A cigarette smoke cooling material and its preparation method and application
By adsorbing a combination of the heat transfer shell by the hollow core of the low melting point metal heat absorption and the hollow sphere of the concave and concave rod, the problem of the impact of cooling materials on the flue gas concentration in the heating cigarette is solved, efficient cooling and self-circulation are achieved, and product quality is improved and stability.
Patent Information
- Application Number
- CN202310210733.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-07
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-03-07
AI Technical Summary
The existing cooling materials of heated cigarettes will affect the flue gas concentration when reducing the flue gas temperature, and the material stability and self-circulation ability are insufficient, affecting product quality.
The combination of low-melting point metal heat absorption hollow core and concave and concave rod hollow sphere adsorbs the heat transfer shell. Water molecules are adsorbed through the surface of the concave and concave rod hollow sphere and conducts the flue gas temperature. The low-melting point metal absorbs heat, achieving efficient cooling and ensuring material stability .
Effectively reduce the temperature of cigarette smoke, avoid excessive flue gas temperature affecting the taste, realize self-circulation, stable product and low cost, and are suitable for the field of filtration and cooling of cigarette smoke.
Smart Images

Figure CN116326822B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of filtering and cooling materials, and relates to a cigarette smoke cooling material and a preparation method and application thereof. Background Art
[0002] Heated cigarettes are an important form of new tobacco products. They mainly release aerosols by heating tobacco materials through heating distillation (below 500°C). Compared with traditional cigarettes, heated cigarettes only heat tobacco materials instead of burning them, which reduces the harmful components produced during the high-temperature combustion of tobacco, and the release of sidestream smoke and environmental smoke is also significantly reduced. Although mainstream heated cigarettes in the international market, such as Philip Morris International's iQOS, British American Tobacco's Glo, and Japan Tobacco's Ploom Tech, have been hot-selling, domestic research on heated cigarettes is still in the research and development stage. Because heated cigarettes are shorter, the inlet smoke temperature is too hot. In response to this, various tobacco companies have adopted different solutions in the design of the cooling section of cigarettes. For example, embossed gathered PLA film, fiber woven bundles with cooling effect, embossed gathered aluminum foil composite paper and cooling cavity firmware are used.
[0003] In general, smoke cooling measures are mainly focused on two aspects: cooling by adding cooling materials and designing cooling structures. In terms of material cooling, heat absorbing materials, heat storage materials, heat conductive materials, etc. can all be used to heat cigarette smoke and cool it down to achieve the transfer of smoke heat. This method is also the most important research method at present.
[0004] CN108576918A discloses a low-temperature cigarette with a cooling section. The cooling section is injection molded by mixing polylactic acid and polyethylene in a certain mass ratio. The smoke flowing in from the tobacco section flows out from the mouthpiece after passing through the cooling section. The cooling section is formed with pores for smoke circulation. CN109674085A discloses a heat storage capsule for reducing the temperature of mainstream cigarette smoke and its preparation and application, including a wall material and a core material, and the wall material is polylactic acid. When high-temperature smoke passes through a polylactic acid polymer, the polylactic acid undergoes a glass transition and absorbs heat, consuming the heat energy of the smoke. On the other hand, when water vapor in the smoke passes through the polylactic acid polymer, it condenses on its surface, causing the smoke to be dried. However, after the polylactic acid sheet comes into contact with high-temperature flue gas and undergoes a glass transition, melting and bonding will occur, blocking the longitudinally extending flue gas channel, and the flue gas will no longer flow through the inside of the polylactic acid sheet. At the same time, polylactic acid materials will also have a partial adsorption effect on glycerol in the flue gas, reducing the glycerol content in the flue gas and causing a decline in the smoking quality.
[0005] In addition to adding heat-absorbing, heat-storing and heat-conducting additives to heated cigarettes to reduce smoke temperature, the smoke cooling effect can also be enhanced by adjusting the cigarette structure, such as using cavities to buffer heat storage, lengthening smoke channels, and enhancing heat exchange between smoke and the external environment. The above cooling measures can partially reduce smoke temperature, but there are still certain shortcomings.
[0006] Although existing cooling materials can achieve a good cooling effect, they will also have an adsorption effect on glycerin, thereby reducing the quality of flue gas, and there are problems such as adhesion during the use of the materials. Although cooling through structural design has little effect on the flue gas concentration, the cooling effect is limited.
[0007] In summary, it is a technical problem to be urgently solved in this field to study a self-circulating cooling material that can effectively reduce the smoke temperature without affecting the smoke concentration, has high material stability, can be self-circulated and has great practical significance for improving the quality of heated cigarette products. Summary of the invention
[0008] The object of the present invention is to provide a cigarette smoke cooling material and a preparation method and application thereof, so as to reduce the smoke temperature and avoid the smoke temperature being too high and affecting the taste.
[0009] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0010] One of the purposes of the present invention is to provide a cigarette smoke cooling material, which comprises a heat-absorbing hollow core and an adsorption heat-transfer shell. The material of the heat-absorbing hollow core comprises a bismuth-lead-tin-indium alloy, and the material of the adsorption heat-transfer shell comprises a convexographite hollow ball.
[0011] The heat-absorbing hollow core of the present invention is a low-melting-point metal heat-absorbing hollow core. The cigarette smoke cooling material of the present invention absorbs water molecules in the smoke through the hydrophilicity of the surface of the hollow attapulgite balls, and transmits the smoke temperature to the inside. The low-melting-point metal heat-absorbing core absorbs the heat of the smoke and consumes the heat by melting, thereby achieving the purpose of reducing the smoke temperature and avoiding the effect of excessive smoke temperature on the taste. The cigarette smoke cooling material can significantly reduce the temperature of cigarette smoke, and can achieve self-circulation use, the product is stable, the cost is low, and it can be widely used in the field of cigarette smoke filtration and cooling.
[0012] In the present invention, a hollow attapulgite ball adsorption heat transfer shell is adopted. On the one hand, attapulgite has high mechanical strength and thermal stability, which can ensure that the material will not be damaged during the preparation and use process and has good stability; on the other hand, the hollow attapulgite ball has a small diameter, abundant internal pores, and a large specific surface area, which can realize efficient heat conduction between the cigarette smoke outside the shell and the low-melting-point metal heat-absorbing hollow core, and after the surface of the hollow attapulgite ball shell is modified, its hydrophilicity can be used to reduce the adsorption performance of the cigarette oil, improve the adsorption of water vapor in the smoke, and avoid the reduction of the smoke suction quality; the low-melting-point metal heat-absorbing hollow core is adopted As a heat absorbing material, it can efficiently transfer heat when the smoke temperature is lower than the melting point of the mixed metal, and can absorb a large amount of heat by utilizing the mixed metal to transform from solid phase to liquid phase when the smoke temperature is higher than the melting point of the mixed metal, thereby quickly adjusting the smoke temperature; in addition, during the intervals between smoking, the temperature of the filter mouthpiece drops, and the low-melting-point metal heat-absorbing hollow core turns back into a solid phase, realizing the self-circulation of the cooling material during the smoking process; through the combined use of the attapulgite hollow ball adsorption heat transfer shell and the low-melting-point metal heat-absorbing hollow core, the cooling material can significantly reduce the cigarette smoke temperature, realize self-circulation and stable product performance.
[0013] As a preferred technical solution of the present invention, the mass ratio of bismuth metal, lead metal, tin metal and indium metal in the bismuth-lead-tin-indium alloy is (38-43):(25-28):(13-15):(14-24), wherein the mass ratio can be 38:25:15:22, 40:25:14:21, 43:28:13:16 or 42:26:14:18, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0014] As a preferred technical solution of the present invention, the diameter of the attapulgite hollow sphere is 2 to 4 mm, wherein the diameter can be 2 mm, 2.2 mm, 2.4 mm, 2.6 mm, 2.8 mm, 3.0 mm, 3.2 mm, 3.4 mm, 3.6 mm, 3.8 mm or 4 mm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0015] Preferably, the thickness of the attapulgite hollow sphere is 0.2-1 mm, wherein the thickness may be 0.2 mm, 0.3 mm, 0.4 mm, 0.5 mm, 0.6 mm, 0.7 mm, 0.8 mm, 0.9 mm or 1 mm, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0016] As a preferred technical solution of the present invention, the mass ratio of the heat-absorbing hollow inner core and the adsorption heat-transfer outer shell is (0.5-1):3, wherein the mass ratio can be 0.5:3, 0.6:3, 0.7:3, 0.8:3, 0.9:3 or 1:3, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0017] A second object of the present invention is to provide a method for preparing the cigarette smoke cooling material as described in the first object, the preparation method comprising:
[0018] (1) After first heating paraffin and bismuth metal, lead metal, tin metal and indium metal are added in sequence and then second heated to obtain a molten mixed metal, the molten mixed metal is dripped into a hollow ball mold, and cooled to obtain the heat-absorbing hollow core particles;
[0019] (2) adding attapulgite powder to deionized water and mixing, and then printing and sintering in sequence to obtain a hemispherical attapulgite shell, and then immersing and drying the hemispherical attapulgite shell in a silane coupling agent to obtain a surface-modified hemispherical attapulgite shell;
[0020] (3) placing the heat-absorbing hollow core particles of step (1) inside any one of the surface-modified hemispherical attapulgite shells of step (2), and encapsulating them with another surface-modified hemispherical attapulgite shell to obtain the cigarette smoke cooling material.
[0021] As a preferred technical solution of the present invention, the mass ratio of paraffin and bismuth metal in step (1) is (1-3):1, wherein the mass ratio can be 1:1, 2:1 or 3:1, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0022] Preferably, the temperature of the first heating in step (1) is 270-290°C, wherein the temperature can be 270°C, 272°C, 274°C, 276°C, 278°C, 280°C, 282°C, 284°C, 286°C, 288°C or 290°C, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0023] Preferably, the temperature of the second heating in step (1) is 340-360°C, wherein the temperature can be 340°C, 342°C, 344°C, 346°C, 348°C, 350°C, 352°C, 354°C, 356°C, 358°C or 360°C, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0024] Preferably, the second heating time in step (1) is 25 to 35 min, wherein the time can be 25 min, 26 min, 27 min, 28 min, 29 min, 30 min, 31 min, 32 min, 33 min, 34 min or 35 min, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0025] Preferably, the hollow ball mold in step (1) is a hemispherical attapulgite mold with a diameter of 1.9 to 3.9 mm and an internal solid sphere with a diameter of 1.8 to 3.8 mm, wherein the diameter of the hollow ball mold is 1.9 mm, 2.0 mm, 2.1 mm, 2.2 mm, 2.3 mm, 2.4 mm, 2.5 mm, 2.6 mm, 2.7 mm, 2.8 mm, 2.9 mm, 3.0 mm, 3.1 mm, 3.2 mm, 3.3 mm, 3.4 mm, 3.5 mm, 3.6 mm, 3.7 mm, 3.8 mm or 3.9 mm, etc., wherein the diameter of the internal solid sphere can be 1.8 mm, 2.0 mm, 2.4 mm, 2.6 mm, 2.8 mm, 3.0 mm, 3.2 mm, 3.4 mm, 3.6 mm or 3.8 mm, etc., but is not limited to the listed values, and other values not listed within the above numerical ranges are also applicable.
[0026] As a preferred technical solution of the present invention, the mass ratio of the attapulgite powder and deionized water in step (2) is 100:(23-28), wherein the mass ratio can be 100:23, 100:24, 100:25, 100:26, 100:27 or 100:28, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0027] Preferably, printing is performed when the liquid index of the mixed solution in step (2) reaches 0.25 to 0.30, wherein the liquid index can be 0.25, 0.26, 0.27, 0.28, 0.29 or 0.30, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0028] Preferably, the printing in step (2) is 3D printing.
[0029] Preferably, after printing in step (2), a precursor of a hemispherical attapulgite shell is obtained.
[0030] Preferably, the diameter of the precursor of the hemispherical attapulgite shell is 2 to 4 mm, wherein the diameter may be 2 mm, 3 mm or 4 mm, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0031] Preferably, the thickness of the precursor of the hemispherical attapulgite shell is 0.2 to 1 mm, wherein the thickness can be 0.2 mm, 0.3 mm, 0.4 mm, 0.5 mm, 0.6 mm, 0.7 mm, 0.8 mm, 0.9 mm or 1 mm, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0032] Preferably, the sintering temperature in step (2) is 700-900°C, wherein the temperature can be 700°C, 720°C, 740°C, 760°C, 780°C, 800°C, 820°C, 840°C, 860°C, 880°C or 900°C, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0033] Preferably, the sintering time in step (2) is 4 to 8 hours, wherein the time can be 4 hours, 5 hours, 6 hours, 7 hours or 8 hours, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0034] As a preferred technical solution of the present invention, the silane coupling agent in step (2) is isobutyltriethoxysilane.
[0035] Preferably, the mass ratio of the hemispherical attapulgite shell and the silane coupling agent in step (2) is 1:(5-10), wherein the mass ratio can be 1:5, 1:6, 1:7, 1:8, 1:9 or 1:10, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0036] Preferably, the immersion time in step (2) is 25 to 35 min, wherein the time can be 25 min, 26 min, 27 min, 28 min, 29 min, 30 min, 31 min, 32 min, 33 min, 34 min or 35 min, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0037] Preferably, the drying temperature in step (2) is 30-40°C, wherein the temperature can be 30°C, 31°C, 32°C, 33°C, 34°C, 35°C, 36°C, 37°C, 38°C, 39°C or 40°C, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0038] Preferably, the drying time in step (2) is 20 to 28 hours, wherein the time can be 20 hours, 21 hours, 22 hours, 23 hours, 24 hours, 25 hours, 26 hours, 27 hours or 28 hours, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0039] As a preferred technical solution of the present invention, in step (3), the joints of the two hemispherical attapulgite shells are bonded with adhesive.
[0040] A third object of the present invention is to provide an application of the cigarette smoke cooling material as described in the first object, wherein the cigarette smoke cooling material is applied in the technical field of filtering and cooling materials.
[0041] Compared with the prior art, the present invention has the following beneficial effects:
[0042] The cooling material in the present invention is composed of a low-melting-point metal heat-absorbing hollow core and a attapulgite hollow ball adsorption heat-transfer shell. The attapulgite hollow ball surface hydrophilicity adsorbs water molecules in the smoke and conducts the smoke temperature to the inside. The low-melting-point metal heat-absorbing core absorbs the heat of the smoke and consumes the heat by melting, thereby achieving the purpose of reducing the smoke temperature and avoiding excessive smoke temperature affecting the taste. The cigarette smoke cooling material can significantly reduce the cigarette smoke temperature and can achieve self-circulation. The product is stable and low in cost. It can be widely used in the field of cigarette smoke filtration and cooling; the maximum temperature of the cigarette containing the cooling material when smoking is ≤47.6℃. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 This is a temperature test result diagram of the original cigarette during the smoking process in Comparative Example 1 of the present invention.
[0044] Figure 2 This is a graph showing the temperature test results of a cigarette containing the cooling material in Example 1 of the present invention during smoking.
[0045] Figure 3 This is a graph showing the temperature test results of a cigarette containing the cooling material in Example 2 of the present invention during smoking.
[0046] Figure 4 This is a graph showing the temperature test results of a cigarette containing the cooling material in Example 3 of the present invention during smoking. DETAILED DESCRIPTION
[0047] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0048] Example 1
[0049] The present embodiment provides a cigarette smoke cooling material, which is composed of a low-melting-point metal heat-absorbing hollow inner core and a attapulgite hollow ball adsorption heat-transfer outer shell; the attapulgite hollow ball has a diameter of 2 mm and a thickness of 0.2 mm, and the mass ratio of the low-melting-point metal heat-absorbing hollow inner core / attapulgite hollow ball adsorption heat-transfer outer shell is 1:3.
[0050] This embodiment provides a method for preparing a cigarette smoke cooling material, which specifically includes the following steps:
[0051] (1) Weigh 3.8 g of paraffin wax and 3.8 g of bismuth, mix them, heat to 280° C. to melt the paraffin wax and bismuth, then add 2.5 g of lead, 1.3 g of tin, and 2.4 g of indium, respectively, increase the heating temperature to 350° C. and keep warm for 30 min to melt and mix all the metals, finally drop the mixed metals into a hollow ball mold, and after the mixed metals are completely cooled, obtain low-melting-point metal endothermic hollow core particles, the hollow ball mold is a hemispherical attapulgite mold with a diameter of 1.9 mm and an inner solid sphere with a diameter of 1.8 mm;
[0052] (2) After adding 100 g of attapulgite powder to 23 g of deionized water, the mixture was stirred and kneaded until its liquid index reached 0.25, and then printed using a 3D printer (model SLX-DY2020, brand Shui Liuxing Ceramics Museum) at a printing speed of 2.5 cm 2 / h, a hemispherical attapulgite shell with a diameter of 2mm and a thickness of 0.2mm is obtained, and then the hemispherical attapulgite shell is placed in a muffle furnace and calcined at 700℃ for 8h to obtain a plurality of hemispherical attapulgite shells with a mass of about 10mg. 30 hemispherical attapulgite shells (300mg in total) are placed in 1500mg of isobutyltriethoxysilane, immersed for 30min, taken out and dried at 30℃ for 24h to obtain a surface-modified hemispherical attapulgite shell;
[0053] (3) Weigh 6.7 mg of the low-melting-point metal heat-absorbing hollow core particles obtained in step (1) and place them inside the surface-modified hemispherical attapulgite shell obtained in step (2), then encapsulate it with another hemispherical attapulgite shell, and apply a layer of tobacco hot melt adhesive at the joint of the two hemispherical attapulgite shells to obtain one cigarette smoke cooling material. Repeat step (3) to obtain 10 cooling materials and place them in the cigarette cooling area.
[0054] Example 2
[0055] The present embodiment provides a cigarette smoke cooling material, which is composed of a low-melting-point metal heat-absorbing hollow inner core and a attapulgite hollow ball adsorption heat-transfer outer shell; the attapulgite hollow ball has a diameter of 4 mm and a thickness of 1 mm, and the mass ratio of the low-melting-point metal heat-absorbing hollow inner core / attapulgite hollow ball adsorption heat-transfer outer shell is 0.5:3.
[0056] This embodiment provides a method for preparing a cigarette smoke cooling material, which specifically includes the following steps:
[0057] (1) Weighing 12.9 g of paraffin and 4.3 g of bismuth, mixing them, heating to 280° C. to melt the paraffin and bismuth, then adding 2.8 g of lead, 1.5 g of tin, and 1.4 g of indium, respectively, raising the heating temperature to 350° C. and keeping the temperature for 30 min to melt and mix all the metals, finally dropping the mixed metals into a hollow ball mold, and after the mixed metals are completely cooled, obtaining low-melting-point metal endothermic hollow core particles, the hollow ball mold is a hemispherical attapulgite mold with a diameter of 3.9 mm and an inner solid sphere with a diameter of 3.8 mm;
[0058] (2) After adding 100 g of attapulgite powder to 28 g of deionized water, the mixture was stirred and kneaded until its liquid index reached 0.30, and then printed using a 3D printer (model SLX-DY2020, brand Shui Liuxing Ceramics Museum) at a printing speed of 2.5 cm 2 / h, to obtain a hemispherical attapulgite shell with a diameter of 4mm and a thickness of 1mm, and then place the hemispherical attapulgite shell in a muffle furnace and calcine at 900°C for 4h to obtain a plurality of hemispherical attapulgite shells with a mass of about 25mg; take 30 obtained hemispherical attapulgite shells (750mg in total) and place them in 3750mg of isobutyltriethoxysilane, after immersing for 30min, take them out and dry them at 40°C for 24h to obtain a surface-modified hemispherical attapulgite shell;
[0059] (3) Weigh 8.3 mg of the low-melting-point metal heat-absorbing hollow core particles obtained in step (1) and place them inside the surface-modified hemispherical attapulgite shell obtained in step (2), then encapsulate it with another hemispherical attapulgite shell, and apply a layer of hot melt adhesive for cigarettes at the joint of the two hemispherical attapulgite shells to obtain one cigarette smoke cooling material. Repeat step (3) to obtain 10 cooling materials and place them in the cigarette cooling area.
[0060] Example 3
[0061] The present embodiment provides a cigarette smoke cooling material, which is composed of a low-melting-point metal heat-absorbing hollow inner core and a attapulgite hollow ball adsorption heat-transfer outer shell; the diameter of the attapulgite hollow ball is 3 mm and the thickness is 0.5 mm, and the mass ratio of the low-melting-point metal heat-absorbing inner core / attapulgite hollow ball adsorption heat-transfer outer shell is 0.75:3.
[0062] This embodiment provides a method for preparing a cigarette smoke cooling material, which specifically includes the following steps:
[0063] (1) Weigh 7.6 g of paraffin and 3.8 g of bismuth and mix them, heat them to 280° C. to melt the paraffin and bismuth, then add 2.8 g of lead, 1.3 g of tin, and 2.4 g of indium, respectively, increase the heating temperature to 350° C. and keep warm for 30 min to melt and mix all the metals, finally drop the mixed metals into a hollow ball mold, and after the mixed metals are completely cooled, obtain low-melting-point metal endothermic hollow core particles, the hollow ball mold is a hemispherical attapulgite mold with a diameter of 2.9 mm, and the inner solid sphere is a hemispherical attapulgite mold with a diameter of 2.8 mm;
[0064] (2) After adding 100 g of attapulgite powder to 28 g of deionized water, the mixture was stirred and kneaded until its liquid index reached 0.30, and then printed using a 3D printer (model SLX-DY2020, brand Shui Liuxing Ceramics Museum) at a printing speed of 2.5 cm 2 / h, to obtain a hemispherical attapulgite shell with a diameter of 3 mm and a thickness of 0.5 mm, and then place the hemispherical attapulgite shell in a muffle furnace and calcine at 900°C for 8 hours to obtain a plurality of hemispherical attapulgite shells with a mass of about 15 mg, take 30 of the obtained hemispherical attapulgite shells (a total of 450 mg) and place them in 4500 mg of isobutyltriethoxysilane, after immersion for 30 minutes, take out and dry at 40°C for 24 hours to obtain a hemispherical attapulgite shell after surface modification;
[0065] (3) Weigh 7.5 mg of the low-melting-point metal heat-absorbing hollow core particles obtained in step (1) and place them inside the surface-modified hemispherical attapulgite shell obtained in step (2), then encapsulate it with another hemispherical attapulgite shell, and apply a layer of tobacco hot melt adhesive at the joint of the two hemispherical attapulgite shells to obtain one cigarette smoke cooling material. Repeat step (3) to obtain 10 cooling materials and place them in the cigarette cooling area.
[0066] Comparative Example 1
[0067] This comparative example uses the original cigarette (i.e., the original cigarette without adding cooling material) as comparative example 1.
[0068] The smoke temperature of the cigarette smoke cooling materials provided in Examples 1-3 and Comparative Example 1 was tested. The test results are as follows: Figure 2-4 and Figure 1 shown.
[0069] The test method is as follows: simulate smoking according to the cigarette smoking mode specified in the national standard YC / T29-1996, use a K-type thermocouple temperature detector to detect the temperature at the center of the cigarette filter rod 2mm away from the mouth end when the cigarette is smoked, simulate smoking 9 times, each smoking interval is 30s, and record the highest temperature;
[0070] Among them, the temperature test results of the original smoke during the smoking process are shown in the figure below: Figure 1As shown;
[0071] The temperature test results of the cigarette including the cooling material provided in Example 1 during the smoking process are shown in the figure below: Figure 2 As shown;
[0072] The temperature test results of the cigarette including the cooling material provided in Example 2 during the smoking process are shown in the figure below: Figure 3 As shown;
[0073] The temperature test results of the cigarette including the cooling material provided in Example 3 during the smoking process are shown in the figure below: Figure 4 shown.
[0074] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. A cigarette smoke cooling material, It is characterized in that The cigarette smoke cooling material comprises a heat-absorbing hollow core and an adsorption heat-conducting outer shell, the material of the heat-absorbing hollow core comprises a bismuth-lead-tin-indium alloy, and the material of the adsorption heat-conducting outer shell comprises a attapulgite hollow ball.
2. The cigarette smoke cooling material according to claim 1, It is characterized in that The mass ratio of bismuth metal, lead metal, tin metal and indium metal in the bismuth-lead-tin-indium alloy is (38-43):(25-28):(13-15):(14-24).
3. The cigarette smoke cooling material according to claim 1, It is characterized in that The diameter of the attapulgite hollow sphere is 2 to 4 mm.
4. The cigarette smoke cooling material according to claim 1, It is characterized in that The thickness of the attapulgite hollow sphere is 0.2-1 mm.
5. The cigarette smoke cooling material according to claim 1, It is characterized in that The mass ratio of the heat-absorbing hollow inner core to the adsorption heat-conducting outer shell is (0.5-1):
3.
6. A method for preparing the cigarette smoke cooling material according to any one of claims 1 to 5, It is characterized in that The preparation method comprises: (1) After first heating paraffin and bismuth metal, lead metal, tin metal and indium metal are added in sequence and then second heated to obtain a molten mixed metal, the molten mixed metal is dripped into a hollow ball mold, and cooled to obtain the heat-absorbing hollow core particles; (2) adding attapulgite powder to deionized water and mixing, and then printing and sintering in sequence to obtain a hemispherical attapulgite shell, and then immersing and drying the hemispherical attapulgite shell in a silane coupling agent to obtain a surface-modified hemispherical attapulgite shell; (3) placing the heat-absorbing hollow core particles of step (1) inside any one of the surface-modified hemispherical attapulgite shells of step (2), and encapsulating them with another surface-modified hemispherical attapulgite shell to obtain the cigarette smoke cooling material.
7. The preparation method according to claim 6, It is characterized in that The mass ratio of paraffin wax to bismuth metal in step (1) is (1-3):
1.
8. The preparation method according to claim 6, It is characterized in that The first heating temperature in step (1) is 270-290°C.
9. The preparation method according to claim 6, It is characterized in that The temperature of the second heating in step (1) is 340-360°C.
10. The preparation method according to claim 6, It is characterized in that The second heating time in step (1) is 25 to 35 minutes.
11. The preparation method according to claim 6, It is characterized in that The hollow ball mold in step (1) is a hemispherical attapulgite mold with a diameter of 1.9 to 3.9 mm and an inner solid sphere with a diameter of 1.8 to 3.8 mm.
12. The preparation method according to claim 6, It is characterized in that The mass ratio of the attapulgite powder to deionized water in step (2) is 100:(23-28).
13. The preparation method according to claim 6, It is characterized in that When the liquid index of the mixed solution in step (2) reaches 0.25 to 0.30, printing is performed.
14. The preparation method according to claim 6, It is characterized in that The printing in step (2) is 3D printing.
15. The preparation method according to claim 6, It is characterized in that After printing in step (2), a precursor of a hemispherical attapulgite shell is obtained.
16. The preparation method according to claim 15, It is characterized in that The diameter of the precursor of the hemispherical attapulgite shell is 2 to 4 mm.
17. The preparation method according to claim 15, It is characterized in that The thickness of the precursor of the hemispherical attapulgite shell is 0.2-1 mm.
18. The preparation method according to claim 6, It is characterized in that The sintering temperature in step (2) is 700-900°C.
19. The preparation method according to claim 6, It is characterized in that The sintering time in step (2) is 4 to 8 hours.
20. The preparation method according to claim 6, It is characterized in that The silane coupling agent in step (2) is isobutyltriethoxysilane.
21. The preparation method according to claim 6, It is characterized in that The mass ratio of the hemispherical attapulgite shell to the silane coupling agent in step (2) is 1:(5-10).
22. The preparation method according to claim 6, It is characterized in that The immersion time in step (2) is 25 to 35 minutes.
23. The preparation method according to claim 6, It is characterized in that The drying temperature in step (2) is 30-40°C.
24. The preparation method according to claim 6, It is characterized in that The drying time in step (2) is 20 to 28 hours.
25. The preparation method according to claim 6, It is characterized in that Step (3) The joints of the two hemispherical attapulgite shells are bonded with adhesive.
26. An application of the cigarette smoke cooling material according to any one of claims 1 to 5, It is characterized in that The cigarette smoke cooling material is applied to the technical field of filtering cooling materials.