A hydrophilic anticoagulant coating for a pump tube for an extracorporeal circulation circuit and a preparation method thereof

By forming a hydrophilic anticoagulant coating with a polymer interpenetrating network skeleton structure on medical catheters, the problem of insufficient adhesion of the catheter coating is solved, long-term hydrophilicity and anticoagulant effects are achieved, and the rate of thrombosis is reduced. .

CN116285620BActive Publication Date: 2024-10-01NINGBO TIANYI MEDICAL APPLIANCE CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202211724390.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-30
Publication Date
2024-10-01
Estimated Expiration
2042-12-30

AI Technical Summary

Technical Problem

The hydrophilic anticoagulant coating of existing medical catheters has insufficient adhesion, resulting in unsustainable lubrication effect and increased thrombosis rate.

Method used

A hydrophilic anticoagulant coating composed of a skeleton polymer, a super-lubricant hydrophilic polymer and a coupling agent is used to form a polymer interpenetrating network skeleton structure through the graft polymerization reaction of active monomers and nitrocellulose to improve the coating adhesion. Focus on strengthening the polar groups on the surface of the base material through plasma treatment to enhance the adhesion and anti-coagulation effect of the coating.

Benefits of technology

Significantly improves the adhesion between the catheter and the pump tube, maintains long-term hydrophilicity and anticoagulant properties, and reduces the friction between the catheter and the tissue and the thrombosis rate.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to a hydrophilic anticoagulant coating for a pump tube for an extracorporeal circulation pipeline and a preparation method thereof, and belongs to the field of medical technology. The hydrophilic anticoagulant coating of the present invention is made of raw materials including the following weight percentages: 0.55% to 2.8% of a skeleton polymer, 0.8% to 3.6% of a super-lubricating hydrophilic polymer, 0.05% to 2.2% of a coupling agent, 8% to 31% of an organic solvent, and 66% to 97% of water; the preparation method includes preparing a skeleton polymer, configuring a coating liquid, and preparing a pump tube for an extracorporeal circulation pipeline containing a hydrophilic anticoagulant coating. The hydrophilic anticoagulant coating of the present invention effectively improves the adhesion between the coating and the pump tube substrate material while giving the pump tube for an extracorporeal circulation pipeline hydrophilicity and anticoagulant properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of medical technology and relates to a hydrophilic anticoagulant coating of a pump tube for an extracorporeal circulation pipeline and a preparation method thereof. Background Art

[0002] Medical catheters are essential consumables widely used in various surgical operations and intubation surgeries. Currently, most medical catheter base materials are made of polymer materials such as polyvinyl chloride (PVC), polyurethane (PUR), and silicone rubber. Their surfaces are highly hydrophobic.

[0003] During the treatment, the catheter will have a large friction with the human organs and tissues, which will cause poor patient comfort and may cause tissue damage and infection. Lubricants such as glycerol and silicone oil can be applied to the catheter surface to reduce friction, but the lubricant is easy to fall off, the lubrication effect is not sustainable, and the lubricant residue in the tissue will cause bacteria to breed and cause infection.

[0004] Super-lubricating hydrophilic polymers can form a stable hydrophilic cross-linked coating on the surface of the catheter, using the non-ionic (such as hydroxyl, amine, ether bond, etc.) or ionic (such as carboxyl, sulfonic acid, quaternary amino, etc.) hydrophilic groups contained in the molecules to absorb a large amount of water to form a hydration layer, giving the coating hydrophilicity and super-lubricity, significantly reducing the friction between the catheter and the tissue. In recent years, hydrophilic polymer materials such as polyvinyl pyrrolidone (PVP), polyacrylamide (PAM), polyethylene glycol (PEG), polyvinyl alcohol (PVA), natural polysaccharides and derivatives have been used for surface modification of medical catheters. However, the hydrophobicity of PVC, PUR, silicone rubber and other substrates used in medical catheters leads to poor adhesion between them and hydrophilic polymer coatings such as PVP, PAM, PEG, polysaccharides, etc., and there are problems such as easy detachment of the hydrophilic coating and unsustainable lubrication effect.

[0005] The hydrophilic modification must be moderate; otherwise, it will not only fail to increase the compatibility of the catheter with blood, but will increase the rate of thrombosis. Summary of the invention

[0006] The purpose of the present invention is to address the technical problem in the prior art that the hydrophilic anticoagulant layer formed by super-lubricating hydrophilic polymers on the pump tube for extracorporeal circulation piping has insufficient adhesion to the pump tube. A hydrophilic anticoagulant coating for the pump tube for extracorporeal circulation piping and a preparation method thereof are proposed, which can effectively improve the adhesion between the coating and the pump tube base material while giving the pump tube for extracorporeal circulation piping hydrophilicity and anticoagulant properties.

[0007] The purpose of the present invention can be achieved by the following technical solutions:

[0008] A hydrophilic anticoagulant coating for a pump tube for an extracorporeal circulation circuit, wherein the hydrophilic anticoagulant coating is made of the following raw materials in percentage by weight:

[0009] Backbone polymer 0.55%~2.8%,

[0010] Super lubricating hydrophilic polymer 0.8%~3.6%,

[0011] Coupling agent 0.05%~2.2%,

[0012] Organic solvent 8%~31%,

[0013] Water 66%~90%.

[0014] Preferably, the backbone polymer is produced by the reaction of an active monomer and nitrocellulose, and the active monomer is one or more of diphenylmethane diisocyanate, toluene diisocyanate or hexamethylene diisocyanate.

[0015] Preferably, the super lubricating hydrophilic polymer is one or more of polyvinyl pyrrolidone, polyacrylic acid resin, polyacrylamide and sodium polyacrylate.

[0016] Preferably, the coupling agent is any one of KH-550, KH-560, KH-570, KH-520, KH-540, HD-602, HD-603, and Si-402.

[0017] Preferably, the organic solvent is one or more of acetone, dimethylacetamide and ethanol.

[0018] Preferably, the pump tube for the extracorporeal circulation circuit is made of polyvinyl chloride (PVC), polyurethane (PUR) or silicone rubber.

[0019] Another object of the present invention is to provide a method for preparing a hydrophilic anticoagulant coating of a pump tube for an extracorporeal circulation circuit, the preparation method comprising the following steps:

[0020] S1, preparing a backbone polymer, dissolving the dried nitrocellulose in an organic solvent, then adding an active monomer, heating and reacting under the protection of an inert gas, and cooling after the reaction is completed to obtain a backbone polymer;

[0021] S2, preparing a coating liquid, dissolving a super lubricating hydrophilic polymer () in water, adding an organic solvent, then adding a backbone polymer, stirring thoroughly, adding a coupling agent, and standing to obtain a coating liquid;

[0022] S3. Prepare an extracorporeal circulation tubing pump tube containing a hydrophilic anticoagulant coating, perform surface treatment on the extracorporeal circulation tubing pump tube, then apply the prepared coating liquid on the inner wall of the pump tube, let the coated pump tube stand, then perform a curing treatment to solidify the coating on the inner wall of the pump tube, and then place it at room temperature and pressure to obtain an extracorporeal circulation tubing pump tube with a hydrophilic anticoagulant coating.

[0023] Preferably, the method for drying the nitrocellulose in step S1 is distillation under reduced pressure to constant weight.

[0024] Preferably, the heating reaction in step S1 is carried out at a temperature of 40-60° C. for 80-100 min.

[0025] Preferably, the sufficient stirring in step S2 is performed by magnetic stirring.

[0026] Preferably, the surface treatment method in step S3 includes solvent circulation cleaning, hydroxylation or plasma treatment.

[0027] The active monomers in the present invention can undergo graft polymerization reaction with the surface of the pump tube substrate material and the active hydrogen of nitrocellulose, thereby forming a polymer interpenetrating network skeleton structure on the surface of the substrate material, so that the adhesion of the coating of the present invention on the surface of the pump tube substrate material is enhanced. At the same time, the coating constructs a slip surface on the surface of the pump tube substrate, which can inhibit water or blood wetting and thus hinder the adsorption of proteins, platelets, etc. on the surface of the material / device, and play an anticoagulant role. The present invention uses plasma technology to pre-treat the surface of the pump tube, generate polar groups on the surface of the substrate, and can improve the adhesion of the coating.

[0028] Compared with the prior art, the present invention has the following beneficial effects: the present invention uses diphenylmethane diisocyanate, toluene diisocyanate or hexamethylene diisocyanate as active monomers to carry out graft polymerization reaction with the base material of the pump tube for extracorporeal circulation and the active hydrogen of nitrocellulose, and a polymer interpenetrating network skeleton structure can be formed on the surface of the base material of the pump tube, thereby improving the adhesion of the hydrophilic anticoagulant coating on the pump tube. DETAILED DESCRIPTION

[0029] The following are specific embodiments of the present invention, which further describe the technical solutions of the present invention, but the present invention is not limited to these embodiments. Example 1

[0030] The hydrophilic anticoagulant coating of the pump tube for the extracorporeal circulation pipeline in this embodiment is made of raw materials including the following weight percentages:

[0031] Backbone polymer 1.7%,

[0032] Super lubricating hydrophilic polymer 2.0%,

[0033] Coupling agent 1.2%,

[0034] Organic solvent 18%,

[0035] Water 77%.

[0036] The method for preparing the hydrophilic anticoagulant coating of the pump tube for the extracorporeal circulation pipeline of the present invention comprises the following steps:

[0037] (1) Preparing a backbone polymer, placing nitrocellulose in a round-bottom flask, and distilling under reduced pressure to constant weight to remove water, taking an appropriate amount of solvent acetone into the round-bottom flask to dissolve the nitrocellulose, and then adding active monomer diphenylmethane diisocyanate, filling with nitrogen under sealed conditions, heating to 50°C and maintaining the temperature for 90 minutes under magnetic stirring and nitrogen protection, and cooling after the reaction is completed to obtain a backbone polymer;

[0038] (2) preparing a coating liquid, dissolving a super lubricating hydrophilic polymer polyvinyl pyrrolidone in water under rotating stirring conditions, then adding an organic solvent ethanol, and then adding a backbone polymer, adding a coupling agent KH-550 after sufficient magnetic stirring, and then standing to obtain a coating liquid;

[0039] (3) Prepare an extracorporeal circulation tubing pump tube containing a hydrophilic anticoagulant coating. Clean the extracorporeal circulation tubing pump tube and perform plasma treatment. Then, apply the prepared coating liquid on the inner wall of the pump tube in a circulating manner. Let the coated pump tube stand for 5 minutes, heat it to 80°C and keep it for 3 hours to solidify the coating on the inner wall of the pump tube. After leaving it at room temperature and pressure for 23 hours, the extracorporeal circulation tubing pump tube with a hydrophilic anticoagulant coating is obtained. Example 2

[0040] The hydrophilic anticoagulant coating of the pump tube for the extracorporeal circulation pipeline in this embodiment is made of raw materials including the following weight percentages:

[0041] Backbone polymer 2.2%,

[0042] Super lubricating hydrophilic polymer 0.8%,

[0043] Coupling agent 2.0%,

[0044] Organic solvent 25%,

[0045] Water 70%.

[0046] The hydrophilic anticoagulant coating of the pump tube for the extracorporeal circulation pipeline in this embodiment is made of raw materials including the following weight percentages:

[0047] The method for preparing the hydrophilic anticoagulant coating of the pump tube for the extracorporeal circulation pipeline of the present invention comprises the following steps:

[0048] (1) Preparing a backbone polymer, placing nitrocellulose in a round-bottom flask, and distilling under reduced pressure to constant weight to remove water, taking an appropriate amount of solvent acetone into the round-bottom flask to dissolve the nitrocellulose, and then adding active monomer diphenylmethane diisocyanate, filling with nitrogen under sealed conditions, heating to 50°C and maintaining the temperature for 90 minutes under magnetic stirring and nitrogen protection, and cooling after the reaction is completed to obtain a backbone polymer;

[0049] (2) preparing a coating liquid, dissolving a super lubricating hydrophilic polymer polyacrylic acid resin in water under rotating stirring conditions, then adding an organic solvent ethanol, and then adding a backbone polymer, adding a coupling agent KH-560 after sufficient magnetic stirring, and then standing to obtain a coating liquid;

[0050] (3) Prepare an extracorporeal circulation tubing pump tube containing a hydrophilic anticoagulant coating. Clean the extracorporeal circulation tubing pump tube and perform plasma treatment. Then, apply the prepared coating liquid on the inner wall of the pump tube in a circulating manner. Let the coated pump tube stand for 4 minutes, heat it to 80°C and keep it for 3 hours to solidify the coating on the inner wall of the pump tube. After leaving it at room temperature and pressure for 24 hours, the extracorporeal circulation tubing pump tube with a hydrophilic anticoagulant coating is obtained. Example 3

[0051] The hydrophilic anticoagulant coating of the pump tube for the extracorporeal circulation pipeline in this embodiment is made of raw materials including the following weight percentages:

[0052] Backbone polymer 0.6%,

[0053] Super lubricating hydrophilic polymer 0.9%,

[0054] Coupling agent 0.5%,

[0055] Organic solvent 8%,

[0056] Water 90%.

[0057] The method for preparing the hydrophilic anticoagulant coating of the pump tube for the extracorporeal circulation pipeline of the present invention comprises the following steps:

[0058] (1) Preparing a backbone polymer, placing nitrocellulose in a round-bottom flask, distilling under reduced pressure to constant weight to remove water, taking an appropriate amount of solvent acetone into the round-bottom flask to dissolve the nitrocellulose, and then adding active monomer toluene diisocyanate, filling with nitrogen under sealed conditions, heating to 60°C and maintaining the temperature for 80 minutes under magnetic stirring and nitrogen protection, and cooling after the reaction is completed to obtain a backbone polymer;

[0059] (2) preparing a coating liquid, dissolving a super lubricating hydrophilic polymer polyacrylamide in water under rotating stirring conditions, then adding an organic solvent acetone, and then adding a backbone polymer, adding a coupling agent KH-570 after sufficient magnetic stirring, and then standing to obtain a coating liquid;

[0060] (3) Prepare an extracorporeal circulation tubing pump tube containing a hydrophilic anticoagulant coating. Clean the extracorporeal circulation tubing pump tube and perform plasma treatment. Then, apply the prepared coating liquid on the inner wall of the pump tube in a circulating manner. Let the coated pump tube stand for 3 minutes, heat it to 80°C and keep it for 3 hours to solidify the coating on the inner wall of the pump tube. After leaving it at room temperature and pressure for 22 hours, the extracorporeal circulation tubing pump tube with a hydrophilic anticoagulant coating is obtained. Example 4

[0061] The hydrophilic anticoagulant coating of the pump tube for the extracorporeal circulation pipeline in this embodiment is made of raw materials including the following weight percentages:

[0062] Backbone polymer 2.8%,

[0063] Super lubricating hydrophilic polymer 3.0%,

[0064] Coupling agent 2.2%,

[0065] Organic solvent 20%,

[0066] Water 72%.

[0067] The method for preparing the hydrophilic anticoagulant coating of the pump tube for the extracorporeal circulation pipeline of the present invention comprises the following steps:

[0068] (1) Preparing a backbone polymer, placing nitrocellulose in a round-bottom flask, and distilling under reduced pressure to constant weight to remove water, taking an appropriate amount of solvent dimethylacetamide and adding it to the round-bottom flask to dissolve the nitrocellulose, and then adding active monomer diisocyanate, filling with nitrogen under sealed conditions, heating to 40°C and maintaining the temperature for 100 minutes under magnetic stirring and nitrogen protection, and cooling after the reaction is completed to obtain a backbone polymer;

[0069] (2) preparing a coating liquid, dissolving a super lubricating hydrophilic polymer sodium polyacrylate in water under rotating stirring conditions, then adding an organic solvent dimethylacetamide, and then adding a backbone polymer, adding a coupling agent KH-520 after sufficient magnetic stirring, and then standing to obtain a coating liquid;

[0070] (3) Prepare an extracorporeal circulation tubing pump tube containing a hydrophilic anticoagulant coating. Clean the extracorporeal circulation tubing pump tube and perform plasma treatment. Then, apply the prepared coating liquid on the inner wall of the pump tube in a circulating manner. Let the coated pump tube stand for 4 minutes, heat it to 80°C and keep it for 3 hours to solidify the coating on the inner wall of the pump tube. After leaving it at room temperature and pressure for 23 hours, the extracorporeal circulation tubing pump tube with a hydrophilic anticoagulant coating is obtained.

[0071] Comparative Example 1

[0072] Uncoated pump tubing for extracorporeal circulation circuits.

[0073] The relevant performance tests were performed on the pump tubes for extracorporeal circulation circuits with hydrophilic anticoagulant coatings prepared in the embodiments of the present invention and the comparative examples, and the methods are as follows:

[0074] (1) The contact angles of the pump tubes in Examples 1 to 5 and Comparative Example 1 were measured by a contact angle analyzer using a drop method; (2) The pump tubes in Examples 1 to 5 and Comparative Example 1 were immersed in distilled water for 3 hours, and then the contact angles were measured by a contact angle analyzer; (3) After the pump tubes in Examples 1 to 5 and Comparative Example 1 were immersed in distilled water for 3 hours, the sliding performance of the surfaces was tested using a universal material testing machine. The test results are shown in Table 1.

[0075] Table 1: Test results of the pump tubes in Examples 1 to 5 and Comparative Example 1

[0076] Performance Examples Contact angle (°) Contact angle after immersion for 3 hours (°) Surface friction (N) Example 1 39.6 44.0 0.040 Example 2 42.9 46.5 0.062 Example 3 42.3 45.8 0.058 Example 4 39.5 44.4 0.052 Comparative Example 1 76.3 76.4 1.8

[0077] As shown in Table 1, after the pump tube in the embodiment of the present invention is coated, the contact angle is significantly reduced, indicating that more hydrophilic groups are connected to the surface of the pump tube substrate, and the hydrophilicity is enhanced. After being immersed in distilled water for 3 hours, its contact angle is not much different from that at the beginning of the coating, indicating that the coating has good continuous hydrophilicity. The sliding performance test results show that the lubrication performance of the surface of the pump tube with the coating is significantly reduced, and the coating enables the pump tube to obtain better lubrication performance.

[0078] The specific embodiments described herein are merely examples of the spirit of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in similar ways, but they will not deviate from the spirit of the present invention or exceed the scope defined by the appended claims.

Claims

1. A method for preparing a hydrophilic anticoagulant coating of a pump tube for an extracorporeal circulation circuit, characterized in that: The hydrophilic anticoagulant coating is made of the following raw materials in weight percentage: Backbone polymer 0.55%~2.8%, Super lubricating hydrophilic polymer 0.8%~3.6%, Coupling agent 0.05%~2.2%, Organic solvent 8%~31%, Water 66%~90%, The backbone polymer is generated by the reaction of an active monomer and nitrocellulose, wherein the active monomer is one or more of diphenylmethane diisocyanate, toluene diisocyanate or hexamethylene diisocyanate; The super lubricating hydrophilic polymer is one or more of polyvinyl pyrrolidone, polyacrylic acid resin, polyacrylamide, and sodium polyacrylate; The coupling agent is any one of KH-550, KH-560, KH-570, KH-520, KH-540, HD-602, HD-603, and Si-402; The preparation method comprises the following steps: S1, preparing a backbone polymer, dissolving the dried nitrocellulose in an organic solvent, then adding an active monomer, heating and reacting under the protection of an inert gas, and cooling after the reaction is completed to obtain a backbone polymer; S2, preparing a coating liquid, dissolving a super lubricating hydrophilic polymer in water, adding an organic solvent, then adding a backbone polymer, stirring thoroughly, adding a coupling agent, and standing to obtain a coating liquid; S3. Prepare an extracorporeal circulation tubing pump tube containing a hydrophilic anticoagulant coating, perform surface treatment on the extracorporeal circulation tubing pump tube, then apply the prepared coating liquid on the inner wall of the pump tube, let the coated pump tube stand, then perform a curing treatment to solidify the coating on the inner wall of the pump tube, and then place it at room temperature and pressure to obtain an extracorporeal circulation tubing pump tube with a hydrophilic anticoagulant coating.

2. The method for preparing the hydrophilic anticoagulant coating of the pump tube for the extracorporeal circulation circuit according to claim 1, characterized in that: The organic solvent is one or more of acetone, dimethylacetamide and ethanol.

3. The method for preparing the hydrophilic anticoagulant coating of the pump tube for extracorporeal circulation according to claim 1, characterized in that: The method for drying the nitrocellulose in step S1 is to distill under reduced pressure to a constant weight.

4. The method for preparing the hydrophilic anticoagulant coating of the pump tube for the extracorporeal circulation circuit according to claim 1, characterized in that: The heating reaction in step S1 is carried out at a temperature of 40-60° C. for 80-100 min.

5. The method for preparing the hydrophilic anticoagulant coating of the pump tube for the extracorporeal circulation circuit according to claim 1, characterized in that: The surface treatment method in step S3 includes solvent circulation cleaning, hydroxylation or plasma treatment.

Citation Information

Cited By

  • Anticoagulant blood pipeline and method and device for preparing anticoagulant blood pipeline

    CN117838964A