water to the phenolated lignin solution in step (2), the volume ratio of C1-C4 lower aliphatic alcohol or water to the phenolated lignin solution is 0.5-10:1.

Citation Information

Patent Citations

  • Phenolate lignin tackiness agent and preparing method of phenolate lignin tackiness agent

    CN104004479A

  • Demethylated lignin, preparation method thereof and application of the demethylated lignin in phenolic resin adhesive