A high wear-resistant and corrosion-resistant slider for linear guide rail and preparation method thereof
By rationally proportioning Cr, Nb, Mo, W, Si, Ni, C and other elements, as well as the addition of zirconium and titanium, and using bamboo charcoal and rutile nano-titanium dioxide as additives, combined with metal powder injection molding technology, the traditional slippery problem has been solved. The problem of poor wear resistance and corrosion resistance of the block has been solved, and the preparation of slide blocks with high wear resistance and high corrosion resistance has been realized, which extends the service life and reduces the cost.
Patent Information
- Application Number
- CN202310165750.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-27
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-02-27
AI Technical Summary
The traditional slider materials have poor wear resistance and corrosion resistance, resulting in insufficient service life of linear guide sliders, making it difficult to meet the high-precision and high-performance requirements of industrial automation equipment.
Using a reasonable ratio of Cr, Nb, Mo, W, Si, Ni, C and other elements, combined with the addition of zirconium and titanium, and bamboo charcoal and rutile nanometer titanium dioxide as additives, high wear resistance is prepared through metal powder injection molding technology , High corrosion resistance slider, using multi-stage vacuum sintering process and optimized formula of binder to form a slider with excellent wear resistance and corrosion resistance.
Significantly improves the wear resistance and corrosion resistance of the slider, reduces production costs, extends the service life of the slider, simplifies the process, increases the hardness and tensile strength of the material, and enhances the density and toughness of the material .
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of powder metallurgy, and in particular to a highly wear-resistant and corrosion-resistant slider for a linear guide rail and a preparation method thereof. Background Art
[0002] Linear guides are widely used in industrial automation equipment, and their moving parts - sliders are an important part of linear guides. The sliders have the characteristics of high precision, complex shapes and high performance requirements. Their lifespan determines the lifespan of the linear module. However, the traditional slider material is made of bearing steel, and the manufacturing technology of the raw material is a rolling process, resulting in poor wear resistance and corrosion resistance.
[0003] Therefore, improving the wear resistance and corrosion resistance of the slider is of great significance to improving the service life of the slider. Summary of the invention
[0004] In order to improve the wear resistance and corrosion resistance of the slider and thus increase the service life of the slider, the present application provides a high wear resistance and high corrosion resistance slider for a linear guide rail and a preparation method thereof.
[0005] In the first aspect, the present application provides a highly wear-resistant and corrosion-resistant slider for a linear guide rail, which adopts the following technical solution:
[0006] A highly wear-resistant and corrosion-resistant slider for a linear guide rail, comprising the following raw material ratios: Cr: 14-20wt%, Si: 0.3-1.0wt%, Mn: 0.3-1.0wt%, Nb: 0.5-4.0%, Mo: 0.3-1.5wt%, W: 0.3-5.0wt%, Ni: 0.1-0.5wt%, P≤0.02wt%, S≤0.02wt%, C: 0.8-1.9wt%, other impurities content ≤0.01%, and the balance is Fe.
[0007] By adopting the above technical solution, Cr is selected as the main strengthening element. When the Cr content reaches a certain level, Cr and oxygen can form dense oxides to block the further occurrence of corrosion, thereby producing good corrosion resistance. The preferred content is 14-20wt%; Nb is used as an additive element to expand the process characteristics of the material and increase the high-temperature mechanical properties of the material. If the content is too small, there will be no such characteristics, and if it is too much, the brittleness and cost of the material will be increased. Therefore, the preferred content is 0.5-4.0wt%; Mo can refine the structure and improve the toughness of the material. The preferred content is 0.3-1.5wt%; The addition of W can form WC particles with C in the material, greatly improving the wear resistance of the material, so adding a small amount of W is sufficient. Significantly improve the material properties. Excessive addition of W will easily form a decarburized phase, which will greatly increase the brittleness of the material. Therefore, its preferred addition amount is 0.3-5.0wt%; the addition of Si improves the smelting performance of the alloy, but excessive addition will cause structural defects such as pores. Its content is preferably 0.3-1.0wt%; the addition of Mn can reduce the brittle phase produced by the S element in the material, and its content is preferably 0.3-1.0wt%; the addition of Ni can improve the toughness of the material, but excessive Ni content will lead to a decrease in wear resistance, and its content is controlled at 0.1-0.5wt%; C needs to form a large amount of C compounds with the alloy, and heat treatment forms high-carbon martensite, so its content is controlled at 0.8-1.9wt%.
[0008] The present application adopts the above reasonable formula setting to obtain a slider having excellent wear resistance and corrosion resistance.
[0009] Preferably, it also includes 0.4-0.7wt% Zr and 0.13-0.21wt% Ti.
[0010] By adopting the above technical scheme, zirconium can refine the structural organization of the slider, promote the formation of fine crystals, the growth of organizational grains, increase pinning dislocations, stabilize substructures, and improve the hardness and tensile strength of the material macroscopically. At the same time, zirconium can also form FeZr3 phase with iron in the matrix, reduce the porosity of the alloy material, and make up for the shortcoming of high porosity of powder metallurgy materials. In addition, zirconium can also form low-melting-point ZrTi with titanium. ZrTi is mixed and diffused in the organization, overlapping each other to form a Zr-Ti skeleton with certain strength and plasticity, and other alloy particles are filled in between to enhance the toughness and density of the material.
[0011] Preferably, the invention further comprises 4-5 wt% of an auxiliary agent, wherein the auxiliary agent is a mixture of bamboo charcoal powder and rutile nano titanium dioxide in a mass ratio of 2:(2-3).
[0012] By adopting the above technical solution, bamboo charcoal itself has a series of advantages such as good thermal conductivity, high temperature resistance, corrosion resistance, self-lubrication, good chemical stability, and low thermal expansion coefficient. However, due to the low mechanical strength of bamboo charcoal itself and a small amount of pores on the back, the overall strength of the slider will be reduced. Rutile nano titanium dioxide has a higher hardness, which can not only fill the internal pores of bamboo charcoal and improve the strength of bamboo charcoal, but also improve the wear resistance and antioxidant properties of the slider and have a reinforcing effect.
[0013] In a second aspect, the present application provides a method for preparing a highly wear-resistant and corrosion-resistant slider for a linear guide rail, using the following technical solution:
[0014] A method for preparing a highly wear-resistant and corrosion-resistant slider for a linear guide rail comprises the following steps:
[0015] S1, mixing: mixing the raw materials and the binder at a temperature of 160-190°C in a sealed environment and granulating to form feed;
[0016] S2, injection molding: injecting the feed material into a mold to form a green body;
[0017] S3, degreasing: degreasing the green body to form a brown body;
[0018] S4, sintering: vacuum sintering the brown blank to form a sintered part;
[0019] S5, forming: the sintered parts are subjected to secondary processing to form finished products.
[0020] By adopting the above technical solution, the slider manufactured by metal powder injection molding technology can significantly reduce the production cost of the slider and has excellent wear resistance and corrosion resistance.
[0021] Preferably, in S1, the amount of the binder added is 4-12% of the total mass of the raw materials.
[0022] Preferably, the binder is made of the following raw materials in parts by weight: 50-95 parts of polyoxymethylene, 2-15 parts of polypropylene, 2-15 parts of high-density polyethylene and 1-10 parts of nickel-coated molybdenum disulfide.
[0023] By adopting the above technical solution, nickel-coated molybdenum disulfide is used as a lubricant to reduce the friction between the feed and the inner surface of the mold, which is convenient for molding and demoulding; polypropylene and high-density polyethylene are the skeleton components of the feed, which improve the strength of the injection molded green body. The binder of the present invention does not contain metal elements and can be completely removed after the degreasing process without changing the composition and performance of the sintered product.
[0024] Preferably, the binder further comprises 5-8 parts by weight of a polyol, wherein the polyol is one or more of trimethylolpropane, xylitol and sorbitol.
[0025] By adopting the above technical solution, the polyol is a water-soluble substance, and when mixed with other components, the system has better fluidity and the debonding step is easier, thereby greatly reducing the scrap rate of the product.
[0026] Preferably, in S4, the vacuum sintering is carried out in stages, including a low-temperature pre-sintering stage of 850-950°C, a medium-temperature heating sintering stage of 1000-1100°C, and a high-temperature insulation sintering stage of 1200-1300°C, and the vacuum degree is 3-5Pa.
[0027] By adopting the above technical scheme, metal recovery and volatilization of adsorbed gas and moisture occur in the low-temperature pre-firing stage, and the forming agent in the green sheet is decomposed and removed; recrystallization begins to appear in the medium-temperature heating sintering stage, and the deformed grains in the particles are restored and reorganized into new grains. At the same time, the oxides on the surface are reduced, and sintering necks are formed at the particle interface; the diffusion and flow in the high-temperature insulation sintering stage are fully carried out and nearly completed, forming a large number of closed pores, which continue to shrink, so that the pore size and the total number of pores are reduced, and the density of the sintered body is significantly increased.
[0028] Preferably, in S5, the secondary treatment includes shaping, heat treatment and surface treatment.
[0029] Preferably, the secondary treatment is to place the sintered part in Ar gas, rapidly heat it to 800-950° C., keep it warm for 1-4 hours, and then place the sintered part in a quenching medium for rapid cooling to obtain the final product.
[0030] By adopting the above technical solution, the metal powder injection molding process is used in the preparation of the slider, which simplifies the process, reduces costs, and can quickly form a finished product, and the finished product also has high wear resistance and high corrosion resistance.
[0031] In summary, the present application includes at least one of the following beneficial technical effects:
[0032] 1. In the present application, Cr is used as the main additive element, and Nb, Mo, W, Si, Mn, Ni and C are used as auxiliary elements. By cooperating with each other, the excellent characteristics of each element are fully utilized, and the slider obtained has excellent wear resistance and corrosion resistance;
[0033] 2. The present application adds zirconium and titanium elements. The zirconium element can improve the hardness and tensile strength of the material and reduce the porosity of the alloy material. At the same time, zirconium and titanium form a low-melting-point ZrTi structure that diffuses evenly and overlaps with each other to form a Zr-Ti skeleton with certain strength and plasticity. Other alloy particles fill in between, which enhances the toughness and density of the material.
[0034] 3. The present application improves the wear resistance and corrosion resistance of the slider by adding an additive, a mixture of bamboo charcoal and rutile nano titanium dioxide, through the synergistic effect of bamboo charcoal and rutile nano titanium dioxide;
[0035] 4. The preparation method of the present application adopts metal powder injection molding technology, which can not only significantly reduce the production cost of the slider, but also the prepared slider has excellent wear resistance and corrosion resistance. DETAILED DESCRIPTION
[0036] The present application is further described in detail below through examples.
[0037] Example
[0038] Example 1
[0039] This embodiment discloses a highly wear-resistant and corrosion-resistant slider for a linear guide rail, the implementation formula of which is made according to the following mass percentage, including Cr14-Si0.3-Mn0.3-Nb0.5-Mo0.3-W0.3-Ni0.1-C0.8-P0.02-S0.02, and the remainder is Fe and other impurities (the content of other impurities is ≤0.01).
[0040] This embodiment also discloses a method for preparing a highly wear-resistant and corrosion-resistant slider for a linear guide rail, comprising the following steps:
[0041] S1, weighing 100 kg of metal powder according to the formula and mixing and granulating with 9 kg of binder at a temperature of 160 ° C in a sealed environment to form a feed; wherein the binder comprises a mixture of the following raw materials in parts by weight: 5 kg of polyoxymethylene, 1.5 kg of polypropylene, 1.5 kg of high-density polyethylene and 1 kg of nickel-coated molybdenum disulfide; wherein the polyoxymethylene brand is DuPont of the United States, the polypropylene brand is BX3900, purchased from Shanghai Shunshi Plastic Chemical Co., Ltd., the high-density polyethylene is purchased from Dongguan Mingjia Plastic Products Co., Ltd., and the nickel-coated molybdenum disulfide has a particle size of 300 mesh and is purchased from Nangong Dinghong Metal Materials Co., Ltd.;
[0042] S2, using an injection molding machine to fill the feed into a mold for injection molding to form a green body;
[0043] S3, degreasing the green body to form a brown body; preliminarily removing the binder in the green body by extraction or catalysis at room temperature, the catalysis temperature is 120°C; degreasing the green body that has been preliminarily degreased again at a high temperature, the temperature of high-temperature degreasing is 450°C;
[0044] S4, evacuate the sintering furnace to a vacuum of 3Pa; first set the sintering furnace temperature to 850°C, place the brown blank in the sintering furnace for heating, then set the sintering furnace temperature to 1000°C for medium-temperature heating sintering, and finally set the sintering furnace temperature to 1200°C for high-temperature insulation to obtain a sintered part;
[0045] S5, placing the sintered part in Ar gas, rapidly heating it to 800°C, keeping it at that temperature for 4 hours, and then placing the sintered part in a quenching medium for rapid cooling to obtain the final product.
[0046] Example 2
[0047] This embodiment is basically the same as Embodiment 1, except that the high wear-resistant and corrosion-resistant slider for linear guide rails in this embodiment is made according to the following mass percentage, including Cr16-Si0.7-Mn0.7-Nb2.5-Mo1.0-W2.8-Ni0.3-C1.4-P0.01-S0.01, with the remainder being Fe and other impurities (the content of other impurities ≤ 0.01).
[0048] Example 3
[0049] This embodiment is basically the same as Embodiment 1, except that the high wear-resistant and corrosion-resistant slider for linear guide rails in this embodiment is made according to the following mass percentage, including Cr20-Si1.0-Mn1.0-Nb4.0-Mo1.5-W5.0-Ni0.5-C1.9, with the remainder being Fe and other impurities (the content of other impurities ≤0.01).
[0050] Example 4
[0051] This embodiment is basically the same as Embodiment 2, except that the high wear-resistant and corrosion-resistant slider for linear guide rails in this embodiment is made according to the following mass percentage, including Cr16-Si0.7-Mn0.7-Nb2.5-Mo1.0-W2.8-Ni0.3-C1.4-P0.01-S0.01-Zr0.4-Ti0.21, with the remainder being Fe and other impurities (the content of other impurities ≤ 0.01).
[0052] Example 5
[0053] This embodiment is basically the same as Embodiment 2, except that the high wear-resistant and corrosion-resistant slider for linear guide rails in this embodiment is made according to the following mass percentage, including Cr16-Si0.7-Mn0.7-Nb2.5-Mo1.0-W2.8-Ni0.3-C1.4-P0.01-S0.01-Zr0.7-Ti0.13, with the remainder being Fe and other impurities (the content of other impurities ≤0.01).
[0054] Example 6
[0055] This embodiment is basically the same as Embodiment 4, except that the high wear-resistant and corrosion-resistant slider for linear guide rails in this embodiment is made according to the following formula in mass percentage, including Cr16-Si0.7-Mn0.7-Nb2.5-Mo1.0-W2.8-Ni0.3-C1.4-P0.01-S0.01-Zr0.4-Ti0.21-bamboo charcoal powder 2-rutile nano titanium dioxide 2, and the remainder is Fe and other impurities (the content of other impurities ≤0.01), wherein the particle size of bamboo charcoal powder is 2000 mesh, the particle size of rutile nano titanium dioxide is S=15, L=50, the specific surface area is 50m2 / g, and it is purchased from Ningbo Jiwei Nano New Material Technology Co., Ltd.
[0056] Example 7
[0057] This embodiment is basically the same as Embodiment 2, except that the high wear-resistant and corrosion-resistant slider for linear guide rails in this embodiment is made according to the following mass percentage, including Cr16-Si0.7-Mn0.7-Nb2.5-Mo1.0-W2.8-Ni0.3-C1.4-P0.01-S0.01-Zr0.4-Ti0.21-bamboo charcoal powder 2-rutile nano titanium dioxide 3, and the remainder is Fe and other impurities (the content of other impurities is ≤0.01).
[0058] Example 8
[0059] This embodiment is basically the same as embodiment 7, except that: S1, 100 kg of metal powder is weighed according to the formula and mixed with 12 kg of binder at a temperature of 160°C in a sealed environment and granulated to form a feed; wherein the binder comprises a mixture of the following raw materials in parts by weight: 10 kg of polyoxymethylene, 0.4 kg of polypropylene, 0.4 kg of high-density polyethylene, 0.2 kg of nickel-coated molybdenum disulfide and 1 kg of trimethylolpropane; trimethylolpropane is purchased from Jinan Aoxing Chemical Co., Ltd. (in this embodiment, trimethylolpropane can also be replaced by an equal amount of xylitol, sorbitol or a mixture of trimethylolpropane, xylitol and sorbitol).
[0060] Example 9
[0061] This embodiment is basically the same as embodiment 7, except that: S1, 100Kg of metal powder is weighed according to the formula and mixed with 4Kg of binder at a temperature of 160°C in a sealed environment and granulated to form a feed; wherein the binder comprises a mixture of the following raw materials in parts by weight: 3Kg of polyoxymethylene, 0.28Kg of polypropylene, 0.32Kg of high-density polyethylene, 0.08Kg of nickel-coated molybdenum disulfide and 0.32Kg of trimethylolpropane.
[0062] Example 10
[0063] This embodiment is basically the same as Embodiment 9, except that the process parameters used in each step of the preparation method are different.
[0064] Specifically: a high wear-resistant and corrosion-resistant slider for a linear guide rail, comprising the following steps:
[0065] This embodiment also discloses a method for preparing a highly wear-resistant and corrosion-resistant slider for a linear guide rail, comprising the following steps:
[0066] S1, weighing 100 kg of metal powder according to the formula and mixing and granulating with 4 kg of binder at a temperature of 190° C. in a sealed environment to form a feed; wherein the binder comprises a mixture of the following raw materials in parts by weight: 3 kg of polyoxymethylene, 0.28 kg of polypropylene, 0.32 kg of high-density polyethylene, 0.08 kg of nickel-coated molybdenum disulfide and 0.32 kg of trimethylolpropane;
[0067] S2, using an injection molding machine to fill the feed into a mold for injection molding to form a green body;
[0068] S3, degreasing the green body to form a brown body; preliminarily removing the binder in the green body by extraction or catalysis at room temperature, the catalysis temperature is 110°C; degreasing the green body that has been preliminarily degreased again at a high temperature, the temperature of high-temperature degreasing is 550°C;
[0069] S4, evacuate the sintering furnace to a vacuum of 5Pa; first set the sintering furnace temperature to 950°C, place the brown blank in the sintering furnace for heating, then set the sintering furnace temperature to 1100°C for medium-temperature heating sintering, and finally set the sintering furnace temperature to 1300°C for high-temperature insulation to obtain a sintered part;
[0070] S5, placing the sintered part in Ar gas, rapidly heating it to 950°C, keeping it at that temperature for 1 hour, and then placing the sintered part in a quenching medium for rapid cooling to obtain the final product.
[0071] Comparative Example
[0072] Comparative Example 1
[0073] This comparative example discloses a highly wear-resistant and corrosion-resistant slider for a linear guide rail, which is formulated according to the following mass percentages, including Cr13-Si1.1-Mn1.1-Nb4.1-Mo1.6-W5.1-Ni0.6-C2.0-P0.03-S0.03, with the remainder being Fe and other impurities (the content of other impurities ≤0.01).
[0074] Comparative Example 2
[0075] This comparative example discloses a highly wear-resistant and corrosion-resistant slider for a linear guide rail, which is formulated according to the following mass percentages, including Cr21-Si0.2-Mn0.2-Nb0.4-Mo0.2-W0.2-Ni0.05-C0.7-P0.03-S0.03, with the remainder being Fe and other impurities (the content of other impurities ≤0.01).
[0076] Comparative Example 3
[0077] The slider used for the linear guide in this comparative example was purchased from Shandong Bote Precision Machinery Co., Ltd.
[0078] Comparative Example 4
[0079] The slider used for the linear guide in this comparative example was purchased from Germany and its signal number is R162132320 Rexroth linear guide slider.
[0080] Performance Testing
[0081] 1. Wear resistance: The sliders of each embodiment and each comparative example were subjected to wear resistance tests at a load of 50 kgf and 100 kgf and a walking speed of 1 m / s, respectively, and the test results are recorded in Table 1.
[0082] 2. Corrosion resistance: The sliders of each embodiment and each comparative example were corroded in an acidic corrosive solution with a pH value of 1 for 24 hours, and their weight loss rates were tested. The test results are recorded in Table 1.
[0083] Table 1 Performance test data of Examples 1-10 and Comparative Examples 1-4
[0084]
[0085] Referring to Table 1, in combination with Examples 1-3 and Comparative Examples 1-2, it can be seen that when the addition amount of each element in the formula is changed within an appropriate range, the obtained sliders have good wear resistance and corrosion resistance; but when the addition amount of Cr, Nb, Mo, W, Si, Mn, Ni and C elements is more or less, the wear resistance and corrosion resistance of the obtained sliders are reduced. Cr is selected as the main strengthening element. When the Cr content reaches a certain level, Cr and oxygen can form dense oxides to block the further occurrence of corrosion, thereby producing good corrosion resistance. Nb, as an added element, can expand the material's process characteristics and increase the material's high-temperature mechanical properties. If the content is too low, there will be no such characteristics, and if the content is too high, the brittleness and cost of the material will increase. Mo can refine the structure and improve the material's toughness. The addition of W can form WC particles with C in the material, greatly improving the material's wear resistance. Therefore, adding a small amount of W can significantly improve the material's performance. If too much W is added, it is easy to form a decarburized phase, which will greatly increase the material's brittleness. The addition of Si improves the alloy's smelting properties, but too much addition will bring about organizational defects such as pores. The addition of Mn can reduce the brittle phase produced by the S element in the material. The addition of Ni can improve the material's toughness, but too much Ni will lead to a decrease in wear resistance. Since C needs to form a large amount of C compounds with the alloy, high-carbon martensite is formed by heat treatment.
[0086] Referring to Table 1, combined with Examples 1, 4 and 5, it can be seen that adding an appropriate amount of Zr and Ti to the alloy material can further improve the corrosion resistance and wear resistance of the resulting slider. Zr can refine the structural organization of the slider, promote the formation of fine crystals, the growth of organizational grains, increase pinning dislocations, stabilize substructures, and improve the hardness and tensile strength of the slider. At the same time, Zr can also form FeZr3 phase with Fe to reduce the porosity of the alloy material; in addition, Zr can also form low-melting-point ZrTi with Ti to diffuse evenly in the organization, overlap each other to form a Zr-Ti skeleton with certain strength and plasticity, and other alloy particles fill the skeleton, further enhancing the toughness and density of the material, thereby improving the corrosion resistance and wear resistance of the slider.
[0087] Referring to Table 1, in combination with Examples 4, 6 and 7, it can be seen that adding an appropriate amount of bamboo charcoal and rutile nano-titanium dioxide to the alloy material can improve the wear resistance and corrosion resistance of the resulting slider. Bamboo charcoal has the advantages of good high temperature resistance, corrosion resistance, self-lubrication, etc., which can improve the corrosion resistance of the slider, but it itself has the defect of low mechanical strength, and rutile nano-titanium dioxide has a higher hardness, which can not only fill the internal pores of bamboo charcoal and improve the strength of bamboo charcoal, but also has a reinforcing effect on the wear resistance of the slider. Therefore, the corrosion resistance and wear resistance of the slider can be further improved by compounding bamboo charcoal and rutile nano-titanium dioxide.
[0088] Referring to Table 1 and combining with Examples 7-9, it can be seen that by changing the amount of adhesive added and the added ingredients and their ratios when preparing the slider, the resulting sliders all have excellent wear resistance and corrosion resistance. Among them, nickel-coated molybdenum disulfide is used as a lubricant to reduce the friction between the feed and the inner surface of the mold, increase the molding and demolding rates, and improve the preparation efficiency; polypropylene and high-density polyethylene are the skeleton components during feeding, which improve the strength of the injection molded green body; at the same time, by adding polyols, the fluidity of the binder system is better, debonding is easier, and the scrap rate of the resulting slider is reduced. The binder of the present application does not contain metal elements as a whole, and can be completely removed after degreasing without changing the composition and performance of the sintered product.
[0089] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A highly wear-resistant and corrosion-resistant slider for a linear guide rail, characterized in that: The invention is prepared according to the following raw material ratios: Cr: 14-20wt%, Si: 0.3-1.0wt%, Mn: 0.3-1.0wt%, Nb: 0.5-4.0wt%, Mo: 0.3-1.5wt%, W: 0.3-5.0wt%, Ni: 0.1-0.5wt%, P≤0.02wt%, S≤0.02wt%, C: 0.8-1.9wt%, other impurities content ≤0.01wt%, and the balance is Fe; and also includes 4-5wt% of an auxiliary agent, which is a mixture of bamboo charcoal powder and rutile nano titanium dioxide in a mass ratio of 2:(2-3).
2. The highly wear-resistant and corrosion-resistant slider for a linear guide rail according to claim 1, characterized in that: It also includes 0.4-0.7wt% Zr and 0.13-0.21wt% Ti.
3. A method for preparing a highly wear-resistant and corrosion-resistant slider for a linear guide rail according to any one of claims 1 to 2, characterized in that: The following steps are involved: S1, mixing: mixing the raw materials and the binder at a temperature of 160-190°C in a sealed environment and granulating to form feed; S2, injection molding: injecting the feed material into a mold to form a green body; S3, degreasing: degreasing the green body to form a brown body; S4, sintering: vacuum sintering the brown blank to form a sintered part; S5, forming: the sintered part is subjected to secondary processing to form a finished product; The binder is made of the following raw materials in parts by weight: 50-95 parts of polyoxymethylene, 2-15 parts of polypropylene, 2-15 parts of high-density polyethylene and 1-10 parts of nickel-coated molybdenum disulfide; the binder also includes 5-8 parts by weight of a polyol, which is one or more of trimethylolpropane, xylitol and sorbitol.
4. The method for preparing a highly wear-resistant and corrosion-resistant slider for a linear guide rail according to claim 3, characterized in that: In S1, the amount of the binder added is 4-12% of the total mass of the raw materials.
5. The method for preparing a highly wear-resistant and corrosion-resistant slider for a linear guide rail according to claim 3, characterized in that: In S4, the vacuum sintering is carried out in stages, including a low-temperature pre-sintering stage of 850-950°C, a medium-temperature heating sintering stage of 1000-1100°C, and a high-temperature insulation sintering stage of 1200-1300°C, and the vacuum degree is 3-5Pa.
6. The method for preparing a highly wear-resistant and corrosion-resistant slider for a linear guide rail according to claim 3, characterized in that: In S5, the secondary treatment includes shaping, heat treatment and surface treatment.
7. The method for preparing a highly wear-resistant and corrosion-resistant slider for a linear guide rail according to claim 3, characterized in that: The secondary treatment specifically includes placing the sintered part in Ar gas, rapidly heating it to 800-950° C., keeping it warm for 1-4 hours, and then placing the sintered part in a quenching medium for rapid cooling to obtain the final product.