A masterbatch for automobile interior accessories and preparation method thereof

Through the use of modified anti-aging agents, the problem of aging of PC/ABS composites in the light environment is solved, the anti-aging and mechanical properties of the material are improved, and the service life is extended.

CN116285286BActive Publication Date: 2024-11-19GUANGDONG JIUZHOU POLYMER MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310127844.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-17
Publication Date
2024-11-19
Estimated Expiration
2043-02-17

AI Technical Summary

Technical Problem

PC/ABS composite materials tend to age when exposed to light environment for a long time, resulting in a decrease in material strength. The prior art solves the aging problem by adding ultraviolet absorbers and light stabilizers, but requires a large amount of addition to improve dispersion, resulting in a decrease in mechanical properties.

Method used

The modified anti-aging agent is made from composite nanoparticles. By adsorbing the anti-aging agent on the surface of the composite nanoparticles and dispersing it in the modified liquid, the dispersion of the anti-aging agent is improved, the amount of addition is reduced, and the PC resin is combined with ABS resin, compatible agent, MBS copolymer and plastic lubricant optimized ratios to improve the anti-aging properties of the material.

Benefits of technology

It effectively improves the anti-aging properties of the material and extends the service life. The use of modified anti-aging agents reduces the impact on the material strength reduction, and improves the tensile, bending and impact resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004082689990000071
    Figure BDA0004082689990000071
  • Figure BDA0004082689990000081
    Figure BDA0004082689990000081
Patent Text Reader

Abstract

The present application relates to the technical field of plastic alloys, and specifically discloses a masterbatch for automobile interior accessories and a preparation method thereof. The masterbatch for automobile interior accessories comprises the following raw materials in parts by weight: 45-70 parts of PC resin, 25-45 parts of ABS resin, 0.5-1.5 parts of compatibilizer, 1-3 parts of MBS copolymer, 0.5-0.8 parts of modified anti-aging agent, 0.2-0.6 parts of anti-ultraviolet absorber and 0.1-0.4 parts of plastic lubricant; the modified anti-aging agent is prepared by modifying nano-silica; the masterbatch for automobile interior accessories prepared in the present application has good anti-aging performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of plastic alloys, and more specifically, to a masterbatch for automotive interior accessories and a preparation method thereof. Background Art

[0002] PC / ABS alloy material is a polycarbonate product that has the advantages of both PC and ABS. It is often used as plastic for automobiles, such as automobile dashboards, seat supports, air intake grilles, bumper shells and other product packaging shells. PC resin is a strong thermoplastic resin, but it is not resistant to ultraviolet light and is easily exposed to external ultraviolet light, which increases the internal heat energy of the resin and reduces the strength of the resin. ABS resin is a thermoplastic polymer material with high strength, good toughness and easy processing and molding. It has excellent heat resistance and can improve the heat resistance of PC resin. However, if it is exposed to light for a long time, the material is prone to aging, resulting in reduced material strength and shortened material life.

[0003] At present, in the aging resistance of PC / ABS composite materials, UV absorbers and light stabilizers are basically added to the composite materials to solve the aging problem. However, due to the low dispersibility of UV absorbers and light stabilizers in the composite material system, more UV absorbers and light stabilizers need to be added to play an anti-aging role. But at the same time, excessive addition of UV absorbers and light stabilizers will reduce the mechanical properties of the composite materials. Summary of the invention

[0004] In order to improve the anti-aging performance of PC / ABS composite materials, the present application provides a masterbatch for automotive interior accessories and a preparation method thereof.

[0005] In the first aspect, the present application provides a masterbatch for automotive interior accessories, using the following technical solution:

[0006] A masterbatch for automobile interior accessories comprises the following raw materials in parts by weight: 45-70 parts of PC resin, 25-45 parts of ABS resin, 0.5-1.5 parts of compatibilizer, 1-3 parts of MBS copolymer, 0.5-0.8 parts of modified anti-aging agent, 0.2-0.6 parts of anti-ultraviolet absorber and 0.1-0.4 parts of plastic lubricant; the modified anti-aging agent is prepared by modifying composite nanoparticles.

[0007] By adopting the above technical scheme, the present application prepares a masterbatch for automotive interior accessories by using PC resin, ABS resin, compatibilizer, MBS copolymer, modified anti-aging agent, anti-ultraviolet absorber and plastic lubricant. Among them, the modified anti-aging agent in the raw material is prepared by modifying the composite nanoparticles, the composite nanoparticles are used to modify the anti-aging agent, the anti-aging agent is adsorbed on the surface of the composite nanoparticles, and then dispersed in the system, thereby improving the dispersibility of the anti-aging agent, avoiding the need to add a large amount of anti-aging agent due to the low dispersibility of the anti-aging agent, and thus avoiding excessive anti-aging agent from reducing the strength of the alloy material; on the other hand, the added composite nanoparticles can promote the dispersibility of the material in the system, and at the same time, the composite nanoparticles are first modified by the modifying liquid to reduce the amount of hydroxyl groups on their surface, reduce their surface energy, improve their wettability and dispersibility in the organic phase, and avoid the agglomeration of the composite nanoparticles in the organic phase after reduction, and can be better compatible and dispersed with the polymer, thereby indirectly improving the dispersibility of the anti-aging agent in the system and reducing the amount of anti-aging agent added.

[0008] Preferably, the masterbatch for automotive interior accessories comprises the following raw materials in parts by weight: 55-60 parts of PC resin, 30-35 parts of ABS resin, 0.8-1 parts of compatibilizer, 1.5-2.5 parts of MBS copolymer, 0.6-0.7 parts of modified anti-aging agent, 0.4-0.5 parts of anti-ultraviolet absorber and 0.2-0.3 parts of plastic lubricant.

[0009] By adopting the above technical solution, the present application optimizes the ratio between the raw materials of the masterbatch for automobile interior accessories, so that the prepared masterbatch for automobile interior accessories has better tensile properties, bending properties and impact resistance.

[0010] Preferably, the modified anti-aging agent comprises the following raw materials in parts by weight: 2-6 parts of composite nanoparticles, 40-50 parts of modified liquid and 1-2 parts of anti-aging agent; the composite nanoparticles are composed of nano-white carbon black, nano-titanium dioxide and ultrafine mica in equal proportions.

[0011] Preferably, the preparation method of the modified anti-aging agent is:

[0012] 1) Add the composite nanoparticles into the modified solution and disperse them ultrasonically for 3-5 times;

[0013] 2) Then raise the temperature to 65-85°C and stir for 2-5h, add an anti-aging agent, continue to raise the temperature, and stir at 95-110°C for 3-12min;

[0014] 3) After drying and crushing, a modified anti-aging agent is obtained.

[0015] By adopting the above technical scheme, in the present application, nano-white carbon black, nano-titanium dioxide and ultrafine mica are added to the modifying liquid, and the modifying liquid can perform surrounding surface modification on the nano-white carbon black, nano-titanium dioxide and ultrafine mica, and ultrasonic dispersion is used to evenly disperse the nano-white carbon black, nano-titanium dioxide and ultrafine mica to avoid agglomeration of nano powders, and then heating and stirring at 65-85°C to remove the organic solvent component in the mixed solvent, and finally adding an anti-aging agent to evenly attach the anti-aging agent to the surface of the modified composite nanoparticles. The preparation method is simple and easy.

[0016] Preferably, the anti-aging agent is a mixture of dioctadecyl pentaerythritol phosphate, bis(2,4-di-tert-butylphenol) pentaerythritol diphosphite and triphenyl phosphite in a mass ratio of 1:1:(1-3).

[0017] By adopting the above technical scheme, the anti-aging agent in the present application is a mixture of dioctadecyl pentaerythritol phosphate, bis(2,4-di-tert-butylphenol) pentaerythritol diphosphite and triphenyl phosphite. When the mass ratio of dioctadecyl pentaerythritol phosphate, bis(2,4-di-tert-butylphenol) pentaerythritol diphosphite and triphenyl phosphite is 1:1:2, the prepared anti-aging agent is added to the raw material after modification, and the prepared material has the best anti-aging performance.

[0018] Preferably, the raw materials further include 2-6 parts by weight of glass fiber.

[0019] By adopting the above technical solution, glass fibers are also added in the present application. The glass fibers are evenly dispersed in the material to fill the gaps between the materials, thereby improving the bonding strength of the materials and thus improving the anti-aging performance of the materials.

[0020] Preferably, the compatibilizer is one or more of maleic anhydride grafted styrene-butadiene-acrylonitrile terpolymer, acrylonitrile-styrene copolymer grafted maleic anhydride, and polymethyl methacrylate grafted maleic anhydride.

[0021] By adopting the above technical solution, adding a compatibilizer to the raw materials can reduce the interfacial tension between PC resin and ABS resin, reduce the particle size of the dispersed phase, increase the surface area of ​​the dispersed phase, improve the combined force between the dispersed phase and the continuous phase, stabilize the dispersed phase, and further improve the compatibility of PC resin and ABS resin, so that the phase structure will not change, thereby improving the stability of the material.

[0022] Preferably, the anti-ultraviolet absorber is 2-hydroxy-4-n-octyloxybenzophenone.

[0023] By adopting the above technical scheme, 2-hydroxy-4-n-octyloxybenzophenone is used as an anti-ultraviolet absorber in the present application, which can strongly absorb ultraviolet rays, and at the same time has good compatibility with PC resin and ABS resin, low volatility, and can promote the dispersion uniformity of the entire composite anti-aging agent in the system.

[0024] In a second aspect, the present application provides a method for preparing a masterbatch for automotive interior accessories, using the following technical solution:

[0025] A method for preparing a masterbatch for automotive interior accessories comprises the following steps:

[0026] 1) Weigh each raw material, keep the material temperature at 50-60°C, mix for 10-20 minutes to obtain a mixture;

[0027] 2) melt-granulating the mixture obtained in step 1), wherein the melt-granulation is divided into a preheating section, a melting section and an extrusion section; the temperature of the preheating section is 245-250° C. and the dwell time is 5 min; the temperature of the melting section is 240-245° C. and the dwell time is 5 min; the temperature of the extrusion section is 235-240° C.

[0028] By adopting the above technical solution, the masterbatch for automobile interior accessories prepared in the present application has readily available raw materials, a simple and easy preparation method, and can effectively improve production efficiency.

[0029] In summary, this application has the following beneficial effects:

[0030] 1. The present application prepares a masterbatch for automotive interior accessories by using PC resin, ABS resin, compatibilizer, MBS copolymer, modified anti-aging agent, anti-ultraviolet absorber and plastic lubricant. Among them, the modified anti-aging agent in the raw material is prepared by modifying the composite nanoparticles, the composite nanoparticles are used to modify the anti-aging agent, the anti-aging agent is adsorbed on the surface of the composite nanoparticles, and then dispersed in the system, thereby improving the dispersibility of the anti-aging agent, avoiding the need to add a large amount of anti-aging agent due to the low dispersibility of the anti-aging agent, and thus avoiding excessive anti-aging agent from reducing the strength of the alloy material; on the other hand, the added composite nanoparticles can promote the dispersibility of the materials in the system, and at the same time, the composite nanoparticles are first modified by the modification liquid to reduce the amount of hydroxyl groups on their surface, reduce their surface energy, improve their wettability and dispersibility in the organic phase, and avoid the agglomeration of the composite nanoparticles in the organic phase after reduction, so that they can be better compatible and dispersed with the polymer, thereby indirectly improving the dispersibility of the anti-aging agent in the system and reducing the amount of anti-aging agent added.

[0031] 2. The masterbatch for automotive interior accessories prepared in this application has a tensile strength of 51.0MPa, an elongation at break of 67.5%, a flexural strength of 50.3MPa and an impact strength of 50.2kJ / m after being irradiated with a xenon lamp for 1000h. 2 The material produced has good anti-aging performance. DETAILED DESCRIPTION

[0032] The present application is further described in detail below with reference to the embodiments.

[0033] raw material

[0034] The raw materials used in this application are all common commercially available materials.

[0035] Preparation Example

[0036] Preparation Example 1-3

[0037] A modified anti-aging agent of Preparation Example 1-3, whose raw materials and the amounts of each raw material are shown in Table 1, and whose preparation method comprises the following steps:

[0038] 1) Add the composite nanoparticles into the modified solution and disperse them ultrasonically for 3 times;

[0039] 2) Then raise the temperature to 65°C and stir for 3 hours, add an anti-aging agent, continue to raise the temperature, and stir at 95°C for 5 minutes;

[0040] 3) After drying and crushing, a modified anti-aging agent is obtained.

[0041] Among them, the composite nanoparticles are composed of nano-silica, nano-titanium dioxide and ultrafine mica in a mass ratio of 1:1:1, the anti-aging agent is a mixture of dioctadecyl pentaerythritol phosphate, bis(2,4-di-tert-butylphenol) pentaerythritol diphosphite and triphenyl phosphite in a mass ratio of 1:1:1, and the modified liquid is a mixture of γ-mercaptopropyltrimethoxysilane, isopropanol and water in a mass ratio of 2:5:10.

[0042] Table 1 Raw materials and amounts of each raw material used in Preparation Examples 1-3 (kg)

[0043] Preparation Example 1 Preparation Example 2 Preparation Example 3 Composite Nanoparticles 2 4 6 Modified liquid 50 45 40 Anti-aging agents 1 1.5 2

[0044] Preparation Example 4

[0045] A modified anti-aging agent, which is different from Preparation Example 2 in that the anti-aging agent is a mixture of dioctadecyl pentaerythritol phosphate, bis(2,4-di-tert-butylphenol) pentaerythritol diphosphite and triphenyl phosphite in a mass ratio of 1:1:2, and the remaining steps are the same as Preparation Example 1.

[0046] Preparation Example 5

[0047] A modified anti-aging agent, which is different from Preparation Example 2 in that the anti-aging agent is a mixture of dioctadecyl pentaerythritol phosphate, bis(2,4-di-tert-butylphenol) pentaerythritol diphosphite and triphenyl phosphite in a mass ratio of 1:1:3, and the remaining steps are the same as Preparation Example 1.

[0048] Example

[0049] Examples 1-4

[0050] The raw materials and the amounts of the raw materials of the masterbatch for automobile interior accessories of Example 1-4 are shown in Table 2, and the preparation method thereof is as follows:

[0051] 1) Weigh each raw material by weight, keep the material temperature at 50°C, mix for 15 minutes to obtain a mixture;

[0052] 2) The mixed material obtained in step 1) is fed into a screw extruder for melt granulation. The processing technology of the screw extruder is divided into a preheating section, a melting section and an extrusion section; the temperature of the preheating section is 250°C and the dwell time is 5 min; the temperature of the melting section is 245°C and the dwell time is 5 min; the temperature of the extrusion section is 240°C.

[0053] Wherein, the modified anti-aging agent comes from Preparation Example 1, and the plastic lubricant is PETS.

[0054] Table 2 Raw materials and amounts of each raw material in Examples 1-4 (kg)

[0055] Example 1 Example 2 Example 3 Example 4 PC resin 45 55 60 70 ABS resin 45 35 30 25 Compatibilizer 0.5 0.8 1 1.5 MBS copolymer 3 2.5 1.5 1 Modified Anti-aging Agent 0.5 0.5 0.5 0.5 UV absorber 0.2 0.4 0.5 0.6 Plastic Lubricant 0.4 0.3 0.2 0.1

[0056] Example 5

[0057] A masterbatch for automobile interior accessories, which is different from Example 3 in that the modified anti-aging agent comes from Preparation Example 2, and the remaining steps are the same as Example 3.

[0058] Example 6

[0059] A masterbatch for automobile interior accessories, which is different from Example 3 in that the modified anti-aging agent comes from Preparation Example 3, and the remaining steps are the same as Example 3.

[0060] Example 7

[0061] A masterbatch for automobile interior accessories, which is different from Example 5 in that the modified anti-aging agent comes from Preparation Example 4, and the remaining steps are the same as Example 5.

[0062] Example 8

[0063] A masterbatch for automobile interior accessories, which is different from Example 5 in that the modified anti-aging agent comes from Preparation Example 5, and the remaining steps are the same as Example 5.

[0064] Example 9

[0065] A masterbatch for automotive interior accessories, which is different from Example 7 in that the added amount of the modified anti-aging agent is 0.6 kg, and the remaining steps are the same as Example 7.

[0066] Example 10

[0067] A masterbatch for automotive interior accessories, which is different from Example 7 in that the added amount of the modified anti-aging agent is 0.7 kg, and the remaining steps are the same as Example 7.

[0068] Embodiment 11

[0069] A masterbatch for automotive interior accessories, which is different from Example 7 in that the added amount of the modified anti-aging agent is 0.8 kg, and the remaining steps are the same as Example 7.

[0070] Example 12

[0071] A masterbatch for automotive interior accessories, which is different from Example 10 in that 2 kg of glass fiber is also added to the raw materials, and the remaining steps are the same as Example 10.

[0072] Example 13

[0073] A masterbatch for automotive interior accessories, which is different from Example 10 in that 4 kg of glass fiber is also added to the raw materials, and the remaining steps are the same as Example 10.

[0074] Embodiment 14

[0075] A masterbatch for automotive interior accessories, which is different from Example 10 in that 6 kg of glass fiber is also added to the raw materials, and the remaining steps are the same as Example 10.

[0076] Comparative Example

[0077] Comparative Example 1

[0078] A masterbatch for automobile interior accessories, which is different from Example 1 in that an equal amount of an anti-aging agent that has not been treated with composite nanoparticles is added, and the remaining steps are the same as those of Example 1.

[0079] Comparative Example 2

[0080] A masterbatch for automobile interior accessories, which is different from Example 1 in that the added amount of the modified anti-aging agent is 0, and the remaining steps are the same as those of Example 1.

[0081] Comparative Example 3

[0082] A masterbatch for automobile interior accessories, which is different from Example 1 in that the amount of dioctadecyl pentaerythritol phosphate added in the modified anti-aging agent is 0, and the remaining steps are the same as those in Example 1.

[0083] Comparative Example 4

[0084] A masterbatch for automotive interior accessories, which is different from Example 1 in that the amount of bis(2,4-di-tert-butylphenol)pentaerythritol diphosphite added in the modified anti-aging agent is 0, and the remaining steps are the same as those in Example 1.

[0085] Comparative Example 5

[0086] A masterbatch for automobile interior accessories, which is different from Example 1 in that the amount of triphenyl phosphite added in the modified anti-aging agent is 0, and the remaining steps are the same as those in Example 1.

[0087] Performance testing

[0088] Detection method / test method

[0089] The following performance tests were performed on the masterbatches for automotive interior accessories prepared in Examples 1-14 and Comparative Examples 1-5. The test results are shown in Table 3.

[0090] The samples prepared in Examples 1-14 and Comparative Examples 1-5 were irradiated with a xenon lamp in a laboratory for 1000 hours, and their tensile properties, bending properties, and impact resistance were tested before and after the irradiation.

[0091] Among them, the tensile properties are tested in accordance with GB / T1040-1992 "Test method for tensile properties of plastics"; the bending properties are tested in accordance with GB / T19341 "Test method for bending properties of plastics"; and the impact resistance is tested in accordance with GB / T1043-1993 "Rigid Plastic Simply Supported Beam Impact Test Method".

[0092] Table 3 Test results of Examples 1-14 and Comparative Examples 1-5

[0093]

[0094]

[0095] Combined with the test data of Examples 1-4, it can be seen that the ratio of the raw materials in Example 3 is better. The masterbatch for automotive interior accessories prepared by the ratio of Example 3 has high tensile strength, elongation at break, bending strength and impact strength after 1000 hours of xenon lamp irradiation, indicating good anti-aging performance.

[0096] Combining the test data of Example 3 and Examples 5-6, it can be seen that the modified anti-aging agent of Preparation Example 2 is better. The modified anti-aging agent prepared by Preparation Example 2 is added to the preparation process of masterbatch for automotive interior accessories. The masterbatch for automotive interior accessories finally prepared has high tensile strength, elongation at break, flexural strength and impact strength after 1000 hours of xenon lamp irradiation, indicating good anti-aging performance.

[0097] Combining the test data of Example 5 and Example 7-8, it can be seen that when preparing the modified anti-aging agent, the anti-aging agent is a mixture of dioctadecyl pentaerythritol phosphate, bis(2,4-di-tert-butylphenol) pentaerythritol diphosphite and triphenyl phosphite in a mass ratio of 1:1:2. The prepared modified anti-aging agent has good anti-aging performance. After 1000h of xenon lamp irradiation, its tensile strength is 49.5MPa, the elongation at break is 65.9%, the flexural strength is 49.2MPa and the impact strength is 49.0kJ / m 2 Combined with the test data of comparative examples 3-5, it can be seen that there is a synergistic effect between dioctadecyl pentaerythritol phosphate, bis(2,4-di-tert-butylphenol) pentaerythritol diphosphite and triphenyl phosphite. When the addition amount of any one of them is 0, the anti-aging performance of the masterbatch is not as good as when all three are added at the same time.

[0098] From the test data of Example 7 and Examples 9-11, it can be seen that when the addition amount of the modified anti-aging agent is 0.7 kg, the matching between the masterbatch raw materials for automotive interior accessories is better, and the prepared masterbatch for automotive interior accessories has high tensile strength, elongation at break, flexural strength and impact strength after 1000 hours of xenon lamp irradiation, indicating good anti-aging performance.

[0099] Combining the test data of Example 10 and Examples 12-14, it can be seen that adding 4 kg of glass fiber to the raw material can improve the mechanical properties of the material, thereby improving its anti-aging effect. Among them, after 1000 hours of xenon lamp irradiation, its tensile strength can reach 51.0 MPa, elongation at break is 67.5%, bending strength is 50.3 MPa and impact strength is 50.2 kJ / m 2 .

[0100] Combining the test data of Example 1 and Comparative Example 1, it can be seen that the anti-aging performance of the masterbatch obtained by adding the same amount of anti-aging agent that has not been treated with nano-silica is not as good as that of the anti-aging agent after adding the modified anti-aging agent, indicating that nano-silica can effectively improve the dispersibility of the anti-aging agent, thereby improving the anti-aging performance of the material. Combining the test data of Comparative Example 2, it can be seen that without adding the anti-aging agent, the mechanical properties of the obtained material are all deteriorated, indicating that the anti-aging agent can effectively improve the anti-aging performance of the material.

[0101] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A masterbatch for automotive interior accessories, characterized in that: The invention comprises the following raw materials in parts by weight: 45-70 parts of PC resin, 25-45 parts of ABS resin, 0.5-1.5 parts of compatibilizer, 1-3 parts of MBS copolymer, 0.5-0.8 parts of modified anti-aging agent, 0.2-0.6 parts of anti-ultraviolet absorber and 0.1-0.4 parts of plastic lubricant; the modified anti-aging agent is prepared by modifying composite nanoparticles, and the modified anti-aging agent comprises the following raw materials in parts by weight: 2-6 parts of composite nanoparticles, 40-50 parts of modified liquid and 1-2 parts of anti-aging agent; the composite nanoparticles are composed of nano white carbon black, nano titanium dioxide and ultrafine mica in equal mass ratios; the preparation method of the modified anti-aging agent is as follows: 1) Add the composite nanoparticles into the modified solution and disperse them ultrasonically for 3-5 times; 2) Then heat to 65-85℃ and stir for 2-5h, add anti-aging agent, continue to heat, and stir at 95-110℃ for 3-12min; 3) After drying and crushing, a modified anti-aging agent is obtained; The anti-aging agent is a mixture of dioctadecyl pentaerythritol phosphate, bis(2,4-di-tert-butylphenol) pentaerythritol diphosphite and triphenyl phosphite in a mass ratio of 1:1:(1-3).

2. The masterbatch for automotive interior accessories according to claim 1, characterized in that: The masterbatch for automobile interior accessories comprises the following raw materials in parts by weight: 55-60 parts of PC resin, 30-35 parts of ABS resin, 0.8-1 parts of compatibilizer, 1.5-2.5 parts of MBS copolymer, 0.6-0.7 parts of modified anti-aging agent, 0.4-0.5 parts of anti-ultraviolet absorber and 0.2-0.3 parts of plastic lubricant.

3. The masterbatch for automotive interior accessories according to claim 1, characterized in that: The raw materials also include 2-6 parts by weight of glass fiber.

4. The masterbatch for automotive interior accessories according to claim 1, characterized in that: The compatibilizer is one or more of maleic anhydride grafted styrene-butadiene-acrylonitrile terpolymer, acrylonitrile-styrene copolymer grafted maleic anhydride, and polymethyl methacrylate grafted maleic anhydride.

5. The masterbatch for automotive interior accessories according to claim 1, characterized in that: The anti-ultraviolet absorber is 2-hydroxy-4-n-octyloxybenzophenone.

6. A method for preparing a masterbatch for automotive interior accessories according to any one of claims 1 to 5, characterized in that: It includes the following steps: 1) Weigh all raw materials, keep the material temperature at 50-60°C, mix for 10-20 minutes to obtain a mixed material; 2) Melting and granulating the mixture obtained in step 1), wherein the melt granulation is divided into a preheating section, a melting section and an extrusion section; the temperature of the preheating section is 240-260°C, and the dwell time is 5-10 min; the temperature of the melting section is 235-255°C, and the dwell time is 5-10 min; the temperature of the extrusion section is 230-250°C.