Copper paste suitable for three-dimensional configuration, preparation method and application

By using surface-coated organic ligand and prereaction crosslinking in copper slurry, the problem of insufficient viscosity and agglomeration of copper slurry in three-dimensional configuration printing is solved, and efficient preparation of three-dimensional configuration structures and reducing costs are achieved. effect.

CN116313225BActive Publication Date: 2024-11-22ENOVATE3D (HANGZHOU) TECH DEV CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310501981.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-06
Publication Date
2024-11-22
Estimated Expiration
2043-05-06

AI Technical Summary

Technical Problem

The prior art cannot effectively prepare a three-dimensional configuration with a high aspect ratio, and copper slurry has problems such as insufficient viscosity, agglomeration problems and high costs in three-dimensional configuration printing, making it difficult to achieve large-scale application.

Method used

Copper paste composed of copper powder, matrix resin, curing agent, reactive diluent, dispersant and thixotropic additives is used to improve viscosity and dispersion and reduce the risk of agglomeration by covering organic ligands on the surface and cross-linking with pre-reactions. , and purified using an alcohol solvent to protect the organic ligands to form a copper slurry with high crosslinking.

Benefits of technology

It realizes smooth extrusion and long-term printing of high-solid content copper slurry, ensures the stability of the three-dimensional configuration structure and high specific surface area, reduces material costs, and improves printing efficiency and product conformal performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116313225B_ABST
    Figure CN116313225B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of conductive paste, and in particular to a copper paste suitable for three-dimensional configuration, a preparation method and an application thereof, wherein the copper paste suitable for three-dimensional configuration comprises copper powder and an organic carrier cross-linked with the copper powder; the copper powder surface is loaded with an organic ligand; the organic carrier comprises a matrix resin for cross-linking with the organic ligand, an active diluent and a curing agent; and further comprises a dispersant, a thixotropic agent and an adhesion promoter. The present invention controls the morphology of copper particles, and adjusts the cross-linking mode and ratio of the organic carrier and the copper particles. The paste is not easy to collapse during the sintering process, can meet the printing of line widths below 100 μm, and realizes the printing of laminated three-dimensional structures with an aspect ratio ≥ 0.5.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of conductive paste, and in particular to a copper paste suitable for three-dimensional configuration, a preparation method and application thereof. Background Art

[0002] At present, manufacturing technologies such as electroplating or chemical plating technology, printing technology, molding technology, embossing technology and transfer technology cannot produce three-dimensional structures with high aspect ratios. Printing technology and materials are difficult to achieve mass production of flexible metal grid electrodes with high aspect ratios, and the manufacturing efficiency is low; inkjet printing technology is limited by material viscosity and is difficult to manufacture high-performance and high-conformal three-dimensional structures; inkjet printing is difficult to achieve the printing of high-metal content and high-aspect ratio micro-nano structures. Although the combination of nanoimprinting and scraping can achieve the manufacture of metal grids, which has the advantage of high efficiency, the equipment is expensive, and the metal content, surface tension, sintering temperature and other requirements of nano-conductive ink are high. Fixed molds need to be made during preparation, which limits the shape of the three-dimensional structure. At the same time, its complex process, high material consumption and environmental pollution make it impossible to further large-scale application. In summary, low-cost and mass-produced manufacturing technology for three-dimensional structures is still difficult to achieve.

[0003] Silver nanomaterials are currently used to make conductive pastes. However, when silver paste is used as an electrode, silver ions can easily jump from the anode to the cathode due to electromigration, which eventually leads to a short circuit in the electrode. Therefore, the market is looking for a conductive ink that does not have an electron transition effect. Since copper-based materials themselves have low anode solubility and high electromigration activation energy, copper is the best choice for electrode conductive inks. In addition, the conductivity of copper is similar to that of silver, and the raw material cost of copper is only about 1 / 100 of that of silver.

[0004] There are also certain conductive pastes using metal particles as raw materials in the prior art, such as:

[0005] (1) CN104341860A discloses a formula of nano-conductive ink. The conductive copper ink can be sintered at low temperature to have good conductivity. However, due to its low viscosity, it is only suitable for inkjet printing process to be processed into a planar structure. Its linear aspect ratio is low and it cannot print three-dimensional structures.

[0006] (2) CN 110570972 A discloses a conductive paste for use in a metal mesh transparent conductive film and a preparation method thereof. The paste has extremely strong antioxidant and acid, alkali and salt resistance, and can effectively improve the stability and service life of the metal mesh transparent conductive film. However, the paste can only be used for coating by a stamping process to prepare a flexible transparent conductive film, and cannot realize the printing of a three-dimensional structure.

[0007] (3) CN 114864133 A discloses an ultra-low temperature curing silver paste for flexible transparent metal grids, which can achieve excellent grid filling, printability, adhesion, weather resistance and other properties under ultra-low curing temperature and shorter curing time conditions. However, its particle size is large, and it uses more expensive silver as a raw material, and it requires the use of a mold, which limits its large-scale application.

[0008] Therefore, developing a copper paste suitable for high-precision direct writing 3D printing of metal grids can reduce costs, have good conformal properties and a wide range of application scenarios, and can be used to prepare metal grids with high conductivity and high specific surface area on a large area. Summary of the invention

[0009] The present invention aims to overcome the defect that the copper paste in the prior art is not suitable for printing three-dimensional structures, and provides a copper paste suitable for three-dimensional structures, a preparation method and an application to overcome the above defect.

[0010] In order to achieve the above-mentioned purpose, the present invention adopts the following technical solutions:

[0011] In the first aspect, the present invention first proposes a copper paste suitable for three-dimensional configuration, which is composed of the following components by weight percentage: 70-90% copper powder, 2-10% base resin, 0.02-4% curing agent, 0.5-5% active diluent, 2-10% dispersant, 0.6-10% thixotropic additive, and 0.02-2% adhesion promoter;

[0012] The surface of the copper powder is coated with an organic ligand;

[0013] The copper powder is pre-reacted and cross-linked with the matrix resin, the active diluent and the curing agent.

[0014] The conductive paste prepared in the prior art is mainly used in the printing of planar structures. In order to achieve a smooth discharge effect, it is usually necessary to reduce the solid content of the conductive paste, thereby reducing its viscosity. However, this type of low-viscosity conductive paste is prone to leveling and cannot meet the requirements of high conformality. Therefore, it cannot meet the printing of three-dimensional structures with several layers stacked.

[0015] In the prior art, in order to meet the printing requirements of three-dimensional structures, the solid content of the conductive paste is often increased. However, as the solid content increases, although the viscosity increases, which is beneficial to the printing of three-dimensional structures, the agglomeration problem of the substances inside the paste will also be significantly aggravated. The material cannot be extruded smoothly during the printing process. During long-term printing, the agglomerates in the paste are likely to clog the needle, resulting in the inability to achieve large-scale mass production.

[0016] Therefore, in order to achieve smooth extrusion of conductive paste with high solid content, some existing technologies adopt the method of adding diluents to the conductive paste to reduce the viscosity. However, common diluents often significantly reduce the thixotropic index while reducing the viscosity of the material, resulting in a corresponding decrease in the conformal performance of the material.

[0017] In order to address the above-mentioned problems existing in the prior art, the present application adopts a special control method so that the conductive copper paste still has good extrusion performance under the conditions of having a high solid content and satisfying the printing of a three-dimensional structure.

[0018] In view of the problem of agglomeration that is easy to occur in copper paste with high solid content, the present invention has made certain improvements in the selection of raw materials and the implementation of the process.

[0019] (1) Regarding the selection of raw materials: The metal powders selected and used in the metal slurry described in the prior art are all commercially available surface-treated metal powders. The surface ligands of these metal particles are mostly completely removed, and most of them will be unevenly dispersed after adding the organic carrier. The copper powder selected and used in the present invention has an organic ligand on its surface. Due to the presence of organic ligands between copper powder particles, there is a certain repulsive force between adjacent copper powder particles. Therefore, after the copper powder particles in the present invention are added to the organic carrier, they will repel and separate from each other to achieve the purpose of automatic dispersion. At the same time, due to the presence of organic ligands, its compatibility with the organic carrier is greatly improved, thereby reducing the possibility of precipitation from the organic carrier. The presence of organic ligands can also react with the organic carrier during the curing process, thereby causing a cross-linking reaction, so that after curing and sintering, its shrinkage rate is lower and its shape retention is better.

[0020] (2) Regarding the implementation of the process: The conductive paste in the prior art usually adds metal powder (such as copper powder and silver powder) directly into the organic carrier. Therefore, before the paste is solidified, there will be no chemical reaction between the metal powder and the organic carrier. Therefore, the conductive paste in the prior art has the problem that the viscosity cannot be further increased because there is no correlation between the components. In addition, since there is no correlation between the components, during long-term storage, the components may also settle and agglomerate due to the influence of gravity.

[0021] In the present invention, the copper powder has already undergone a cross-linking reaction with the organic carrier before the paste is cured, so that the copper powder in the conductive paste of the present invention has already cross-linked with the organic carrier to form a three-dimensional network structure, thereby effectively improving the viscosity and shape retention of the paste. At the same time, since the copper powder and the organic carrier in the present application are cross-linked by chemical bonding, the copper powder with a higher density and the organic carrier will form an integrated structure, so the conductive paste in the present application is more stable, so even after a long period of storage, there will be no sedimentation and agglomeration.

[0022] Secondly, it has been made clear in the above discussion that the solid content of the conductive paste can be increased and the agglomeration of copper powder can be reduced through selective adjustment of raw materials and processes. Therefore, the conductive paste in the present invention will not be blocked during the printing process even under conditions of a higher solid content, which is conducive to a long printing process and large-scale mass production.

[0023] In the existing slurry, low-boiling point organic solvents generally account for a high proportion, which is prone to linear shrinkage and slurry leveling problems after heating during the sintering process, resulting in cracks and even collapse of the three-dimensional structure during the sintering process. The low-volatile solvent content in the system of the present invention is low, so during the curing process, the shrinkage rate of the circuit is lower and its shape retention is better.

[0024] Preferably, the preparation method of the copper powder is as follows:

[0025] (1) adding a solution containing an organic ligand and a copper salt dropwise into a solution containing a reducing agent, so that the copper salt is reduced, thereby preparing copper particles with the organic ligand coated on the surface;

[0026] (2) The prepared copper particles are washed with an alcohol solvent at 40-60° C., and the copper powder is obtained after washing.

[0027] The method of the present invention can prepare copper particles with small and uniform particle size. At the same time, the inventors of the present application found in experiments that after the copper particles are prepared, in the subsequent purification process of the copper particles, the solvent used in the purification and the temperature used in the purification have an important influence on the organic ligands on the surface of the copper particles.

[0028] The applicant found that after the synthesis of copper particles is completed, the components in the system can be divided into three parts: copper particles-organic ligand complexes, reaction solvents and impurities; among them, impurities include reaction by-products, unreacted precursors, and free organic ligands. These impurities have a significant effect on the conductivity and adhesion after sintering. Therefore, in some documents, nano copper particles are also cleaned and purified after they are prepared. However, in the prior art, the purification step for nano copper particles is usually to use some highly polar solvents (such as water) to clean them. Although these highly polar solvents can remove free ligands that are not bound to nano copper particles, they will also cause the ligands bound to the surface of nano copper particles to fall off. As a result, during the purification and subsequent treatment process, the ligands on the surface of nano copper particles are missing, and the copper element on the surface of nano copper particles is exposed. Therefore, electrostatic adsorption is prone to occur between particles, inducing local agglomeration problems. At the same time, the copper atoms exposed on the surface are also easily oxidized or hydrolyzed, which ultimately affects the uniformity and stability of the particle dispersion of the slurry itself, and is prone to cause needle clogging problems during 3D printing, which is not suitable for 3D printing processes.

[0029] In the present invention, by selecting and using alcohol solvents and controlling the temperature during the purification process, the impurity components doped in the copper particles can be effectively dissolved and removed. The organic ligands loaded on the surface of the copper powder through chemical bonds cannot be removed under the conditions disclosed in the present application, thereby protecting the ligands on the surface of the particles from falling off. This ensures the retention rate of the organic ligands on the surface of the copper particles, thereby effectively improving the antioxidant properties of the copper powder and effectively improving the compatibility with the organic carrier, thereby avoiding subsequent agglomeration of the copper powder, which leads to easy blockage during the printing process.

[0030] Preferably, the copper salt is any one of copper sulfate pentahydrate, copper hydroxide, copper nitrate, copper formate, copper acetate monohydrate, and copper chloride, or any combination of any two or more thereof.

[0031] Preferably, the reducing agent is any one of hypophosphorous acid, ascorbic acid, sodium hypophosphite, sodium borohydride, hydrazine hydrate, and citric acid, or any combination of multiple thereof.

[0032] Preferably, the organic ligand is any one of polyacrylic acid, polyethylene glycol polyvinyl pyrrolidone, polyvinyl alcohol, Tween, and span, or any combination of any two or more thereof.

[0033] Preferably, the reduction temperature in step (1) is 50-80°C.

[0034] Preferably, the base resin is any one of bisphenol A epoxy resin, bisphenol F epoxy resin, mixed epoxy resin, polyurethane resin, EVA, polyester resin, silicone resin, acrylic resin, or any combination of multiple thereof.

[0035] More preferably, the base resin selected for use in the present invention is a mixed epoxy resin having both alicyclic epoxy groups and glycidyl ester groups.

[0036] In the present invention, the matrix resin is selected from a highly active mixed epoxy resin that takes into account the dual characteristics of alicyclic epoxy and glycidyl ester, which has the characteristics of high temperature resistance and can ensure the advantages of low circuit shrinkage and good shape retention during high temperature curing, i.e., sintering. At the same time, the mixed epoxy resin can increase the crosslinking degree of the copper paste, and the heat curing does not affect the shape retention of the copper paste, and the addition of an active diluent can be used to adjust and obtain a copper paste with low viscosity, high crosslinking degree, and low shrinkage.

[0037] Preferably, the curing agent is any one of EP-500, methyltetrahydrophthalic anhydride, dicyandiamide, 2-ethyl-4-methylimidazole, mercaptan, 2-phenylimidazole, isocyanate, and boron amine complex, or any combination of multiple thereof.

[0038] Preferably, the active diluent is any one of butyl glycidyl ether, ethylene glycol diglycidyl ether, phenyl glycidyl ether, o-cresyl glycidyl ether, or any combination of multiple thereof.

[0039] Preferably, the dispersant is any one of ethylene glycol ethyl ether acetate, dibasic acid ester, ethylene glycol monomethyl ether, n-butanol, diethylene glycol butyl ether, butyl carbitol acetate, dodecyl alcohol ester, dipropylene glycol methyl ether acetate, glycerol, isopropanol, and ethylene glycol, or any combination of any two or more thereof.

[0040] Preferably, the thixotropic agent is any one or a combination of any two or more of ethyl cellulose, fumed silica, tributyl citrate, polyamide wax, hydrogenated castor oil or hydroxyethyl cellulose.

[0041] Preferably, the adhesion promoter is any one of a silane coupling agent and a titanate coupling agent, or any combination of multiple thereof.

[0042] In a second aspect, the present invention also provides a method for preparing the copper slurry, comprising the following steps:

[0043] (S.1) Under the protection of an inert gas, copper powder, a matrix resin, a curing agent, a reactive diluent, and a dispersant are heated and stirred to allow the copper powder to pre-react and cross-link with the organic carrier to obtain a mixed slurry;

[0044] (S.2) adding a rheological additive and an adhesion promoter to the mixed slurry, mixing the slurry so that the copper powder and the organic carrier are evenly dispersed to obtain a copper slurry with a high degree of crosslinking;

[0045] (S.3) Grinding and filtering the copper paste with a high degree of cross-linking to obtain the copper paste suitable for three-dimensional configuration.

[0046] As described above, the conductive copper paste in the prior art can be obtained only by uniformly mixing copper powder and an organic carrier. However, since the copper paste prepared by this method is only physically mixed with the organic carrier, under long-term storage conditions, the copper powder is easily deposited to the bottom of the paste due to the large difference between its own density and that of the organic carrier, thereby further agglomerating at the bottom of the paste, which is not conducive to the subsequent printing process.

[0047] The conductive paste of the present invention is not just physically blended with the copper powder and the organic carrier. During mixing, the organic ligand on the surface of the copper powder can react with the matrix resin and the reactive diluent in the organic carrier, thereby connecting the copper powder and the organic carrier by chemical bonding. In this way, the storage stability of the conductive paste can be greatly improved. At the same time, since each copper powder particle is fixed by the organic carrier, there will be no migration and agglomeration between the copper powders during this process, so there will be no material blocking during the 3D printing process, thereby maintaining a smoother printing process while ensuring a high solid content. The conductive paste finally obtained can meet the printing of a three-dimensional structure with several layers stacked, and realize a printing process with a large aspect ratio.

[0048] Preferably, the pre-reaction cross-linking temperature in step (S.1) is 45 to 80° C., and the pre-reaction cross-linking time is 5 to 15 minutes.

[0049] In the present invention, certain restrictions are imposed on the cross-linking temperature and cross-linking time of step (S.1), the purpose of which is to limit the degree of polymerization of the overall slurry. When the degree of polymerization is too high during step (S.1), the viscosity of the overall slurry will increase significantly, which is not conducive to the final printing process. When the degree of polymerization is low, the copper powder and the organic carrier cannot form a perfect connection, which makes it easy for the copper powder to detach from the organic carrier, thereby causing a significant decrease in storage stability.

[0050] In a third aspect, the present invention also provides an application of the copper paste in 3D printing of a three-dimensional metal grid with a large aspect ratio.

[0051] The present invention has the following beneficial effects:

[0052] (1) The particle size is relatively uniform: The copper powder particle size is 0.1-1 μm, which is a small spherical particle and can achieve precision printing below 100 μm.

[0053] (2) High conformality: The metal copper grid can be stacked up to at least eight layers without collapse, with a height of 200 to 270 μm, achieving a large aspect ratio and high specific surface area. It can be used for high-precision direct writing 3D printing and has a wide range of application scenarios.

[0054] (3) High adhesion: The adhesion of the test piece is 4-5B.

[0055] (4) Low price: Considering that the price of copper material is about 1 / 100 of that of silver, copper paste can effectively reduce the paste cost without reducing the overall conductivity of the material. BRIEF DESCRIPTION OF THE DRAWINGS

[0056] Figure 1 This is the SEM image of copper powder (A-2) particles.

[0057] Figure 2 This is the SEM image of copper powder (A-5) particles.

[0058] Figure 3 This is the SEM image of copper powder (A-11) particles.

[0059] Figure 4 SEM image of copper powder (B) particles.

[0060] Figure 5 SEM image of copper powder (C) particles.

[0061] Figure 6 This is a diagram of the three-dimensional configuration printing process.

[0062] Figure 7 The three-dimensional configuration diagram is printed for the copper paste of Example 1.

[0063] Figure 8 The three-dimensional configuration diagram of the copper paste printed in comparative example 5.

[0064] Fig. 9 Comparative Example 10: Copper paste printing three-dimensional configuration diagram.

[0065] Fig.10 Comparative Example 11: Copper paste printing three-dimensional configuration diagram. DETAILED DESCRIPTION

[0066] The present invention is further described below in conjunction with specific embodiments. Those of ordinary skill in the art will be able to implement the present invention based on these descriptions. In addition, the embodiments of the present invention involved in the following description are generally only embodiments of a part of the present invention, rather than all embodiments. Therefore, based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work should fall within the scope of protection of the present invention.

[0067]

Preparation of copper powder

[0068] Preparation method of copper powder (A-1):

[0069] (1) Weigh 20 g of hypophosphorous acid and mix it with 20 g of deionized water to form a uniform solution;

[0070] (2) Weigh 15 g of copper sulfate pentahydrate, dissolve it in 40 g of deionized water, and then add 10 g of PVP to dissolve and mix well to form a solution;

[0071] (3) The solution in (2) was added dropwise to the solution in (1), and stirred at 50° C. for 2 h to form a reddish brown solution;

[0072] (4) Cool to room temperature and centrifuge at 7000 r / min;

[0073] (5) Discard the supernatant, add 100 ml of ethanol to the precipitate, and stir at 50°C for 10 min;

[0074] (6) After the precipitate is centrifuged at 4000 r / min, the supernatant is removed and 50 ml of ethanol is added for shaking and washing for 5 min;

[0075] (7) The precipitate was centrifuged at 4000 r / min, the supernatant was removed, and the precipitate was vacuum dried at 40° C. for 6 h to obtain dry copper powder (A-1).

[0076] Preparation method of copper powder (A-2):

[0077] (1) Weigh 20 g of hypophosphorous acid and mix it with 20 g of deionized water to form a uniform solution;

[0078] (2) Weigh 15 g of copper sulfate pentahydrate, dissolve it in 40 g of deionized water, and then add 10 g of PVP to dissolve and mix well to form a solution;

[0079] (3) The solution in (2) was added dropwise to the solution in (1), and stirred at 60° C. for 2 h to form a reddish brown solution;

[0080] (4) Cool to room temperature and centrifuge at 7000 r / min;

[0081] (5) Discard the supernatant, add 100 ml of ethanol to the precipitate, and stir at 50°C for 10 min;

[0082] (6) After the precipitate is centrifuged at 4000 r / min, the supernatant is removed and 50 ml of ethanol is added for shaking and washing for 5 min;

[0083] (7) The precipitate was centrifuged at 4000 r / min, the supernatant was removed, and the precipitate was vacuum dried at 40° C. for 6 h to obtain dry copper powder (A-2). The SEM image of the copper powder (A-2) particles is shown in FIG. Figure 1 shown.

[0084] Preparation method of copper powder (A-3):

[0085] (1) Weigh 20 g of hypophosphorous acid and mix it with 20 g of deionized water to form a uniform solution;

[0086] (2) Weigh 15 g of copper sulfate pentahydrate, dissolve it in 40 g of deionized water, and then add 10 g of PVP to dissolve and mix well to form a solution;

[0087] (3) The solution in (2) was added dropwise to the solution in (1), and stirred at 65° C. for 2 h to form a reddish brown solution;

[0088] (4) Cool to room temperature and centrifuge at 7000 r / min;

[0089] (5) Discard the supernatant, add 100 ml of ethanol to the precipitate, and stir at 50°C for 10 min;

[0090] (6) After the precipitate is centrifuged at 4000 r / min, the supernatant is removed and 50 ml of ethanol is added for shaking and washing for 5 min;

[0091] (7) The precipitate was centrifuged at 4000 r / min, the supernatant was removed, and the precipitate was vacuum dried at 40° C. for 6 h to obtain dry copper powder (A-3).

[0092] Preparation method of copper powder (A-4):

[0093] (1) Weigh 20 g of hypophosphorous acid and mix it with 20 g of deionized water to form a uniform solution;

[0094] (2) Weigh 15 g of copper sulfate pentahydrate, dissolve it in 40 g of deionized water, and then add 10 g of PVP to dissolve and mix well to form a solution;

[0095] (3) The solution in (2) was added dropwise to the solution in (1), and stirred at 70° C. for 2 h to form a reddish brown solution;

[0096] (4) Cool to room temperature and centrifuge at 7000 r / min;

[0097] (5) Discard the supernatant, add 100 ml of ethanol to the precipitate, and stir at 50°C for 10 min;

[0098] (6) After the precipitate is centrifuged at 4000 r / min, the supernatant is removed and 50 ml of ethanol is added for shaking and washing for 5 min;

[0099] (7) The precipitate was centrifuged at 4000 r / min, the supernatant was removed, and the precipitate was vacuum dried at 40° C. for 6 h to obtain dry copper powder (A-4).

[0100] Preparation method of copper powder (A-5):

[0101] (1) Weigh 20 g of hypophosphorous acid and mix it with 20 g of deionized water to form a uniform solution;

[0102] (2) Weigh 15 g of copper sulfate pentahydrate, dissolve it in 40 g of deionized water, and then add 10 g of PVP to dissolve and mix well to form a solution;

[0103] (3) The solution in (2) was added dropwise to the solution in (1), and stirred at 90° C. for 2 h to form a reddish brown solution;

[0104] (4) Cool to room temperature and centrifuge at 7000 r / min;

[0105] (5) Discard the supernatant, add 100 ml of ethanol to the precipitate, and stir at 50°C for 10 min;

[0106] (6) After the precipitate is centrifuged at 4000 r / min, the supernatant is removed and 50 ml of ethanol is added for shaking and washing for 5 min;

[0107] (7) The precipitate was centrifuged at 4000 r / min, the supernatant was removed, and the precipitate was vacuum dried at 40° C. for 6 h to obtain dry copper powder (A-5). The SEM image of the copper powder (A-5) particles is shown in FIG. Figure 2 shown.

[0108] Preparation method of copper powder (A-6):

[0109] (1) Weigh 20 g of hypophosphorous acid and mix it with 20 g of deionized water to form a uniform solution;

[0110] (2) Weigh 15 g of copper sulfate pentahydrate, dissolve it in 40 g of deionized water, and then add 10 g of PVP to dissolve and mix well to form a solution;

[0111] (3) The solution in (2) was added dropwise to the solution in (1), and stirred at 65° C. for 2 h to form a reddish brown solution;

[0112] (4) Cool to room temperature and centrifuge at 7000 r / min;

[0113] (5) Discard the supernatant, add 100 ml of ethanol to the precipitate, and stir at 35°C for 10 min;

[0114] (6) After the precipitate is centrifuged at 4000 r / min, the supernatant is removed and 50 ml of ethanol is added for shaking and washing for 5 min;

[0115] (7) The precipitate was centrifuged at 4000 r / min, the supernatant was removed, and the precipitate was vacuum dried at 40° C. for 6 h to obtain dry copper powder (A-6).

[0116] Preparation method of copper powder (A-7):

[0117] (1) Weigh 20 g of hypophosphorous acid and mix it with 20 g of deionized water to form a uniform solution;

[0118] (2) Weigh 15 g of copper sulfate pentahydrate, dissolve it in 40 g of deionized water, and then add 10 g of PVP to dissolve and mix well to form a solution;

[0119] (3) The solution in (2) was added dropwise to the solution in (1), and stirred at 65° C. for 2 h to form a reddish brown solution;

[0120] (4) Cool to room temperature and centrifuge at 7000 r / min;

[0121] (5) Discard the supernatant, add 100 ml of ethanol to the precipitate, and stir at 40°C for 10 min;

[0122] (6) After the precipitate is centrifuged at 4000 r / min, the supernatant is removed and 50 ml of ethanol is added for shaking and washing for 5 min;

[0123] (7) The precipitate was centrifuged at 4000 r / min, the supernatant was removed, and the precipitate was vacuum dried at 40° C. for 6 h to obtain dry copper powder (A-7).

[0124] Preparation method of copper powder (A-8):

[0125] (1) Weigh 20 g of hypophosphorous acid and mix it with 20 g of deionized water to form a uniform solution;

[0126] (2) Weigh 15 g of copper sulfate pentahydrate, dissolve it in 40 g of deionized water, and then add 10 g of PVP to dissolve and mix well to form a solution;

[0127] (3) The solution in (2) was added dropwise to the solution in (1), and stirred at 65° C. for 2 h to form a reddish brown solution;

[0128] (4) Cool to room temperature and centrifuge at 7000 r / min;

[0129] (5) Discard the supernatant, add 100 ml of ethanol to the precipitate, and stir at 55°C for 10 min;

[0130] (6) After the precipitate is centrifuged at 4000 r / min, the supernatant is removed and 50 ml of ethanol is added for shaking and washing for 5 min;

[0131] (7) The precipitate was centrifuged at 4000 r / min, the supernatant was removed, and the precipitate was vacuum dried at 40° C. for 6 h to obtain dry copper powder (A-8).

[0132] Preparation method of copper powder (A-9):

[0133] (1) Weigh 20 g of hypophosphorous acid and mix it with 20 g of deionized water to form a uniform solution;

[0134] (2) Weigh 15 g of copper sulfate pentahydrate, dissolve it in 40 g of deionized water, and then add 10 g of PVP to dissolve and mix well to form a solution;

[0135] (3) The solution in (2) was added dropwise to the solution in (1), and stirred at 65° C. for 2 h to form a reddish brown solution;

[0136] (4) Cool to room temperature and centrifuge at 7000 r / min;

[0137] (5) Discard the supernatant, add 100 ml of ethanol to the precipitate, and stir at 60°C for 10 min;

[0138] (6) After the precipitate is centrifuged at 4000 r / min, the supernatant is removed and 50 ml of ethanol is added for shaking and washing for 5 min;

[0139] (7) The precipitate was centrifuged at 4000 r / min, the supernatant was removed, and the precipitate was vacuum dried at 40° C. for 6 h to obtain dry copper powder (A-9).

[0140] Preparation method of copper powder (A-10):

[0141] (1) Weigh 20 g of hypophosphorous acid and mix it with 20 g of deionized water to form a uniform solution;

[0142] (2) Weigh 15 g of copper sulfate pentahydrate, dissolve it in 40 g of deionized water, and then add 10 g of PVP to dissolve and mix well to form a solution;

[0143] (3) The solution in (2) was added dropwise to the solution in (1), and stirred at 65° C. for 2 h to form a reddish brown solution;

[0144] (4) Cool to room temperature and centrifuge at 7000 r / min;

[0145] (5) Discard the supernatant, add 100 ml of ethanol to the precipitate, and stir at 70°C for 10 min;

[0146] (6) After the precipitate is centrifuged at 4000 r / min, the supernatant is removed and 50 ml of ethanol is added for shaking and washing for 5 min;

[0147] (7) The precipitate was centrifuged at 4000 r / min, the supernatant was removed, and the precipitate was vacuum dried at 40° C. for 6 h to obtain dry copper powder (A-10).

[0148] Preparation method of copper powder (A-11):

[0149] (1) Weigh 20 g of hypophosphorous acid and mix it with 20 g of deionized water to form a uniform solution;

[0150] (2) Weigh 15 g of copper sulfate pentahydrate, dissolve it in 40 g of deionized water, and then add 10 g of PVP to dissolve and mix well to form a solution;

[0151] (3) The solution in (2) was added dropwise to the solution in (1), and stirred at 40° C. for 2 h to form a reddish brown solution;

[0152] (4) Cool to room temperature and centrifuge at 7000 r / min;

[0153] (5) Discard the supernatant, add 100 ml of ethanol to the precipitate, and stir at 50°C for 10 min;

[0154] (6) After the precipitate is centrifuged at 4000 r / min, the supernatant is removed and 50 ml of ethanol is added for shaking and washing for 5 min;

[0155] (7) The precipitate was centrifuged at 4000 r / min, the supernatant was removed, and the precipitate was vacuum dried at 40° C. for 6 h to obtain dry copper powder (A-11). The SEM image of the copper powder (A-11) particles is shown in FIG. Figure 3 shown.

[0156] Preparation method of copper powder (B):

[0157] (1) Weigh 20 g of ascorbic acid and mix it with 20 g of deionized water to form a uniform solution;

[0158] (2) Weigh 15 g of copper sulfate pentahydrate, dissolve it in 40 g of deionized water, and then add 10 g of polyethylene glycol 400 and mix well to form a solution;

[0159] (3) The solution in (2) was added dropwise to the solution in (1), and stirred at 80° C. for 2 h to form a reddish brown solution;

[0160] (4) Cool to room temperature and centrifuge at 7000 r / min;

[0161] (5) Discard the supernatant, add 100 ml of ethanol to the precipitate, and stir at 50°C for 10 min;

[0162] (6) After the precipitate is centrifuged at 4000 r / min, the supernatant is removed and 50 ml of ethanol is added for shaking and washing for 5 min;

[0163] (7) The precipitate was centrifuged at 4000 r / min, the supernatant was removed, and the precipitate was vacuum dried at 40° C. for 6 h to obtain dry copper powder (B). The SEM image of the copper powder (B) particles is shown in FIG. Figure 4 shown.

[0164] Preparation method of copper powder (C):

[0165] (1) Weigh 20 g of sodium hypophosphite and mix it with 20 g of deionized water to form a uniform solution;

[0166] (2) Weigh 15 g of copper acetate monohydrate, dissolve it in 40 g of deionized water, and then add 10 g of PVP to dissolve and mix well to form a solution;

[0167] (3) The solution in (2) was added dropwise to the solution in (1), and stirred at 80° C. for 2 h to form a reddish brown solution;

[0168] (4) Cool to room temperature and centrifuge at 7000 r / min;

[0169] (5) Discard the supernatant, add 100 ml of ethanol to the precipitate, and stir at 50°C for 10 min;

[0170] (6) After the precipitate is centrifuged at 4000 r / min, the supernatant is removed and 50 ml of ethanol is added for shaking and washing for 5 min;

[0171] (7) The precipitate was centrifuged at 4000 r / min, the supernatant was removed, and the precipitate was vacuum dried at 40° C. for 6 h to obtain dry copper powder (C). The SEM image of the copper powder (C) particles is shown in FIG. Figure 5 shown.

[0172] The variable parameters in the preparation process of copper powder (A-1)-copper powder (A-10), copper powder (B) and copper powder (C) are shown in Table 1 below:

[0173] Table 1

[0174] serial number Copper salt types Reducing agent type Step (3) Temperature Step (5) Temperature Copper powder (A-1) Copper sulfate pentahydrate Hypophosphorous acid 50℃ 50℃ Copper powder (A-2) Copper sulfate pentahydrate Hypophosphorous acid 60℃ 50℃ Copper powder (A-3) Copper sulfate pentahydrate Hypophosphorous acid 65℃ 50℃ Copper powder (A-4) Copper sulfate pentahydrate Hypophosphorous acid 70℃ 50℃ Copper powder (A-5) Copper sulfate pentahydrate Hypophosphorous acid 90℃ 50℃ Copper powder (A-6) Copper sulfate pentahydrate Hypophosphorous acid 65℃ 35℃ Copper powder (A-7) Copper sulfate pentahydrate Hypophosphorous acid 65℃ 40℃ Copper powder (A-8) Copper sulfate pentahydrate Hypophosphorous acid 65℃ 55℃ Copper powder (A-9) Copper sulfate pentahydrate Hypophosphorous acid 65℃ 60℃ Copper powder (A-10) Copper sulfate pentahydrate Hypophosphorous acid 65℃ 70℃ Copper powder (A-11) Copper sulfate pentahydrate Hypophosphorous acid 40℃ 50℃ Copper powder (B) Copper sulfate pentahydrate ascorbic acid 80℃ 50℃ Copper powder (C) Cupric acetate monohydrate Sodium hypophosphite 80℃ 50℃

[0175] Example 1

[0176] (1) Weigh 0.5 g of mixed epoxy resin MF-3286, 0.16 g of curing agent methyltetrahydrophthalic anhydride, 0.2 g of active diluent ethylene glycol diglycidyl ether, 0.5 g of dispersant diethylene glycol butyl ether, and 8.4 g of dry copper powder (A-2), heat and stir at 60° C. under a nitrogen atmosphere to fully crosslink the copper powder (A-2) and the organic carrier for 10 min, and then cool to room temperature;

[0177] (2) Weighing 0.22 g of thixotropic agent tributyl citrate and 0.02 g of adhesion promoter KH550, adding them to the mixed slurry, and mixing them several times with a slurry mixer at 2000 r / min to fully disperse the copper powder particles and the organic carrier to obtain a copper slurry with a high degree of crosslinking;

[0178] (3) The copper paste was ground on a three-roll mill at a gap of 5 μm for more than three times, and filtered using a 30 μm nylon mesh to obtain a uniformly dispersed copper paste.

[0179] Example 2

[0180] (1) Weigh 0.5 g of mixed epoxy resin MF-3286, 0.16 g of curing agent methyltetrahydrophthalic anhydride, 0.2 g of active diluent ethylene glycol diglycidyl ether, 0.5 g of dispersant diethylene glycol butyl ether, and 8.4 g of dry copper powder (A-3), heat and stir at 60° C. under a nitrogen atmosphere to fully crosslink the copper powder (A-3) and the organic carrier for 10 min, and then cool to room temperature;

[0181] (2) Weighing 0.22 g of thixotropic agent tributyl citrate and 0.02 g of adhesion promoter KH550, adding them to the mixed slurry, and mixing them several times with a slurry mixer at 2000 r / min to fully disperse the copper powder particles and the organic carrier to obtain a copper slurry with a high degree of crosslinking;

[0182] (3) The copper paste was ground on a three-roll mill at a gap of 5 μm for more than three times, and filtered using a 30 μm nylon mesh to obtain a uniformly dispersed copper paste.

[0183] Example 3

[0184] (1) Weigh 0.5 g of mixed epoxy resin MF-3286, 0.16 g of curing agent methyltetrahydrophthalic anhydride, 0.2 g of active diluent ethylene glycol diglycidyl ether, 0.5 g of dispersant diethylene glycol butyl ether, and 8.4 g of dry copper powder (A-4), heat and stir at 60° C. under a nitrogen atmosphere to fully crosslink the copper powder (A-4) and the organic carrier for 10 min, and then cool to room temperature;

[0185] (2) Weighing 0.22 g of thixotropic agent tributyl citrate and 0.02 g of adhesion promoter KH550, adding them to the mixed slurry, and mixing them several times with a slurry mixer at 2000 r / min to fully disperse the copper powder particles and the organic carrier to obtain a copper slurry with a high degree of crosslinking;

[0186] (3) The copper paste was ground on a three-roll mill at a gap of 5 μm for more than three times, and filtered using a 30 μm nylon mesh to obtain a uniformly dispersed copper paste.

[0187] Example 4

[0188] (1) Weigh 0.5 g of mixed epoxy resin MF-3286, 0.16 g of curing agent methyltetrahydrophthalic anhydride, 0.2 g of active diluent ethylene glycol diglycidyl ether, 0.5 g of dispersant diethylene glycol butyl ether, and 8.4 g of dry copper powder (A-7), heat and stir at 60° C. under a nitrogen atmosphere to fully crosslink the copper powder (A-7) and the organic carrier for 10 min, and then cool to room temperature;

[0189] (2) Weighing 0.22 g of thixotropic agent tributyl citrate and 0.02 g of adhesion promoter KH550, adding them to the mixed slurry, and mixing them several times with a slurry mixer at 2000 r / min to fully disperse the copper powder particles and the organic carrier to obtain a copper slurry with a high degree of crosslinking;

[0190] (3) The copper paste was ground on a three-roll mill at a gap of 5 μm for more than three times, and filtered using a 30 μm nylon mesh to obtain a uniformly dispersed copper paste.

[0191] Example 5

[0192] (1) Weigh 0.5 g of mixed epoxy resin MF-3286, 0.16 g of curing agent methyl tetrahydrophthalic anhydride, 0.2 g of active diluent ethylene glycol diglycidyl ether, 0.5 g of dispersant diethylene glycol butyl ether, and 8.4 g of dry copper powder (A-8), heat and stir at 60° C. under a nitrogen atmosphere to fully crosslink the copper powder (A-8) and the organic carrier for 10 min, and then cool to room temperature;

[0193] (2) Weighing 0.22 g of thixotropic agent tributyl citrate and 0.02 g of adhesion promoter KH550, adding them to the mixed slurry, and mixing them several times with a slurry mixer at 2000 r / min to fully disperse the copper powder particles and the organic carrier to obtain a copper slurry with a high degree of crosslinking;

[0194] (3) The copper paste was ground on a three-roll mill at a gap of 5 μm for more than three times, and filtered using a 30 μm nylon mesh to obtain a uniformly dispersed copper paste.

[0195] Example 6

[0196] (1) Weigh 0.5 g of mixed epoxy resin MF-3286, 0.16 g of curing agent methyl tetrahydrophthalic anhydride, 0.2 g of active diluent ethylene glycol diglycidyl ether, 0.5 g of dispersant diethylene glycol butyl ether, and 8.4 g of dry copper powder (A-9), heat and stir at 60° C. under a nitrogen atmosphere to fully crosslink the copper powder (A-9) and the organic carrier for 10 min, and then cool to room temperature;

[0197] (2) Weighing 0.22 g of thixotropic agent tributyl citrate and 0.02 g of adhesion promoter KH550, adding them to the mixed slurry, and mixing them several times with a slurry mixer at 2000 r / min to fully disperse the copper powder particles and the organic carrier to obtain a copper slurry with a high degree of crosslinking;

[0198] (3) The copper paste was ground on a three-roll mill at a gap of 5 μm for more than three times, and filtered using a 30 μm nylon mesh to obtain a uniformly dispersed copper paste.

[0199] Example 7

[0200] (1) Weigh 0.5 g of mixed epoxy resin MF-3286, 0.16 g of curing agent methyl tetrahydrophthalic anhydride, 0.2 g of active diluent ethylene glycol diglycidyl ether, 0.5 g of dispersant diethylene glycol butyl ether, and 8.4 g of dry copper powder (B), heat and stir at 60° C. under a nitrogen atmosphere to fully crosslink the copper powder (B) with the organic carrier for 10 min, and then cool to room temperature;

[0201] (2) Weighing 0.22 g of thixotropic agent tributyl citrate and 0.02 g of adhesion promoter KH550, adding them to the mixed slurry, and mixing them several times with a slurry mixer at 2000 r / min to fully disperse the copper powder particles and the organic carrier to obtain a copper slurry with a high degree of crosslinking;

[0202] (3) The copper paste was ground on a three-roll mill at a gap of 5 μm for more than three times, and filtered using a 30 μm nylon mesh to obtain a uniformly dispersed copper paste.

[0203] Example 8

[0204] (1) Weigh 0.5 g of mixed epoxy resin MF-3286, 0.16 g of curing agent methyltetrahydrophthalic anhydride, 0.2 g of active diluent ethylene glycol diglycidyl ether, 0.5 g of dispersant diethylene glycol butyl ether, and 8.4 g of dry copper powder (C), heat and stir at 60° C. under a nitrogen atmosphere to fully crosslink the copper powder (C) with the organic carrier for 10 min, and then cool to room temperature;

[0205] (2) Weighing 0.22 g of thixotropic agent tributyl citrate and 0.02 g of adhesion promoter KH550, adding them to the mixed slurry, and mixing them several times with a slurry mixer at 2000 r / min to fully disperse the copper powder particles and the organic carrier to obtain a copper slurry with a high degree of crosslinking;

[0206] (3) The copper paste was ground on a three-roll mill at a gap of 5 μm for more than three times, and filtered using a 30 μm nylon mesh to obtain a uniformly dispersed copper paste.

[0207] Example 9

[0208] (1) Weigh 0.5 g of mixed epoxy resin MF-3286, 0.16 g of curing agent methyltetrahydrophthalic anhydride, 0.2 g of active diluent ethylene glycol diglycidyl ether, 0.5 g of dispersant diethylene glycol butyl ether, and 6.4 g of dry copper powder (A-3), heat and stir at 60° C. under a nitrogen atmosphere to fully crosslink the copper powder (A-3) and the organic carrier for 10 min, and then cool to room temperature;

[0209] (2) Weighing 0.22 g of thixotropic agent tributyl citrate and 0.02 g of adhesion promoter KH550, adding them to the mixed slurry, and mixing them several times with a slurry mixer at 2000 r / min to fully disperse the copper powder particles and the organic carrier to obtain a copper slurry with a high degree of crosslinking;

[0210] (3) The copper paste was ground on a three-roll mill at a gap of 5 μm for more than three times, and filtered using a 30 μm nylon mesh to obtain a uniformly dispersed copper paste.

[0211] Example 10

[0212] (1) Weigh 0.5 g of mixed epoxy resin MF-3286, 0.16 g of curing agent methyltetrahydrophthalic anhydride, 0.2 g of active diluent ethylene glycol diglycidyl ether, 0.5 g of dispersant diethylene glycol butyl ether, and 7.3 g of dry copper powder (A-3), heat and stir at 60° C. under a nitrogen atmosphere to fully crosslink the copper powder (A-3) and the organic carrier for 10 min, and then cool to room temperature;

[0213] (2) Weighing 0.22 g of thixotropic agent tributyl citrate and 0.02 g of adhesion promoter KH550, adding them to the mixed slurry, and mixing them several times with a slurry mixer at 2000 r / min to fully disperse the copper powder particles and the organic carrier to obtain a copper slurry with a high degree of crosslinking;

[0214] (3) The copper paste was ground on a three-roll mill at a gap of 5 μm for more than three times, and filtered using a 30 μm nylon mesh to obtain a uniformly dispersed copper paste.

[0215] Embodiment 11

[0216] (1) Weigh 0.5 g of mixed epoxy resin MF-3286, 0.16 g of curing agent methyltetrahydrophthalic anhydride, 0.2 g of active diluent ethylene glycol diglycidyl ether, 0.5 g of dispersant diethylene glycol butyl ether, and 9.0 g of dry copper powder (A-3), heat and stir at 60° C. under a nitrogen atmosphere to fully crosslink the copper powder (A-3) and the organic carrier for 10 min, and then cool to room temperature;

[0217] (2) Weighing 0.22 g of thixotropic agent tributyl citrate and 0.02 g of adhesion promoter KH550, adding them to the mixed slurry, and mixing them several times with a slurry mixer at 2000 r / min to fully disperse the copper powder particles and the organic carrier to obtain a copper slurry with a high degree of crosslinking;

[0218] (3) The copper paste was ground on a three-roll mill at a gap of 5 μm for more than three times, and filtered using a 30 μm nylon mesh to obtain a uniformly dispersed copper paste.

[0219] Example 12

[0220] (1) Weigh 0.5 g of mixed epoxy resin MF-3286, 0.16 g of curing agent methyltetrahydrophthalic anhydride, 0.2 g of active diluent ethylene glycol diglycidyl ether, 0.5 g of dispersant diethylene glycol butyl ether, and 9.8 g of dry copper powder (A-3), heat and stir at 60° C. under a nitrogen atmosphere to fully crosslink the copper powder (A-3) and the organic carrier for 10 min, and then cool to room temperature;

[0221] (2) Weighing 0.22 g of thixotropic agent tributyl citrate and 0.02 g of adhesion promoter KH550, adding them to the mixed slurry, and mixing them several times with a slurry mixer at 2000 r / min to fully disperse the copper powder particles and the organic carrier to obtain a copper slurry with a high degree of crosslinking;

[0222] (3) The copper paste was ground on a three-roll mill at a gap of 5 μm for more than three times, and filtered using a 30 μm nylon mesh to obtain a uniformly dispersed copper paste.

[0223] Embodiment 13

[0224] (1) Weigh 0.5 g of mixed epoxy resin MF-3286, 0.16 g of curing agent methyl tetrahydrophthalic anhydride, 0.2 g of active diluent ethylene glycol diglycidyl ether, 0.5 g of dispersant diethylene glycol butyl ether, and 8.4 g of dry copper powder (A-3), heat and stir at 55° C. under a nitrogen atmosphere to fully crosslink the copper powder (A-3) and the organic carrier for 15 minutes, and then cool to room temperature;

[0225] (2) Weighing 0.22 g of thixotropic agent tributyl citrate and 0.02 g of adhesion promoter KH550, adding them to the mixed slurry, and mixing them several times with a slurry mixer at 2000 r / min to fully disperse the copper powder particles and the organic carrier to obtain a copper slurry with a high degree of crosslinking;

[0226] (3) The copper paste was ground on a three-roll mill at a gap of 5 μm for more than three times, and filtered using a 30 μm nylon mesh to obtain a uniformly dispersed copper paste.

[0227] Embodiment 14

[0228] (1) Weigh 0.5 g of mixed epoxy resin MF-3286, 0.16 g of curing agent methyltetrahydrophthalic anhydride, 0.2 g of active diluent ethylene glycol diglycidyl ether, 0.5 g of dispersant diethylene glycol butyl ether, and 8.4 g of dry copper powder, heat and stir at 65° C. under a nitrogen atmosphere to fully crosslink the copper powder (A-3) and the organic carrier for 5 min, and then cool to room temperature;

[0229] (2) Weighing 0.22 g of thixotropic agent tributyl citrate and 0.02 g of adhesion promoter KH550, adding them to the mixed slurry, and mixing them several times with a slurry mixer at 2000 r / min to fully disperse the copper powder particles and the organic carrier to obtain a copper slurry with a high degree of crosslinking;

[0230] (3) The copper paste was ground on a three-roll mill at a gap of 5 μm for more than three times, and filtered using a 30 μm nylon mesh to obtain a uniformly dispersed copper paste.

[0231] Embodiment 15

[0232] (1) Weigh 0.5 g of mixed epoxy resin MF-3286, 0.16 g of curing agent methyltetrahydrophthalic anhydride, 0.2 g of active diluent ethylene glycol diglycidyl ether, 0.5 g of dispersant diethylene glycol butyl ether, and 8.4 g of dry copper powder (A-1), heat and stir at 60° C. under a nitrogen atmosphere to fully crosslink the copper powder (A-1) and the organic carrier, and then cool to room temperature for 10 minutes;

[0233] (2) Weighing 0.22 g of thixotropic agent tributyl citrate and 0.02 g of adhesion promoter KH550, adding them to the mixed slurry, and mixing them several times with a slurry mixer at 2000 r / min to fully disperse the copper powder particles and the organic carrier to obtain a copper slurry with a high degree of crosslinking;

[0234] (3) The copper paste was ground on a three-roll mill at a gap of 5 μm for more than three times, and filtered using a 30 μm nylon mesh to obtain a uniformly dispersed copper paste.

[0235] Comparative Example 1

[0236] (1) Weigh 0.5 g of mixed epoxy resin MF-3286, 0.16 g of curing agent methyltetrahydrophthalic anhydride, 0.2 g of active diluent ethylene glycol diglycidyl ether, 0.5 g of dispersant diethylene glycol butyl ether, and 8.4 g of dry copper powder (A-11), heat and stir at 60° C. under a nitrogen atmosphere to fully crosslink the copper powder (A-1) and the organic carrier, and then cool to room temperature for 10 minutes;

[0237] (2) Weighing 0.22 g of thixotropic agent tributyl citrate and 0.02 g of adhesion promoter KH550, adding them to the mixed slurry, and mixing them several times with a slurry mixer at 2000 r / min to fully disperse the copper powder particles and the organic carrier to obtain a copper slurry with a high degree of crosslinking;

[0238] (3) The copper paste was ground on a three-roll mill at a gap of 5 μm for more than three times, and filtered using a 30 μm nylon mesh to obtain a uniformly dispersed copper paste.

[0239] Comparative Example 2

[0240] (1) Weigh 0.5 g of mixed epoxy resin MF-3286, 0.16 g of curing agent methyl tetrahydrophthalic anhydride, 0.2 g of active diluent ethylene glycol diglycidyl ether, 0.5 g of dispersant diethylene glycol butyl ether, and 8.4 g of dry copper powder (A-5), heat and stir at 60° C. under a nitrogen atmosphere to fully crosslink the copper powder (A-5) and the organic carrier, and then cool to room temperature for 10 minutes;

[0241] (2) Weighing 0.22 g of thixotropic agent tributyl citrate and 0.02 g of adhesion promoter KH550, adding them to the mixed slurry, and mixing them several times with a slurry mixer at 2000 r / min to fully disperse the copper powder particles and the organic carrier to obtain a copper slurry with a high degree of crosslinking;

[0242] (3) The copper paste was ground on a three-roll mill at a gap of 5 μm for more than three times, and filtered using a 30 μm nylon mesh to obtain a uniformly dispersed copper paste.

[0243] Comparative Example 3

[0244] (1) Weigh 0.5 g of mixed epoxy resin MF-3286, 0.16 g of curing agent methyltetrahydrophthalic anhydride, 0.2 g of active diluent ethylene glycol diglycidyl ether, 0.5 g of dispersant diethylene glycol butyl ether, and 8.4 g of dry copper powder (A-6), heat and stir at 60° C. under a nitrogen atmosphere to fully crosslink the copper powder (A-6) and the organic carrier, and then cool to room temperature for 10 minutes;

[0245] (2) Weighing 0.22 g of thixotropic agent tributyl citrate and 0.02 g of adhesion promoter KH550, adding them to the mixed slurry, and mixing them several times with a slurry mixer at 2000 r / min to fully disperse the copper powder particles and the organic carrier to obtain a copper slurry with a high degree of crosslinking;

[0246] (3) The copper paste was ground on a three-roll mill at a gap of 5 μm for more than three times, and filtered using a 30 μm nylon mesh to obtain a uniformly dispersed copper paste.

[0247] Comparative Example 4

[0248] (1) Weigh 0.5 g of mixed epoxy resin MF-3286, 0.16 g of curing agent methyl tetrahydrophthalic anhydride, 0.2 g of active diluent ethylene glycol diglycidyl ether, 0.5 g of dispersant diethylene glycol butyl ether, and 8.4 g of dry copper powder (A-10), heat and stir at 60° C. under a nitrogen atmosphere to fully crosslink the copper powder (A-10) and the organic carrier for 10 min, and then cool to room temperature;

[0249] (2) Weighing 0.22 g of thixotropic agent tributyl citrate and 0.02 g of adhesion promoter KH550, adding them to the mixed slurry, and mixing them several times with a slurry mixer at 2000 r / min to fully disperse the copper powder particles and the organic carrier to obtain a copper slurry with a high degree of crosslinking;

[0250] (3) The copper paste was ground on a three-roll mill at a gap of 5 μm for more than three times, and filtered using a 30 μm nylon mesh to obtain a uniformly dispersed copper paste.

[0251] Comparative Example 5

[0252] (1) Weigh 0.5 g of mixed epoxy resin MF-3286, 0.16 g of curing agent methyl tetrahydrophthalic anhydride, 0.2 g of active diluent ethylene glycol diglycidyl ether, 0.5 g of dispersant diethylene glycol butyl ether, and 3.9 g of dry copper powder (A-3), heat and stir at 60° C. under a nitrogen atmosphere to fully crosslink the copper powder (A-3) and the organic carrier for 10 min, and then cool to room temperature;

[0253] (2) Weighing 0.22 g of thixotropic agent tributyl citrate and 0.02 g of adhesion promoter KH550, adding them to the mixed slurry, and mixing them several times with a slurry mixer at 2000 r / min to fully disperse the copper powder particles and the organic carrier to obtain a copper slurry with a high degree of crosslinking;

[0254] (3) The copper paste was ground on a three-roll mill at a gap of 5 μm for more than three times, and filtered using a 30 μm nylon mesh to obtain a uniformly dispersed copper paste.

[0255] Comparative Example 6

[0256] (1) Weigh 0.5 g of mixed epoxy resin MF-3286, 0.16 g of curing agent methyltetrahydrophthalic anhydride, 0.2 g of active diluent ethylene glycol diglycidyl ether, 0.5 g of dispersant diethylene glycol butyl ether, and 14.4 g of dry copper powder (A-3), heat and stir at 60° C. under a nitrogen atmosphere to fully crosslink the copper powder (A-3) and the organic carrier for 10 min, and then cool to room temperature;

[0257] (2) Weighing 0.22 g of thixotropic agent tributyl citrate and 0.02 g of adhesion promoter KH550, adding them to the mixed slurry, and mixing them several times with a slurry mixer at 2000 r / min to fully disperse the copper powder particles and the organic carrier to obtain a copper slurry with a high degree of crosslinking;

[0258] (3) The copper paste was ground on a three-roll mill at a gap of 5 μm for more than three times, and filtered using a 30 μm nylon mesh to obtain a uniformly dispersed copper paste.

[0259] Comparative Example 7

[0260] (1) Weigh 0.5 g of mixed epoxy resin MF-3286, 0.16 g of curing agent methyltetrahydrophthalic anhydride, 0.2 g of active diluent ethylene glycol diglycidyl ether, 0.5 g of dispersant diethylene glycol butyl ether, and 8.4 g of dry copper powder (A-3), heat and stir at 45° C. under a nitrogen atmosphere to fully crosslink the copper powder (A-3) and the organic carrier for 15 min, and then cool to room temperature;

[0261] (2) Weighing 0.22 g of thixotropic agent tributyl citrate and 0.02 g of adhesion promoter KH550, adding them to the mixed slurry, and mixing them several times with a slurry mixer at 2000 r / min to fully disperse the copper powder particles and the organic carrier to obtain a copper slurry with a high degree of crosslinking;

[0262] (3) The copper paste was ground on a three-roll mill at a gap of 5 μm for more than three times, and filtered using a 30 μm nylon mesh to obtain a uniformly dispersed copper paste.

[0263] Comparative Example 8

[0264] (1) Weigh 0.5 g of mixed epoxy resin MF-3286, 0.16 g of curing agent methyltetrahydrophthalic anhydride, 0.2 g of active diluent ethylene glycol diglycidyl ether, 0.5 g of dispersant diethylene glycol butyl ether, and 8.4 g of dry copper powder (A-3), heat and stir at 75° C. under a nitrogen atmosphere to fully crosslink the copper powder (A-3) and the organic carrier for 5 min, and then cool to room temperature;

[0265] (2) Weighing 0.22 g of thixotropic agent tributyl citrate and 0.02 g of adhesion promoter KH550, adding them to the mixed slurry, and mixing them several times with a slurry mixer at 2000 r / min to fully disperse the copper powder particles and the organic carrier to obtain a copper slurry with a high degree of crosslinking;

[0266] (3) The copper paste was ground on a three-roll mill at a gap of 5 μm for more than three times, and filtered using a 30 μm nylon mesh to obtain a uniformly dispersed copper paste.

[0267] Comparative Example 9

[0268] (1) Weigh 0.5 g of mixed epoxy resin MF-3286, 0.16 g of curing agent methyltetrahydrophthalic anhydride, 0.5 g of dispersant diethylene glycol butyl ether, and 8.4 g of dry copper powder, heat and stir at 60° C. under a nitrogen atmosphere to fully crosslink the copper powder (A-3) and the organic carrier for 10 min, and then cool to room temperature;

[0269] (2) Weighing 0.22 g of thixotropic agent tributyl citrate and 0.02 g of adhesion promoter KH550, adding them to the mixed slurry, and mixing them several times with a slurry mixer at 2000 r / min to fully disperse the copper powder particles and the organic carrier to obtain a copper slurry with a high degree of crosslinking;

[0270] (3) The copper paste was ground on a three-roll mill at a gap of 5 μm for more than three times, and filtered using a 30 μm nylon mesh to obtain a uniformly dispersed copper paste.

[0271] Comparative Example 10

[0272] (1) Weigh 0.5 g of bisphenol A epoxy resin E51, 0.16 g of curing agent methyl tetrahydrophthalic anhydride, 0.2 g of active diluent ethylene glycol diglycidyl ether, 0.5 g of dispersant diethylene glycol butyl ether, and 8.4 g of dry copper powder (A-3), heat and stir at 60° C. under a nitrogen atmosphere to fully crosslink the copper powder (A-3) and the organic carrier for 10 min, and then cool to room temperature;

[0273] (2) Weighing 0.22 g of thixotropic agent tributyl citrate and 0.02 g of adhesion promoter KH550, adding them to the mixed slurry, and mixing them several times with a slurry mixer at 2000 r / min to fully disperse the copper powder particles and the organic carrier to obtain a copper slurry with a high degree of crosslinking;

[0274] (3) The copper paste was ground on a three-roll mill at a gap of 5 μm for more than three times, and filtered using a 30 μm nylon mesh to obtain a uniformly dispersed copper paste.

[0275] Comparative Example 11

[0276] (1) Weigh 0.5 g of acrylic resin KPL-63666, 0.16 g of curing agent methyl tetrahydrophthalic anhydride, 0.2 g of active diluent ethylene glycol diglycidyl ether, 0.5 g of dispersant diethylene glycol butyl ether, and 8.4 g of dry copper powder (A-3), heat and stir at 60° C. under a nitrogen atmosphere to fully crosslink the copper powder (A-3) and the organic carrier for 10 min, and then cool to room temperature;

[0277] (2) Weighing 0.22 g of thixotropic agent tributyl citrate and 0.02 g of adhesion promoter KH550, adding them to the mixed slurry, and mixing them several times with a slurry mixer at 2000 r / min to fully disperse the copper powder particles and the organic carrier to obtain a copper slurry with a high degree of crosslinking;

[0278] (3) The copper paste was ground on a three-roll mill at a gap of 5 μm for more than three times, and filtered using a 30 μm nylon mesh to obtain a uniformly dispersed copper paste.

[0279]

Performance test

[0280] (1) Particle size observation: Use a Phenom scanning electron microscope to characterize the size and morphology of copper nanoparticles: ① Take a small amount of slurry and dilute it in deionized water or organic solvent at a ratio of 1:500; ② Ultrasonicate the diluted solution to fully disperse it, pipette a small amount and add it to the surface of the silicon wafer and heat it to remove excess solvent; ③ Prepare the sample, spray it with gold, and observe the sample to obtain the image information of the size and morphology of the copper nanoparticles.

[0281] (2) Aspect ratio test: Use an ultra-depth-of-field microscope to observe and measure the line width and line height of the printed 3D grid lines.

[0282] (3) Viscosity test: Use Brookfield DVNextCP cone-plate viscometer to measure the viscosity of copper slurry: ① Adjust the torque to zero and adjust the distance between the cone plates to 0.0005 inches; ② Take a volume of 0.5 ml of conductive copper slurry and place it in the center of the sample cup, set the speed and test time, where the speed is 1 rpm; ③ Test to obtain material viscosity information and record it.

[0283] (4) Adhesion test: ① The prepared conductive copper paste was coated on the glass substrate by a coating machine and sintered at 200°C for 30 min under a nitrogen atmosphere to obtain a copper film; ② According to ASTM D3359-2017 as the test standard, a grid knife was used to cut the surface of the test piece at a cutting speed of 20-50 mm / s; ③ The test piece was rotated 90° and the above operation was repeated on the cut to form a grid pattern; ④ The diagonal lines on both sides of the grid pattern were brushed lightly 5 times each; ⑤ A 3M 600-1PK test tape was used to perform a peel test and evaluate the adhesion performance of the material.

[0284] (5) Printing test: Use a Nordson EFD dispensing machine to perform a printing test on the slurry: ① Load the prepared slurry into a 3 ml material tube and install a 50 μm needle, load the entire device into a booster pen, and connect it to the dispensing machine; ② Use the running program to print. The three-dimensional configuration printing process is shown in the figure. Figure 6 shown.

[0285]

Test results

[0286] The relevant indicators of the products prepared in the above embodiments and comparative examples were tested to obtain the following table.

[0287] project Viscosity (Pa·s) Linear shrinkage Adhesion Aspect ratio test Print Test Finished product requirements Example 1 734.4 3.2% 5B 0.692 Stable discharge pass Example 2 756.7 2.9% 5B 0.761 Stable discharge pass Example 3 766.1 3.0% 5B 0.794 Stable discharge pass Example 4 784.9 3.3% 5B 0.781 Stable discharge pass Example 5 731.3 3.4% 5B 0.684 Stable discharge pass Example 6 692.4 3.2% 4B 0.570 Stable discharge pass Example 7 734.1 2.8% 5B 0.769 Stable discharge pass Example 8 703.9 3.0% 5B 0.615 Stable discharge pass Example 9 571.4 4.5% 4B 0.515 Stable discharge pass Example 10 651.8 3.7% 4B 0.524 Stable discharge pass Embodiment 11 803.6 3.0% 5B 0.789 Stable discharge pass Example 12 865.1 1.8% 5B 0.820 Stable discharge pass Embodiment 13 728.7 3.7% 5B 0.647 Stable discharge pass Embodiment 14 771.6 2.6% 5B 0.812 Stable discharge pass Embodiment 15 726.4 3.4% 5B 0.623 Stable discharge pass Comparative Example 1 734.5 3.3% 4B 0.676 High probability of blockage Not passed Comparative Example 2 708.3 3.3% 5B 0.571 Small probability of blockage Not passed Comparative Example 3 810.3 2.1% 5B 0.806 Small probability of blockage Not passed Comparative Example 4 720.2 3.5% 4B 0.463 Stable discharge Not passed Comparative Example 5 348.2 8.2% 3B 0.284 Small probability of blockage Not passed Comparative Example 6 1168.1 1.3% 2B — Unable to discharge Not passed Comparative Example 7 711.0 4.7% 4B 0.452 Stable discharge Not passed Comparative Example 8 979.5 2.7% 5B — Unable to discharge Not passed Comparative Example 9 787.7 2.3% 4B 0.623 Small probability of blockage Not passed Comparative Example 10 686.1 3.3% 5B 0.467 Stable discharge Not passed Comparative Example 11 612.5 14.9% 4B 0.457 Stable discharge Not passed

[0288]

Result Analysis

[0289] From the above results we can know:

[0290] Figure 7 The three-dimensional configuration diagram of the copper paste printing of Example 1 is shown. Combined with the data in the above table, it can be seen that the finished product meets the requirements of linear shrinkage below 5% after sintering, adhesion of 4B and above, aspect ratio above 0.5 and stable discharge during printing.

[0291] In the process of preparing copper powder, the reduction temperature in step (3) has a significant effect on the size of copper particles, which ultimately affects the stability of the slurry discharge. In Comparative Example 1, due to the low reaction temperature, the copper particles are not fully reduced, the copper cores are easy to agglomerate, and slowly grow in the later stage to form many large agglomerates, and there is a high probability of material blocking during the printing process; in Comparative Example 2, the reaction temperature of A-5 copper powder is too high, which accelerates the reaction rate of copper particles, and the nuclei cannot be slowly nucleated, but the particles grow rapidly, resulting in a larger particle size, so material blocking is likely to occur.

[0292] In the process of preparing copper powder, the temperature in step (5) affects the content of ligands in the system. In comparative example 4, the ligands are purified too thoroughly and cannot be effectively cross-linked with the organic carrier, resulting in a decrease in the adhesion of the final slurry and a significant decrease in conformity, resulting in a low aspect ratio of the printed sample.

[0293] The cross-linking reaction temperature affects the viscosity and conformality of the slurry. In Comparative Example 7, the cross-linking reaction temperature is low, resulting in an insufficiently tight connection between the particles, ligands and the organic carrier, reduced adhesion, and a low aspect ratio of the final sample. In Comparative Example 8, the cross-linking reaction temperature is too high, resulting in an excessively strong cross-linking reaction of the organic carrier, a significant increase in viscosity, and obstruction in the discharging process, resulting in the inability to discharging.

[0294] The solid content of the slurry affects the dispersion of the particles, thus affecting the stability of the material, and also affects the material shape retention and linear shrinkage after sintering. The solid content of the copper slurry in Comparative Example 5 is low, resulting in a linear shrinkage of >5% after sintering, severe slurry leveling, poor shape retention, and reduced adhesion. The three-dimensional configuration of the copper slurry printed in Comparative Example 5 is shown in Figure 2. Figure 8 As shown. In Comparative Example 6, the high solid content of the slurry causes the copper particles to be unable to be completely dispersed in the organic carrier, resulting in the inability to form a slurry that can be directly written and printed. The role of the active diluent is to cross-link with the ligand and the particles to enhance adhesion, and to reduce the solvent volatility after sintering while reducing the slurry concentration, thereby achieving a small linear shrinkage rate. In Comparative Example 9, no active diluent was added, resulting in an increase in slurry viscosity, a slight decrease in adhesion, a decrease in slurry dispersibility, and a blockage phenomenon.

[0295] A highly active hybrid epoxy resin that takes into account both the characteristics of alicyclic epoxy and glycidyl ester is preferred. After adding the organic carrier, the ligand is first heated at low temperature to fully crosslink with the hybrid epoxy resin and the curing agent to form a three-dimensional network structure. The initial viscosity is low, and after crosslinking, it drops to room temperature, the slurry viscosity increases and the shape retention is improved, and the copper particles are also well dispersed and are not easy to agglomerate into blocks. Comparative Example 10 Copper paste printing three-dimensional configuration diagram is shown in Fig. 9 As shown, the three-dimensional configuration diagram of copper paste printing in comparative example 11 is as follows Fig.10 The epoxy resin and acrylic resin in Comparative Examples 10 and 11 can provide some viscosity, but the cross-linking effect with the curing agent is poor and a three-dimensional grid structure cannot be formed, resulting in poor shape retention of the slurry and an aspect ratio of less than 0.5.

Claims

1. A copper paste suitable for three-dimensional configuration, characterized in that: According to weight percentage, it is composed of the following components: copper powder 70-90%, base resin 2-10%, curing agent 0.02-4%, active diluent 0.5-5%, dispersant 2-10%, thixotropic additive 0.6-10%, adhesion promoter 0.02-2%; The base resin is a mixed epoxy resin having both alicyclic epoxy groups and glycidyl ester groups; The surface of the copper powder is coated with an organic ligand; The copper powder is pre-reacted and cross-linked with the matrix resin, the active diluent and the curing agent, the pre-reaction and cross-linking temperature is any temperature of 55 to 65° C., and the pre-reaction and cross-linking time is any time of 5 to 15 minutes; The preparation method of the copper powder is as follows: (1) adding a solution containing an organic ligand and a copper salt dropwise into a solution containing a reducing agent at a reduction temperature of 50 to 80° C., so that the copper salt is reduced to prepare copper particles coated with organic ligands on the surface; (2) The prepared copper particles are washed by an alcohol solvent at 40-60° C., and the copper powder is obtained after washing.

2. The copper paste suitable for three-dimensional configuration according to claim 1, characterized in that: The curing agent is any one of methyltetrahydrophthalic anhydride, dicyandiamide, 2-ethyl-4-methylimidazole, mercaptan, 2-phenylimidazole, isocyanate, and boron amine complex, or any combination of multiple thereof.

3. The copper paste suitable for three-dimensional configuration according to claim 1, characterized in that: The active diluent is any one of butyl glycidyl ether, ethylene glycol diglycidyl ether, phenyl glycidyl ether, and o-cresyl glycidyl ether, or any combination of multiple thereof.

4. The copper paste suitable for three-dimensional configuration according to claim 1, characterized in that: The dispersant is any one of ethylene glycol ethyl ether acetate, dibasic acid ester, ethylene glycol monomethyl ether, n-butanol, diethylene glycol butyl ether, butyl carbitol acetate, dodecyl alcohol ester, dipropylene glycol methyl ether acetate, glycerol, isopropanol, and ethylene glycol, or any combination of multiple thereof.

5. The copper paste suitable for three-dimensional configuration according to claim 1, characterized in that: The thixotropic agent is any one of ethyl cellulose, fumed silica, tributyl citrate, polyamide wax, hydrogenated castor oil or hydroxyethyl cellulose or any combination of multiple thereof.

6. The copper paste suitable for three-dimensional configuration according to claim 1, characterized in that: The adhesion promoter is any one of a silane coupling agent and a titanate coupling agent or any combination of multiple thereof.

7. A method for preparing the copper slurry according to any one of claims 1 to 6, characterized in that: The following steps are involved: (S.1) Under the protection of inert gas, copper powder, base resin, curing agent, active diluent and dispersant are heated and stirred, so that the materials undergo pre-reaction cross-linking to obtain a mixed slurry; (S.2) adding a thixotropic agent and an adhesion promoter to the mixed slurry, and mixing the slurry so that the copper powder and the organic carrier are evenly dispersed to obtain a copper slurry with a high degree of crosslinking; (S.3) Grinding and filtering the copper paste with a high degree of cross-linking to obtain the copper paste suitable for three-dimensional configuration.

8. Use of the copper paste as claimed in any one of claims 1 to 6 in 3D printing of a three-dimensional metal grid with a large aspect ratio.