A titanium / lanthanum co-doped diamond-like carbon coating and preparation method thereof

Through a diamond-like coating with titanium/lanthanum doping, the TiN transition layer and gradient layer are deposited using radio frequency magnetron sputtering technology, which solves the shortcomings of the existing coating in terms of wear resistance and internal stress, and achieves high hardness and low hardness Friction coefficient and excellent cutting life.

CN116288153BActive Publication Date: 2024-11-22SHANGHAI INST OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310322721.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-11-22
Estimated Expiration
2043-03-30

AI Technical Summary

Technical Problem

The existing diamond-like coatings have shortcomings in wear resistance, internal stress and film-based bonding, resulting in a short life of not long when cutting non-ferrous metals, and the internal stress and friction coefficient increased by doping elements are not ideal.

Method used

Using titanium/lanthanum co-doped diamond-like coating, the TiN transition layer and gradient power titanium/lanthanum co-doped diamond-like gradient layer are deposited through radio frequency magnetron sputtering technology, and the transition layer and gradient layer are designed to reduce internal stress and improve internal stress. The membrane-based binding force forms a TiN/(Ti,La)-DLC coating.

Benefits of technology

High hardness, low coefficient of friction, low internal stress and good chemical inertia are achieved, while improving the film-based bonding force, so that the tool can exhibit excellent cutting life when cutting non-ferrous metals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116288153B_ABST
    Figure CN116288153B_ABST
Patent Text Reader

Abstract

The present invention relates to a titanium / lanthanum co-doped diamond-like coating and a preparation method thereof. The diamond-like coating comprises a transition layer (2) and a gradient layer (3) on the surface of a substrate (1). The transition layer (2) is a TiN layer, and the gradient layer (3) is a gradient power titanium / lanthanum co-doped diamond-like layer; the gradient layer (3) comprises three gradient layers; the method comprises ion etching cleaning of the substrate (1), deposition of the transition layer (2) and deposition of the gradient layer (3); and pretreatment of the substrate (1) before ion etching cleaning of the substrate (1). Compared with the prior art, the present invention not only has the high hardness, low friction coefficient and good chemical inertness of the diamond-like coating, but also exhibits low internal stress, and adopts the design of the transition layer and the gradient layer to improve the film-base bonding force, and the tool coated with the coating exhibits excellent cutting life when cutting non-ferrous metals.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of surface modification and relates to a titanium / lanthanum co-doped diamond-like coating and a preparation method thereof. Background Art

[0002] With the continuous development of modern industry, the requirements for mechanical surface properties are gradually increasing. In order to adapt to different requirements such as high strength, high hardness, wear resistance, high temperature resistance, and corrosion resistance, various surface treatment technologies are usually used to process the surface of materials to make them suitable for various complex environments. At the same time, development concepts such as energy conservation and emission reduction, green environmental protection, etc. have also put forward higher requirements for the design and application of materials. Surface modification of metal materials can increase the life of parts, reduce wear, and improve economic benefits. Surface coating technology is a kind of material surface modification, which plays an important role in improving wear resistance, corrosion resistance, and antioxidant performance. Coating technology can usually be divided into chemical vapor deposition (CVD) and physical vapor deposition (PVD). Since the 1960s, CVD and PVD technologies have been widely used in the surface treatment of cutting tools, which has greatly improved the performance of various aspects of cutting tools, especially the life. At the same time, coating technology has broad application prospects in many aspects such as aerospace, intelligent manufacturing, and new composite materials.

[0003] Diamond-like carbon (DLC) coating, as an amorphous carbon film, has been widely used in many fields such as mechanics, electronics, optics, etc. due to its excellent tribological properties, high hardness, good chemical inertness, etc. However, at the same time, DLC coating also has the disadvantages of high internal stress and poor film-base bonding, which limits its application in many aspects.

[0004] Patent CN102925862A discloses a method for preparing a Ti-doped DLC coating, wherein a pre-treated substrate is placed on a rotating rack rod of an arc and magnetron sputtering composite coating device, a columnar arc Ti target is used as a Ti source, and a plane C target is used as a C source. There are three pairs of plane C targets, which are evenly distributed on the inner wall of the furnace body. High-purity Ar is used as the main ionizing gas to ensure an effective glow discharge process; high-purity N2 is used as a reaction gas to ionize it and combine it with Ti and C elements to deposit a Ti-doped DLC coating on the substrate surface. Although this patent adopts a preparation method of Ti-doped DLC, the dry friction coefficient of the coating is 0.2, and the wear resistance and friction reduction properties are relatively weak, and the doping of Ti increases the internal stress of the coating.

[0005] Patent CN110306153A discloses a method for preparing a Cr-doped DLC coating, which makes full use of the advantages of high-power pulsed magnetron sputtering film finish, uniformity, and high density, and adopts a bottom layer and transition layer design method to improve the shortcomings of poor adhesion and film toughness of the DLC coating. Although the patent adopts a gradient design, the sputtering power of each gradient coating is quite different, the coating thickness is 1.45μm, and the prepared diamond-like coating has a large internal stress.

[0006] Patent CN113913735A discloses a vanadium / yttrium co-doped DLC coating and a preparation method thereof, the preparation method comprising: first depositing a Cr or Ti base layer on a substrate, then depositing a CrC or TiC transition layer on the surface of the base layer, and then using vanadium and yttrium as doping metal sources to deposit a vanadium-yttrium co-doped DLC coating on the surface of the transition layer. Although the patent adopts a vanadium / yttrium co-doped DLC coating preparation method, the dry friction coefficient of the coating is 0.15, the wear resistance and friction reduction performance are relatively weak, and yttrium doping will cause the prepared coating to have a large internal stress due to the low charge density. Summary of the invention

[0007] The purpose of the present invention is to provide a titanium / lanthanum co-doped diamond-like coating and a preparation method thereof in order to overcome at least one defect of the above-mentioned prior art. The present invention not only has the high hardness, low friction coefficient and good chemical inertness of the diamond-like coating, but also exhibits low internal stress. The design of the transition layer and the gradient layer improves the film-base bonding strength. The tool coated with the coating exhibits excellent cutting life when cutting non-ferrous metals.

[0008] The purpose of the present invention can be achieved by the following technical solutions:

[0009] One of the technical solutions of the present invention is to provide a titanium / lanthanum co-doped diamond-like carbon coating, which includes a transition layer and a gradient layer on the surface of a substrate, wherein the transition layer is a TiN layer, and the gradient layer is a gradient power titanium / lanthanum co-doped diamond-like carbon (DLC) layer, which is deposited and prepared using radio frequency magnetron sputtering technology to finally form a TiN / (Ti,La)-DLC coating.

[0010] Furthermore, the thickness of the gradient layer is 3.2-3.5 μm.

[0011] Furthermore, the gradient layer includes three gradient layers, and the thickness of each gradient layer is 1.0 to 1.2 μm.

[0012] Furthermore, the thickness of the transition layer is 0.1-0.3 μm.

[0013] One of the technical solutions of the present invention is to provide a method for preparing a titanium / lanthanum co-doped diamond-like carbon coating, the method comprising the following steps:

[0014] S1. Matrix ion etching cleaning: Place the matrix into a vacuum chamber, introduce ionized gas, clean the matrix, remove the oxide scale on the matrix surface, and activate the matrix surface;

[0015] S2. Transition layer deposition: the cleaned substrate is placed on the rotating rack fixture of the magnetron sputtering equipment chamber, the reaction gas is introduced, the ionized gas flux remains unchanged, the Ti target is turned on, and the Ti target is used as one of the Ti element sources to deposit the transition layer;

[0016] S3. Gradient layer deposition: After the transition layer deposition is completed, turn off the reaction gas, increase the ionized gas flux, turn on the graphite target and LaTi target, use the graphite target as the source of the C element, use the LaTi target as the doping source, maintain the graphite target power, and perform multi-layer gradient deposition of the gradient layer with different LaTi target powers.

[0017] Furthermore, the substrate is pretreated before step S1, and the specific steps are: degreasing and polishing the surface of the substrate, ultrasonic cleaning, and finally drying.

[0018] Furthermore, the ultrasonic cleaning is carried out in ethanol or acetone, and water in sequence, with a frequency of 30 to 40 kHz and a time of 10 to 15 minutes;

[0019] The drying gas is nitrogen or dry air.

[0020] Further, in step S1, the substrate is a cemented carbide or a metal ceramic;

[0021] The vacuum degree is 0.25-0.50Pa, the ionized gas is argon, to ensure the glow discharge process, the flow rate is 200-220sccm;

[0022] The ionization voltage is 800 to 1100 V, the substrate bias is -1000 to -900 V, and the cleaning time is 20 to 25 minutes.

[0023] Furthermore, in step S2, the rotating rack has a rotation speed of 5 to 10 r / min to ensure uniformity of the coating;

[0024] The gas pressure is 0.5-0.6 Pa, the reaction gas is nitrogen, and the flow rate is 120-130 sccm;

[0025] The Ti target power is 100-110 W, and the deposition time is 25-30 min.

[0026] Furthermore, in step S3, the LaTi target is La 0.03 Ti 0.97Target, La:Ti atomic ratio is 3:97;

[0027] The gas pressure is 0.5-0.6 Pa, the ionized gas is argon, and the flow rate is 240-260 sccm;

[0028] The power of graphite target is 120~125W;

[0029] The first LaTi target power is 20-25W, and the deposition time is 2.0-2.2h;

[0030] The second LaTi target power is 40-45W, and the deposition time is 2.0-2.2h;

[0031] The third LaTi target power was 60-65W, and the deposition time was 2.0-2.2h.

[0032] The method adopts a TiN transition layer and a gradient La / Ti co-doped DLC coating design with different powers, so that the difference in thermal expansion coefficient between the coating and the substrate and between the layers is reduced, thereby reducing the internal stress of the coating and improving the film-substrate bonding strength.

[0033] Trace amounts of La and Ti doping can change the degree of carbon network cross-linking inside the coating and inhibit sp 2 The formation of -C bonds reduces the surface roughness of the coating and forms a very smooth surface.

[0034] The doped trace La element exists in the form of nanocrystals, which releases the internal stress caused by the distortion of bond length and bond angle through intracrystalline dislocation movement, and at the same time pins the C atoms at the nanocrystal grain boundaries, so that the coating has almost no change in hardness while greatly reducing the internal stress.

[0035] Compared with the prior art, the present invention has the following advantages:

[0036] (1) The present invention uses a titanium / lanthanum co-doped diamond-like coating with high hardness, chemical inertness and good tribological properties;

[0037] (2) The doping of the rare earth element lanthanum in the present invention greatly reduces the residual internal stress of the coating;

[0038] (3) The present invention adopts the design of transition layer and gradient layer to improve the bonding strength between the coating and the substrate, so that the tool exhibits excellent cutting life when cutting non-ferrous metals. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 Schematic diagram of the structure of the titanium / lanthanum co-doped diamond-like carbon coating in an embodiment of the present invention;

[0040] Figure 2This is a graph showing the internal stress test results of the titanium / lanthanum co-doped diamond-like carbon coating in an embodiment of the present invention;

[0041] Figure 3 This is a graph showing the hardness test results of the titanium / lanthanum co-doped diamond-like carbon coating in an embodiment of the present invention;

[0042] Figure 4 This is a graph showing the film-substrate bonding strength test results of the titanium / lanthanum co-doped diamond-like carbon coating in an embodiment of the present invention;

[0043] Figure 5 This is a graph showing the test results of the friction coefficient of the titanium / lanthanum co-doped diamond-like carbon coating in an embodiment of the present invention;

[0044] Figure 6 This is a test result diagram of the cutting distance of a cutting tool using a titanium / lanthanum co-doped diamond-like carbon coating in an embodiment of the present invention.

[0045] Description of the markings in the figure:

[0046] 1—matrix, 2—transition layer, 3—gradient layer. DETAILED DESCRIPTION

[0047] The present invention is described in detail below in conjunction with specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and a specific operation process, but the protection scope of the present invention is not limited to the following embodiments.

[0048] Unless otherwise specified, the equipment used in the following examples are all conventional equipment in the art; the reagents used are all commercially available products or prepared by conventional methods in the art unless otherwise specified. Anything not described in detail in the following examples can be achieved by conventional experimental means in the art.

[0049] Example:

[0050] A titanium / lanthanum co-doped diamond-like carbon coating, such as Figure 1 As shown, a TiN transition layer 2 and a gradient power titanium / lanthanum co-doped diamond-like carbon (DLC) gradient layer 3, i.e., a TiN / (Ti,La)-DLC coating, are sequentially deposited on the surface of a substrate 1 by using radio frequency magnetron sputtering technology. The thickness of the transition layer 2 is 0.2 μm, the thickness of the gradient layer 3 is 3.3 μm, and the thickness of each gradient layer is 1.1 μm.

[0051] A method for preparing a titanium / lanthanum co-doped diamond-like carbon coating, the specific steps are as follows:

[0052] (1) Pretreatment of substrate 1: A cemented carbide substrate with a size of 25×25×4 mm was used as substrate 1. After degreasing and polishing, the substrate 1 was ultrasonically cleaned in ethanol (concentration of 95%) and deionized water at 30 kHz for 10 min, and finally dried with nitrogen (purity of 99.99%).

[0053] (2) Ion etching cleaning of substrate 1: Place substrate 1 into a vacuum chamber with a vacuum degree of 0.25 Pa, introduce ionized gas argon (purity of 99.99%), ensure glow discharge process, argon flow rate of 200 sccm, argon ion ionization voltage of 1000 V, substrate 1 bias voltage of -900 V, clean substrate 1, remove oxide scale on the surface of substrate 1, activate the surface of substrate 1, and continue for 20 min;

[0054] (3) Deposition of transition layer 2: The surface treated substrate 1 is placed on the rotating rack fixture of the magnetron sputtering equipment chamber. The rotating rack rotates at 5 r / min to ensure the uniformity of the coating. The pressure in the furnace chamber is set to 0.5 Pa. Nitrogen gas is introduced as a reaction gas with a nitrogen flow rate of 120 sccm. The argon flow rate remains unchanged. The Ti target (purity of 99.9%) is turned on. A cylindrical Ti target is used as one of the Ti element sources. The Ti target power is 100 W. The TiN layer is prepared for 25 min.

[0055] (4) Deposition of gradient layer 3: After the preparation of transition layer 2, turn off nitrogen, increase the flux of ionized gas, and set the argon flow rate to 240 sccm. Ensure that the pressure in the furnace is 0.5 Pa, turn on the graphite target (purity is 99.99%) and La 0.03 Ti 0.97 target (La:Ti atomic ratio is 3:97), with cylindrical graphite target as the source of C element, and cylindrical La 0.03 Ti 0.97 The target is used as the doping source, and the graphite target power is kept at 120W, La 0.03 Ti 0.97 The target power was maintained at 20 W, the deposition time was 2.0 h, and La 0.03 Ti 0.97 The target power was maintained at 40W, the deposition time was 2.0h, and La 0.03 Ti 0.97 The target power was 60 W, the deposition time was 2.0 h, and La / Ti co-doped DLC coatings were prepared by multi-layer gradient with different LaTi target powers.

[0056] An internal stress test of a titanium / lanthanum co-doped diamond-like carbon coating, the specific steps are as follows:

[0057] The internal stress of the coating is calculated by the curvature method and the Stonely formula. The calculation formula is:

[0058]

[0059] Where: E s is the Young's modulus of matrix 1, v s is the Poisson's ratio of matrix 1, t s is the thickness of substrate 1, t c is the thickness of the coating, R0 is the radius of curvature of the sample before coating, and R is the radius of curvature of the sample after coating. The radius of curvature of the sample before and after coating were measured by a surface profiler (FORM TALYSURF200).

[0060] like Figure 2 As shown, after three measurements and calculations, the lowest internal stress of the coating can be 0.6 GPa, and the average internal stress of the coating is 0.7 GPa.

[0061] A hardness test of a titanium / lanthanum co-doped diamond-like carbon coating, the specific steps are as follows:

[0062] The test is carried out by the continuous stiffness test method (CSM). A certain pressure is applied to the surface of the sample, and then released after a specified time. The coating hardness is obtained by the nanoindenter (MTS-Nano IndenterⅡ). The indentation load is set to 15mN, the thermal drift rate is 0.05nm / s, and the load holding time is 5s. To ensure the accuracy of the measurement results, the maximum indentation depth should be within 1 / 10 of the coating thickness.

[0063] like Figure 3 As shown, the arithmetic average value was taken after five measurements, and the final hardness of the coating was measured to be 27.05 GPa.

[0064] A film-substrate bonding test of a titanium / lanthanum co-doped diamond-like carbon coating, the specific steps are as follows:

[0065] Through the scratch method, the coated substrate is first fixed, and then a stylus with a smooth cone tip is used to scratch at a speed of 2mm / s, with the stylus perpendicular to the coating surface. The pressure on the stylus is gradually increased at 20N / min, the maximum pressure is 100N, and the sliding distance is 4mm, so that cracks appear in the coating. At this time, the minimum force applied is the film-substrate bonding force of the coating.

[0066] like Figure 4 As shown, the maximum film-base bonding strength of the coating measured in three tests is 65N, and the average value of the film-base bonding strength of the coating is 61.67N.

[0067] The friction coefficient test of a titanium / lanthanum co-doped diamond-like carbon coating is carried out in the following steps:

[0068] A friction tester (UMT-3) was used to conduct a reciprocating friction test. The friction pair was selected to be a zirconia ceramic bead with a diameter of 8 mm, a load of 10 N, a reciprocating linear motion of 0.2 m / s, a reciprocating motion amplitude of 10 mm, and a friction condition of 40% atmospheric humidity. During the experiment, the coating sample was fixed on the test bench, and the friction pair was made to reciprocate on the coating surface. The real-time friction force of the coating surface was measured by the sensor in the friction tester, and the friction coefficient can be estimated by the ratio of friction force to normal pressure.

[0069] like Figure 5 As shown, the minimum friction coefficient of the coating measured in three tests can reach 0.1, and the average friction coefficient is 0.12.

[0070] A titanium / lanthanum co-doped diamond-like carbon coating was applied to the cutting distance test of the tool. The specific steps are as follows:

[0071] Through cutting experiments, using VMC-100Ⅱ machine tool as the carrier, 2A50 aluminum alloy as the cutting material, and dry cutting, the tool life is calculated by the length of the tool on the aluminum alloy surface. The cutting parameters are: feed rate a f is 0.05mm, the axis speed n is 3980rev / min, and the back cutting depth a p is 2mm.

[0072] like Figure 6 As shown, the average value of three tests was taken, and the experimentally measured cutting distance was 210m.

[0073] Under the above process conditions, a titanium / lanthanum co-doped diamond-like coating can be obtained. It has been determined that the titanium / lanthanum co-doped diamond-like coating prepared by the method of this embodiment has a smooth and dense surface, an internal stress of 0.7 GPa, a coating hardness of 27.05 GPa, a film-base bonding force of 61.67 N, a friction coefficient of 0.12 when the friction pair is zirconium oxide, and a cutting distance of 210 m when cutting 2A50 aluminum alloy. This shows that the titanium / lanthanum co-doped diamond-like coating has good wear resistance and friction reduction properties, high hardness, low internal stress, and high film-base bonding force.

[0074] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. A titanium / lanthanum co-doped diamond-like carbon coating, characterized in that: The diamond-like coating comprises a transition layer (2) and a gradient layer (3) on the surface of a substrate (1), wherein the transition layer (2) is a TiN layer, and the gradient layer (3) is a gradient power titanium / lanthanum co-doped diamond-like layer; During the deposition of the transition layer (2), the reaction gas is nitrogen, and the Ti target is used as the source of the titanium element. During the deposition of the gradient layer (3), an ionized gas is introduced, and the graphite target is used as the source of the carbon element, and the LaTi target is used as the doping source. The power of the graphite target is maintained, and the power of the LaTi target is increased. The gradient layer (3) is deposited in multiple layers. LaTi target is La 0.03 Ti 0.97 Target, La:Ti atomic ratio is 3:97; The gas pressure is 0.5~0.6 Pa, the ionized gas is argon, and the flow rate is 240~260 sccm; The power of graphite target is 120~125 W; The first LaTi target power was 20-25 W, and the deposition time was 2.0-2.2 h; The second LaTi target power was 40-45 W, and the deposition time was 2.0-2.2 h; The third LaTi target power was 60~65 W, and the deposition time was 2.0~2.2 h.

2. A titanium / lanthanum co-doped diamond-like carbon coating according to claim 1, characterized in that: The gradient layer (3) has a thickness of 3.2-3.5 μm.

3. The titanium / lanthanum co-doped diamond-like carbon coating according to claim 1, characterized in that: The gradient layer (3) comprises three gradient layers, and the thickness of each gradient layer is 1.0-1.2 μm.

4. The titanium / lanthanum co-doped diamond-like carbon coating according to claim 1, characterized in that: The transition layer (2) has a thickness of 0.1-0.3 μm.

5. A method for preparing a titanium / lanthanum co-doped diamond-like carbon coating according to any one of claims 1 to 4, characterized in that: The method comprises the following steps: S1. Ion etching and cleaning of the substrate (1): placing the substrate (1) into a vacuum chamber, introducing ionized gas, and cleaning the substrate (1); S2. Deposition of transition layer (2): Place the cleaned substrate (1) on the rotating rack fixture of the magnetron sputtering equipment chamber, introduce the reaction gas, keep the ionized gas flux constant, turn on the Ti target, and deposit the transition layer (2); S3. Deposition of gradient layer (3): After the transition layer (2) is deposited, the reaction gas is turned off, the flux of the ionized gas is increased, the graphite target and the LaTi target are turned on, the graphite target power is maintained, and the gradient layer (3) is deposited in multiple layers with different LaTi target powers.

6. The method for preparing a titanium / lanthanum co-doped diamond-like carbon coating according to claim 5, characterized in that: Step S1 is to pre-treat the substrate (1), and the specific steps are: degreasing and polishing the surface of the substrate (1), ultrasonic cleaning, and finally drying.

7. The method for preparing a titanium / lanthanum co-doped diamond-like carbon coating according to claim 6, characterized in that: The ultrasonic cleaning is carried out in ethanol or acetone, and water, at a frequency of 30-40 kHz and for 10-15 min. The drying gas is nitrogen or dry air.

8. The method for preparing a titanium / lanthanum co-doped diamond-like carbon coating according to claim 5, characterized in that: In step S1, the substrate (1) is a cemented carbide or a metal ceramic; The vacuum degree is 0.25~0.50 Pa, the ionized gas is argon, and the flow rate is 200~220 sccm; The ionization voltage is 800~1100 V, the substrate (1) bias is -1000~-900 V, and the cleaning time is 20~25 min.

9. The method for preparing a titanium / lanthanum co-doped diamond-like carbon coating according to claim 5, characterized in that: In step S2, the rotating rack has a rotation speed of 5-10 r / min; The gas pressure is 0.5~0.6 Pa, the reaction gas is nitrogen, and the flow rate is 120~130 sccm; The Ti target power is 100~110 W, and the deposition time is 25~30 min.