Electrochromic glass and method for manufacturing the same
By printing electrodes and electrochromic layers on the surface of curved glass and using suction cup flattening technology, the wrinkle problem in electrochromic glass composite sheets is solved, reducing production costs and expanding the application range, and suitable for complex curvature products.
Patent Information
- Application Number
- CN202310423143.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-19
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-04-19
AI Technical Summary
Existing electrochromic glasses are prone to wrinkle defects when combined with complex curved glass sheets, resulting in high production costs and limited application range.
By printing electrodes and electrochromic layers on the curved glass surface, then performing glass sheets, avoiding the use of electrochromic films, and printing with a suction cup flat glass surface to ensure the stability and uniformity of the printing layer, suitable for more complex or Products with variable curvature.
It effectively avoids the wrinkles caused by electrochromic films in the film combinatorial process, reduces production costs, expands the application range of products, and is suitable for complex curvature products such as skylights and door glasses.
Smart Images

Figure CN116339030B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of vehicle glass, and in particular to an electrochromic glass and a manufacturing method thereof. Background Art
[0002] Electrochromic glass is generally achieved by compounding a layer of electrochromic film between two pieces of glass, and under the action of an external electric field, the color and transparency change effect is achieved. The conductive material layer is usually indium tin oxide (ITO), which is relatively expensive. In addition, in the application process of automotive glass products, when the electrochromic film is combined with complex curved glass, the poor fit between the two will cause wrinkle appearance defects. In order to improve the wrinkle defect, edge digging and other methods are generally used for improvement. The process operation process is complicated, defective products are produced, and production costs are increased.
[0003] Therefore, at this stage, it is necessary to reduce the production cost of electrochromic products and improve the cost-effectiveness of electrochromic glass products, so as to promote the application of electrochromic products in the automotive field on a larger scale, such as complex curvature products: sunroofs, door glass, etc. Summary of the invention
[0004] In order to solve the problem that the electrochromic film and glass are prone to wrinkles during the lamination process in the prior art, the present invention provides an electrochromic glass and a manufacturing method thereof. The present invention obtains an electrochromic glass product by printing electrodes and an electrochromic layer on the surface of the curved glass and then laminating the glass, avoiding the use of an electrochromic film (such as an EC film), thereby avoiding or slowing down the generation of wrinkles in the electrochromic film during the lamination process; and there is no need to specially customize an electrochromic film that matches the curvature of the glass, so the application range is wider and it can be applied to products with more complex or variable curvatures.
[0005] In order to achieve the above purpose, the present invention adopts the following technical solutions:
[0006] In one aspect, the present invention provides a method for manufacturing electrochromic glass, the manufacturing method comprising the following steps:
[0007] A first curved glass substrate is sucked flat with a suction cup, and a first electrode, an electrochromic layer, and a second electrode are printed in sequence on one surface of the first glass substrate; the first glass substrate and a second curved glass substrate are bonded together with an intermediate layer adhesive material so that the first electrode, the electrochromic layer, and the second electrode are sandwiched between the two glass substrates to obtain the electrochromic glass.
[0008] According to the manufacturing method of the present invention, preferably, the main curvature radius of the electrochromic glass is 1200 mm to 3000 mm.
[0009] According to the manufacturing method of the present invention, preferably, the printing specifically includes the following processes:
[0010] Using the suction cup to suck the first glass substrate flat, and then printing the first electrode on one surface of the first glass substrate; after printing, restoring the curvature of the first glass substrate, and then drying;
[0011] Repeatedly using the suction cup to suck the first glass substrate flat, printing the electrochromic layer on the first electrode, restoring the curvature of the first glass substrate after printing, and then drying;
[0012] Repeatedly using the suction cup to suck the first glass substrate flat, printing the second electrode on the electrochromic layer, restoring the curvature of the first glass substrate after printing, and then drying;
[0013] Sintering is performed to complete the solidification of the first electrode, the electrochromic layer and the second electrode.
[0014] The printing area of the present invention is relatively large and is basically consistent with the glass substrate. After each printing is completed, the curvature of the glass substrate is restored and then dried. During this process, the large-area printing layer will not be broken; after all printing is completed, sintering is performed to ensure the stability of the printing layer.
[0015] According to the manufacturing method of the present invention, preferably, the suction cup is adsorbed onto the convex surface of the first glass substrate and sucked flat, and then the printing is performed on the concave surface of the first glass substrate.
[0016] Due to the complex curvature of curved glass, the use of traditional screen printing technology may result in uneven printing thickness of the conductive layer, causing voltage fluctuations and affecting the electrochromic effect. The present invention uses a suction cup to flatten the curved glass before each printing, so that the curved glass is flattened before printing, thereby avoiding the problem of uneven printing thickness. In the process of flattening the curved glass, if the curved glass is deformed unevenly, there may be a risk of cracking; the present invention solves the possible risk of cracking through the specific setting of the suction cup. For glass substrates with an aspect ratio of approximately 1:1 to 1:4, the present invention preferably uses a plurality of suction cups to be arranged in a row along the central axis consistent with the length direction of the first glass substrate and simultaneously adsorb the convex surface of the first glass substrate.
[0017] Setting too many suction cups will lead to linear concentration of pressure distribution of adsorbed glass, uneven distribution of adsorption pressure and excessive adsorption pressure, which will cause glass breakage during adsorption process; too few suction cups are not enough to completely suck the glass flat, affecting the subsequent printing effect. According to the current conventional glass size, the number of suction cups is generally 2 to 4, among which 3 suction cups are set to achieve the best flattening effect. Therefore, preferably, three suction cups are arranged in a row along the central axis consistent with the length direction of the first glass substrate to adsorb the convex surface of the first glass substrate at the same time; the middle suction cup of the three suction cups is located in the middle position, and the two side suction cups on both sides are symmetrically arranged; that is, the left and right suction cups are at the same distance from the edge of the glass, and the left and right suction cups are also at the same distance from the middle suction cup. On the central axis, the distance ratio of the side suction cup to the edge of the glass to the middle suction cup is 2:1 to 2:4, and the most preferred ratio is 2:3. That is, assuming that the distance between the side suction cup and the glass edge of the first glass substrate is X, and the distance between the side suction cup and the middle suction cup is Y, 2X+2Y is the length of the first glass (the measurement of X and Y is based on the center of the suction cup), and X:Y=2:3; at this time, the curved glass will obtain uniform deformation and will not cause the glass to crack, while achieving the best leveling effect; more importantly, under this leveling effect, there will be no risk of cracking during the printing process.
[0018] According to the manufacturing method of the present invention, preferably, the drying temperature is 140-180° C. and the drying time is 2 min-3 min.
[0019] According to the manufacturing method of the present invention, preferably, the sintering temperature is 550-640° C. and the sintering time is 4 min-6 min.
[0020] According to the manufacturing method of the present invention, corresponding to the specified drying and sintering conditions, preferably, the thickness of the first electrode and the second electrode obtained by printing is independently 8μm to 12μm; the thickness of the electrochromic layer is 3μm to 7μm; the total thickness of the first electrode, the electrochromic layer and the second electrode is ≤30μm. When the thickness exceeds 30μm, the printed layer may break or the glass may crack. For example, in the process of flattening to restoring the original curvature, the electrode layer and the electrochromic layer may break or the glass may crack. The electrode layer and the electrochromic layer may break during the sintering process.
[0021] According to the manufacturing method of the present invention, preferably, the printing adopts a screen printing process or an inkjet printing process; wherein the thickness of the printed layer formed by the inkjet printing process can be thinner, but the cost is higher; the present invention more preferably adopts a screen printing process.
[0022] According to the manufacturing method of the present invention, preferably, the first electrode and the second electrode are printed using silver paste. More preferably, the silver paste comprises 50wt.% to 85wt.% silver powder, 1wt.% to 3wt.% glass powder and 12wt.% to 48wt.% oil. The electrodes printed by the silver paste with the preferred composition have better conductive stability.
[0023] The electrochromic layer contains an electrochromic material capable of electrochromic change, and the electrochromic material is an organic material or an inorganic material. As an inorganic material, a metal oxide can be used. ① Reductive electrochromic material: for example, formed by vanadium oxide, niobium oxide, indium oxide, iridium oxide, nickel oxide, cobalt oxide, molybdenum oxide or a mixture of several thereof. ② Oxidative electrochromic material: for example, oxides of Cr, Mn, Fe, Co, Ni, Rh or Ir; hydroxides of Cr, Mn, Fe, Co, Ni, Rh or Ir; and Prussian blue. LiNiOx, IrO2, NiO, V2O5, LixCoO2, Rh2O3 or CrO3 can also be used. After the electrode is applied with voltage, the substances in the electrochromic layer undergo a chemical reaction, so that the glass presents a specific color; the magnitude of the voltage affects the depth of the color of the electrochromic layer, and the depth of the color is adjusted by controlling the magnitude of the voltage (for example, gradually increasing the voltage at a voltage interval of 1V to 5V). After power is cut off, the electrochromic layer begins a reversible reaction and the color of the glass returns to its initial state.
[0024] According to the manufacturing method of the present invention, preferably, the intermediate layer adhesive material is PVB or EVA.
[0025] According to the manufacturing method of the present invention, preferably, the printing adopts a screen printing process, and the printing parameters include: a printing speed of (400±50) mm / s, a printing pressure of 0.2MPa~0.5MPa, and a viscosity of the printing material of 25Pa.s~50Pa.s. This parameter setting can effectively deposit the silver paste and the printing material of the electrochromic layer on the glass surface, and can well control the printing thickness of each layer within the specified range. The present invention limits the specific setting of the suction cup to ensure that the curved glass that is sucked flat during the printing process under the printing parameters will not have the risk of cracking.
[0026] Another aspect of the present invention provides an electrochromic glass obtained by the above manufacturing method.
[0027] According to the electrochromic glass of the present invention, preferably, the thickness of the first glass substrate and the second glass substrate are independently 1.8 mm to 2.5 mm; and the thickness of the intermediate layer adhesive material is 0.2 mm to 1.0 mm.
[0028] The present invention obtains an electrochromic glass product by printing electrodes and an electrochromic layer on the surface of curved glass and then laminating the glass, avoiding the use of an electrochromic film (such as an EC film), thereby avoiding or slowing down the generation of wrinkles in the electrochromic film during the lamination process; and there is no need to specially customize an electrochromic film that matches the curvature of the glass, so the application range is wider and it can be applied to products with more complex or variable curvatures. The present invention improves on the existing printing process, has low production costs, and can be mass-produced; and can be applied to products with complex curvatures, such as skylights and door glass products, and the product applicability is wider. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 It is a schematic diagram of the structure of the electrochromic glass of the present invention.
[0030] Figure 2 It is a schematic diagram of flattening curved glass in the manufacturing method of the present invention.
[0031] Figure 3 The figure is a schematic diagram of the process flow of a method for manufacturing electrochromic glass in a preferred embodiment of the present invention.
[0032] Description of reference numerals:
[0033] 1- first glass substrate;
[0034] 2- first electrode;
[0035] 3-Electrochromic layer;
[0036] 4- second electrode;
[0037] 5-Intermediate layer bonding material;
[0038] 6- second glass substrate;
[0039] 7- Middle suction cup;
[0040] 8-Left suction cup;
[0041] 9-right suction cup;
[0042] X-the distance from the left suction cup to the edge of the glass;
[0043] Y-the distance from the left suction cup to the middle suction cup;
[0044] L - length of the first glass substrate. DETAILED DESCRIPTION
[0045] In order to explain the present invention more clearly, the present invention is further described below in conjunction with preferred embodiments. It should be understood by those skilled in the art that the following specific description is illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.
[0046] In addition, some directional words mentioned in the embodiments of the present invention, such as "left", "right", etc., have meanings related to the placement of the glass substrate and should not be construed as limiting the scope of protection of the present invention.
[0047] The present invention mainly provides a method for manufacturing an electrochromic glass, which comprises: sucking a first curved glass substrate flat with a suction cup, and printing a first electrode, an electrochromic layer, and a second electrode in sequence on a surface of the first glass substrate; and combining the first glass substrate with a second curved glass substrate using an intermediate layer adhesive material, so that the first electrode, the electrochromic layer, and the second electrode are sandwiched between the two glass substrates, to obtain the electrochromic glass.
[0048] The structure of the obtained electrochromic glass is as follows Figure 1 As shown, it includes a first glass substrate 1, a first electrode 2, an electrochromic layer 3, a second electrode 4, an intermediate layer adhesive material 5 and a second glass substrate 6 stacked in sequence, wherein the first electrode 2, the electrochromic layer 3 and the second electrode 4 are all formed by printing in sequence directly on one surface of the first glass substrate 1. The thickness of the first glass substrate 1 and the second glass substrate 6 are independently 1.8 mm to 2.5 mm; the total thickness of the first electrode 2, the electrochromic layer 3 and the second electrode 4 is 10 μm to 30 μm, wherein the thickness of the first electrode 2 and the second electrode 4 are independently 8 μm to 12 μm, and the thickness of the electrochromic layer 3 is 3 μm to 7 μm; the thickness of the intermediate layer adhesive material 5 is 0.2 mm to 1.0 mm.
[0049] The first glass substrate 1 and the second glass substrate 6 are curved glass; the main curvature radius of the obtained electrochromic glass is 1200 mm to 3000 mm.
[0050] like Figure 3 As shown, the printing specifically includes the following processes:
[0051] Using the suction cup to suck the first glass substrate flat, and then printing the first electrode on one surface of the first glass substrate; after printing, restoring the curvature of the first glass substrate, and then drying;
[0052] Repeatedly using the suction cup to suck the first glass substrate flat, printing the electrochromic layer on the first electrode, restoring the curvature of the first glass substrate after printing, and then drying;
[0053] Repeatedly using the suction cup to suck the first glass substrate flat, printing the second electrode on the electrochromic layer, restoring the curvature of the first glass substrate after printing, and then drying;
[0054] Sintering is performed to complete the solidification of the first electrode, the electrochromic layer and the second electrode.
[0055] After sintering is completed, the first glass substrate printed with the first electrode, the electrochromic layer and the second electrode is laminated with the second glass substrate through an intermediate layer of adhesive material.
[0056] Generally, printing is performed on the concave surface of the curved glass. Therefore, it is preferred that the suction cup is adsorbed on the convex surface of the first glass substrate and sucked flat, and then the printing is performed on the concave surface of the first glass substrate. Preferably, the drying temperature is 140-180°C and the time is 2min-3min. Preferably, the sintering temperature is 550-640°C and the time is 4min-6min. Corresponding to the defined drying and sintering conditions, the thickness of the first electrode and the second electrode obtained by printing is preferably independently 8μm-12μm; the thickness of the electrochromic layer is preferably 3μm-7μm; the total thickness of the first electrode, the electrochromic layer and the second electrode is preferably ≤30μm. When the thickness exceeds 30μm, the printed layer may break or the glass may crack. For example, in the process of sucking flat to restore the original curvature, the electrode layer, the electrochromic layer may break or the glass may crack. The sintering process may cause the electrode layer and the electrochromic layer to break.
[0057] As for the specific printing process, screen printing or inkjet printing can be used; the thickness of the printed layer formed by the inkjet printing process can be thinner, but the cost is higher; the present invention more preferably uses screen printing.
[0058] Due to the complex curvature of the curved glass, the use of traditional screen printing technology may cause the problem of uneven printing thickness of the conductive layer, resulting in voltage fluctuations and affecting the electrochromic effect. The present invention preferably uses a suction cup to suck the curved glass flat before each printing, so that the curved glass is flattened before printing to avoid the problem of uneven printing thickness. In the process of sucking the curved glass flat, if the curved glass is unevenly deformed, there may be a risk of cracking. The present invention solves the possible risk of cracking through the specific setting of the suction cup.
[0059] As for the specific leveling method, for glass substrates with a length-to-width ratio of about 1:1 to 1:4, it is preferred to use a plurality of suction cups arranged in a row along the central axis of the first glass substrate that is consistent with the length direction to simultaneously adsorb the convex surface of the first glass substrate. Setting too many suction cups will cause the pressure distribution of the adsorbed glass to be linearly concentrated, the adsorption pressure to be unevenly distributed, and the adsorption pressure to be too large, causing the glass to break during the adsorption process; too few suction cups are not enough to completely level the glass, affecting the subsequent printing effect. According to the current conventional glass size, the number of suction cups set is generally 2 to 4, among which 3 suction cups are set to achieve the best leveling effect. Figure 2As shown, the present invention preferably uses three suction cups arranged in a row along the central axis of the first glass substrate 1 that is consistent with the length direction to simultaneously absorb the convex surface of the first glass substrate 1. In order to achieve a better suction and leveling effect, it is more preferred that the middle suction cup 7 of the three suction cups is located in the middle position, and the two side suction cups on both sides, Figure 2 The left suction cup 8 and the right suction cup 9 are symmetrically arranged; that is, the left suction cup 8 and the right suction cup 9 are at the same distance from the edge of the glass, and the distances between the left suction cup 8 and the right suction cup 9 and the middle suction cup 7 are also the same.
[0060] More preferably, on the central axis, the distance ratio of the side suction cup to the glass edge and to the middle suction cup is 2:1 to 2:4, and most preferably 2:3. That is, assuming that the distance between the left suction cup 8 and the right suction cup 9 and the glass edge of the first glass substrate is X, and the distance from the middle suction cup is Y, 2X+2Y is the length L of the first glass (the measurement of X and Y is based on the center of the suction cup), X:Y=2:3; at this time, the curved glass will obtain uniform deformation and will not cause the glass to crack, and at the same time achieve the best flattening effect. For example: when the length L of the first glass is 1000mm, X is 200mm, and Y is 300mm, the flattening effect is the best; more importantly, under this flattening effect, there will be no risk of cracking during the printing process.
[0061] The printing adopts screen printing technology. The first electrode and the second electrode are printed with silver paste; the composition of the silver paste preferably includes 50wt.% to 85wt.% of silver powder, 1wt.% to 3wt.% of glass powder and 12wt.% to 48wt.% of oil agent, and the electrodes printed with the silver paste composed of this composition have better conductive stability.
[0062] The electrochromic layer contains an electrochromic material capable of electrochromic change, and the electrochromic material is an organic material or an inorganic material. As an inorganic material, a metal oxide can be used. ① Reductive electrochromic material: for example, formed by vanadium oxide, niobium oxide, indium oxide, iridium oxide, nickel oxide, cobalt oxide, molybdenum oxide or a mixture of several thereof. ② Oxidative electrochromic material: for example, oxides of Cr, Mn, Fe, Co, Ni, Rh or Ir; hydroxides of Cr, Mn, Fe, Co, Ni, Rh or Ir; and Prussian blue. LiNiOx, IrO2, NiO, V2O5, LixCoO2, Rh2O3 or CrO3 can also be used. After the electrode is applied with voltage, the substances in the electrochromic layer undergo a chemical reaction, so that the glass presents a specific color; the magnitude of the voltage affects the depth of the color of the electrochromic layer, and the depth of the color is adjusted by controlling the magnitude of the voltage (for example, gradually increasing the voltage at a voltage interval of 1V to 5V). After power is cut off, the electrochromic layer begins a reversible reaction and the color of the glass returns to its initial state.
[0063] The printing parameters of the screen printing process preferably include: a printing speed of (400±50) mm / s, a printing pressure of 0.2MPa-0.5MPa, and a viscosity of the printing material of 25Pa.s-50Pa.s. This parameter setting can effectively deposit the silver paste and the printing material of the electrochromic layer on the glass surface, and can well control the printing thickness of each layer within the specified range. The present invention limits the specific setting of the suction cup to ensure that the curved glass that is sucked flat during the printing process under the printing parameters will not have the risk of cracking.
[0064] The intermediate layer adhesive material is PVB or EVA, etc. The lamination process is a mature process in the prior art, and the present invention will not be described in detail here.
[0065] The following provides a set of examples to verify the preparation method of the present invention by conducting a power-on test to verify the electrochromic function of the obtained electrochromic glass. The parameters and test results are shown in Table 1 below. The manufacturing method includes the following steps:
[0066] 1) Use Figure 2 The three suction cups shown are attached to the convex surface of the first glass substrate and flatten it; wherein X:Y=2:3; the concave surface of the first glass substrate after being flattened is printed with a first electrode by screen printing process, with a thickness of 11 μm;
[0067] 2) After the first electrode is printed, the curvature of the first glass substrate is restored, and then it is dried; the drying temperature is 180° C. and the time is 2 minutes;
[0068] 3) sucking the first glass substrate flat again in the manner of step 1), and printing an electrochromic layer on the first electrode with a thickness of 6 μm;
[0069] 4) After the electrochromic layer is printed, the curvature of the first glass substrate is restored, and then the substrate is dried; the drying temperature is 180° C. and the time is 2 minutes;
[0070] 5) Flatten the first glass substrate again in the same manner as in step 1), and print a second electrode on the electrochromic layer with a thickness of 11 μm;
[0071] 6) After the second electrode is printed, the curvature of the first glass substrate is restored, and then it is dried; the drying temperature is 180° C. and the time is 2 minutes;
[0072] 7) Sintering to complete the solidification of the first electrode, the electrochromic layer and the second electrode; the sintering temperature is 620° C. and the time is 5 minutes;
[0073] 8) Using an intermediate layer adhesive material to bond the substrate to the second glass substrate.
[0074] The printing speed of the above screen printing process is 400 mm / s, the printing pressure is 0.4 MPa, and the silver paste viscosity is 30 Pa.s.
[0075] Table 1
[0076]
[0077] The distance parameters X:Y of the suction cups in the preparation process were changed and adjusted for Examples 1-6 in Table 1 to verify the printing conditions in the preparation process. The results are shown in Table 2.
[0078] Table 2
[0079]
[0080] The printing thickness of Examples 1-6 in Table 1 was changed during the preparation process to verify the printing conditions. The results are shown in Table 3.
[0081] Table 3
[0082]
[0083] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not limitations on the implementation methods of the present invention. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is impossible to list all the implementation methods here. All obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.
Claims
1. A method for manufacturing electrochromic glass for a vehicle, characterized in that: The manufacturing method comprises the following steps: The curved first glass substrate is sucked flat with a suction cup, and a first electrode, an electrochromic layer, and a second electrode are sequentially printed on one surface of the first glass substrate; the first glass substrate is laminated with a curved second glass substrate using an intermediate layer adhesive material, so that the first electrode, the electrochromic layer, and the second electrode are sandwiched between the two glass substrates, to obtain the electrochromic glass; Among them, sucking the curved first glass substrate flat using a suction cup includes: using three suction cups to line up along the central axis of the first glass substrate that is consistent with the length direction and simultaneously sucking the convex surface of the first glass substrate; the middle suction cup among the three suction cups is located in the middle position, and the two side suction cups on both sides are symmetrically arranged, wherein the ratio of the distance from the side suction cup to the glass edge to the distance from the side suction cup to the middle suction cup is 2:1~2:
4.
2. The manufacturing method according to claim 1, characterized in that The main curvature radius of the electrochromic glass is 1200 mm to 3000 mm.
3. The manufacturing method according to claim 1, characterized in that: The printing is specifically The process includes: Using the suction cup to suck the first glass substrate flat, and then printing the first electrode on one surface of the first glass substrate; After printing is completed, the curvature of the first glass substrate is restored, and then drying is performed; Repeatedly using the suction cup to suck the first glass substrate flat, printing the electrochromic layer on the first electrode, restoring the curvature of the first glass substrate after printing, and then drying; Repeatedly using the suction cup to suck the first glass substrate flat, printing the second electrode on the electrochromic layer, restoring the curvature of the first glass substrate after printing, and then drying; Sintering is performed to complete the solidification of the first electrode, the electrochromic layer and the second electrode.
4. The manufacturing method according to claim 3, characterized in that The drying temperature is 140-180°C and the drying time is 2 min-3 min.
5. The manufacturing method according to claim 3, characterized in that: The sintering temperature is 550-640° C. and the sintering time is 4 min to 6 min.
6. The manufacturing method according to claim 3, characterized in that: The thickness of the first electrode and the second electrode are independently 8 μm to 12 μm, the thickness of the electrochromic layer is 3 μm to 7 μm; and the total thickness of the first electrode, the electrochromic layer and the second electrode is ≤30 μm.
7. The manufacturing method according to claim 1, characterized in that: The printing adopts screen printing technology or inkjet printing technology.
8. The manufacturing method according to claim 1, characterized in that The printing adopts the screen printing process, and the printing parameters include: a printing speed of 400±50 mm / s, a printing pressure of 0.2 MPa ~ 0.5 MPa, and a viscosity of the printing material of 25 Pa.s ~ 50 Pa.s.
9. The manufacturing method according to claim 1, characterized in that: The thickness of the first glass substrate and the second glass substrate are independently 1.8 mm to 2.5 mm; the thickness of the intermediate layer adhesive material is 0.2 mm to 1.0 mm.
10. An electrochromic glass for a vehicle obtained by the manufacturing method according to any one of claims 1 to 9.