A method for in-situ preparation of quantum dot-doped polymer thin film materials by spin coating process
The quantum doped polymer film is prepared in situ by spin coating, which solves the problems of easy agglomeration and cumbersome preparation process, and achieves uniform dispersion and high stability of quantum dots in polymer matrix, meeting different needs. Film preparation.
Patent Information
- Application Number
- CN202310266647.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-20
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-03-20
AI Technical Summary
The traditional method of preparing quantum dot-polymer films has problems such as the agglomeration of quantum dots and the process is complicated, resulting in unstable luminous properties of the film and the simple method to meet different needs.
The spin coating process is used to prepare quantum doped polymer thin film materials in situ. The quantum dots are formed in the polymer matrix through heat treatment, and the volatile solvents and polymers are used for coordination to inhibit the agglomeration of quantum dots and control the rotation. Coating conditions and heat treatment time regulate the size and morphology of quantum dots.
The uniform dispersion of quantum dots in polymer matrix is achieved, the fluorescence performance and stability of the film is improved, the performance can be maintained in different temperatures and chemical environments, the preparation process is simplified, and the cost is reduced.
Smart Images

Figure CN116351684B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for in-situ preparation of quantum dot-doped polymer film materials based on a spin coating process, which is a simple method for efficiently preparing quantum polymer films of different areas to meet the needs of different occasions. Background Art
[0002] Quantum dot-polymer films are widely used in quantum dot displays, solar integrators, and LED light conversion. The traditional method for preparing quantum dot-polymer films is physical blending, which mainly includes two steps. First, quantum dots are prepared in a solution state, and the quantum dots are purified and dispersed in a polar organic solvent; then the quantum dots are directly or after ligand exchange and blended with the polymer, and the obtained blended solution is prepared into a quantum dot-polymer film by spin coating or scraping. Quantum dots still have stable luminescence performance and absorbance after direct blending with polymers, and the luminescence intensity increases with the increase of quantum dot content, but the color of the luminescence will also change with the change of quantum dot content, which is caused by the agglomeration of quantum dots. This method of preparing quantum dot-polymer films is not only cumbersome, but the luminescence performance of the film is also prone to decay with the extension of use time.
[0003] Therefore, the prior art has defects and needs to be improved. Summary of the invention
[0004] In order to overcome the shortcomings of easy agglomeration of quantum dots and cumbersome preparation process in the process of traditional polymer encapsulation of quantum dots, the present invention proposes a method for in-situ preparation of quantum dot-doped polymer film materials based on spin coating process. After spin coating, quantum dots can be formed in the polymer film matrix by heat treatment of the film. The prepared quantum dots are composed of II-VI and III-V group elements, and the polar groups in the polymer can be used as the generation site of quantum dots. The quantum dots can be generated in the polymer by relying on its polar groups without using ligands or surfactants.
[0005] One of the purposes of the present invention is to disperse the quantum dot precursor and the polymer into a specific solvent so that the three can be blended at the molecular scale. In the present invention, a specific volatile solvent is used at a certain temperature to coordinate the quantum dot precursor with the polymer so that the precursor can be evenly dispersed in the polymer matrix, which effectively inhibits the aggregation of quantum dots after they are generated.
[0006] In the present invention, a quantum dot precursor-polymer dispersion is spin-coated onto a substrate to form a thin film, and a simple method for forming a thin film after the solvent evaporates completely is used. The quartz glass sheet carrying the thin film is placed in an air atmosphere for heat treatment to obtain a quantum dot-polymer composite material. Through the cross-sectional scanning electron microscope image of the quantum dot-polymer film, we can see that the quantum dots are uniformly dispersed in the polymer matrix, and the atomic force microscope image shows that there are circular protrusions on the surface of the film, which are quantum dots wrapped by the polymer. The fluorescence image also confirms that the quantum dot-polymer film was successfully prepared by this method. The film not only exhibits excellent fluorescence properties, but also shows stability in saturated steam at different temperatures and in harsh chemical environments.
[0007] The technical solution of the present invention is as follows:
[0008] A method for in-situ preparation of quantum dot-doped polymer thin film materials by spin coating process, wherein the precursor components required for preparing quantum dots are dissolved and dispersed in the corresponding polymer solution, and the composition, size and appearance of the prepared quantum dot-doped polymer are regulated by controlling the concentration and proportion of the precursor in the polymer solution; the steps include:
[0009] Step 1: dissolving a cadmium precursor in a volatile solvent at 90° C., stirring for a period of time to form a transparent solution, adding a polymer to the transparent solution, and stirring evenly at the temperature; adding a selenium precursor after the solution returns to room temperature, and stirring to obtain a transparent solution;
[0010] Step 2: Take a certain amount of the transparent solution in step 1 and drop it on the substrate for spin coating. After the solvent evaporates completely, a quantum dot precursor-polymer pre-coating film can be obtained;
[0011] Step 3: heat-treat the quantum dot precursor-polymer pre-coating film at a temperature higher than the glass transition temperature of the polymer. The heat treatment process is the process of forming quantum dots from the quantum dot precursor in the polymer matrix. The size and morphology of the quantum dots can be controlled by changing the heat treatment time. After the heat treatment, cool it to room temperature to obtain a quantum dot-doped polymer film material.
[0012] In the method, the quantum dots described in step 1 include all II-VI and III-V group semiconductor quantum dots, such as cadmium selenide quantum dots (CdSe), cadmium telluride quantum dots (CdTe), cadmium sulfide quantum dots (CdS), lead sulfide quantum dots (PbS), lead selenide quantum dots (PbSe), lead telluride quantum dots (PbTe), zinc selenide quantum dots (ZnSe), zinc telluride quantum dots (ZnTe), zinc sulfide quantum dots (ZnS), indium sulfide quantum dots (InS), indium phosphide (InP), indium arsenide (InAs), and copper indium sulfide (CuInS).
[0013] In the method, in step 1, the metal component precursor in the quantum dot precursor is a metal salt, metal oxide, or organic metal compound, including but not limited to cadmium, zinc, and lead salts of myristic acid, stearic acid, and oleic acid.
[0014] In the method, in step 1, the precursor of the non-metal component in the quantum dot precursor is a salt, alkali, oxide, organic matter of the non-metal involved, including but not limited to tri-n-octylphosphine selenide and sodium hydride selenide.
[0015] In the method, in step 1, the polymer is polyvinyl chloride (PVC).
[0016] In the method, in step 1, the organic solvent is tetrahydrofuran.
[0017] The method, in step 1, the concentration of the quantum dot constituent elements contained in the blended precursor is 0.003-0.17 mol / L.
[0018] In the method, in step 1, the mass concentration of the polymer is 0.05 g / ml-0.5 g / ml.
[0019] The method, in step 1, the blending of the precursor and the polymer is carried out at 60-120° C.,
[0020] In the method described, in step 2, the substrate includes a quartz glass sheet, a silicon sheet and all plastic material models.
[0021] In the method, in step 2, the amount of the mixed solution for spin coating is 30 μL-300 μL.
[0022] In the method, in step 2, the spin coating speed is 500rpm-5000rpm.
[0023] In the method, in step 2, the spin coating time is 10s-120s.
[0024] In the method, in step 3, the heat treatment temperature above the glass transition temperature of the polymer is in the range of 120-200°C.
[0025] In the method, in step 4, the heat treatment time ranges from 10 to 600 seconds.
[0026] A quantum dot-polymer film was successfully prepared by mixing a quantum dot precursor with a polymer in a volatile solvent under heating conditions, spin-coating the mixed solution on a substrate, and then heat-treating the solution to synthesize the quantum dots in situ in the polymer matrix.
[0027] The film can be subjected to solid-state heat treatment to obtain a quantum dot-doped polymer film material. The special role of the spin coating process in this method includes the following two aspects: (1) During the spin coating process, the polymer chain is in a coil-like stretched conformation in a good solvent at the initial stage. As the solvent evaporates, the polymer concentration increases, and the coils overlap. Finally, in the film after spin coating, the polymer chains penetrate and entangle with each other to form a nano-network. In this process, the quantum dot precursor can be evenly dispersed in the polymer nano-network formed by the spin coating process, providing a confinement area for the in-situ generation of quantum dots. (2) The thickness of the film can be precisely controlled by controlling the concentration of the solution before spin coating, the spin coating speed and the spin coating time. The precise and appropriate film thickness can not only ensure that the film will not be deformed during the subsequent heat treatment, but also facilitate the optimization of the heat treatment conditions for the in-situ preparation of quantum dots. It plays a decisive role in the generation of quantum dots.
[0028] This method is simple and easy to use, and can prepare thin films of different sizes according to needs. The thickness of the film can be controlled by controlling the concentration of polymers and precursors and the speed of spin coating. Since quantum dots are synthesized in situ, the confidential chemical bonds between quantum dots and polymers can keep the luminescence stability in harsh environments. These characteristics can meet the commercial needs in the field of luminescence while greatly saving costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is a transmission electron microscope image of the quantum dot-polymer film slice prepared in Example 1.
[0030] Figure 2 This is a transmission electron microscope image of the quantum dot-polymer film slice prepared in Example 2.
[0031] Figure 3 This is a transmission electron microscope image of the quantum dot-polymer film slice prepared in Example 3.
[0032] Figure 4 This is a scanning electron microscope image of the cross section of the quantum dot-polymer film prepared in Example 1.
[0033] Figure 5 This is an atomic force microscope photograph of the surface of the quantum dot-polymer film prepared in Example 1.
[0034] Figure 6 This is a fluorescence comparison diagram of the precursor-polymer film before heat treatment and the quantum dot-polymer film obtained after heat treatment in Example 1.
[0035] Figure 7 The fluorescence comparison of the films prepared in Example 1, Comparative Example 1 and Comparative Example 2 before and after 30 days under saturated steam at different temperatures.
[0036] Figure 8 The chemical stabilities of the films prepared in Example 1, Comparative Example 1 and Comparative Example 2 in different chemical environments before and after 24 hours.
[0037] Fig. 9 The photographs of the films prepared in Example 1, Comparative Example 1 and Comparative Example 2 under UV light before and after being in 0.5H2SO4 solution, 1MNaOH solution and 98% alcohol for 7 days are compared. DETAILED DESCRIPTION
[0038] The present invention is described in detail below in conjunction with specific embodiments.
[0039] Example 1 Preparation of polymer luminescent film containing 3.5 nm CdSe quantum dots
[0040] Take 0.45g of cadmium myristic acid and stir it in tetrahydrofuran at 90℃ for 30min to form a transparent solution. Take 0.4g of polyvinyl chloride and dissolve it in the above transparent solution at 90℃. Stir for 30min to form a uniform solution. After the solution is cooled to room temperature, take 80μL of 1mol / L tri-n-octylphosphine selenium and add it to the above mixed solution. Stir for 20min at room temperature to obtain a quantum dot precursor-polymer solution. Heat the above solution at 90℃ for 5min to make it a transparent solution. Take 450 microliters of the above transparent solution on a quartz glass sheet and spin coat it at 3000rpm for 30s to form a transparent quantum dot precursor-polymer film on the glass sheet. The film was heat treated at 160°C in air atmosphere to obtain a CdSe quantum dot-polymer composite film. The film thickness prepared under this rotation speed condition was moderate. The polymer chain activity and precursor migration rate at this film thickness under 160°C conditions controlled the particle size of the quantum dots to be about 3.5nm ( Figure 1 ); Figure 4 The cross section of the film prepared under this condition is shown. It can be seen from the figure that the cross section width is about 3 microns. Figure 5 Shown in the figure is an atomic force microscope photograph of the film, which shows round protrusions on the surface of the film, proving that the CdSe quantum dots are formed inside the polymer matrix rather than on the surface.
[0041] Example 2: Preparation of polymer luminescent film containing 1.7 nm CdSe quantum dots
[0042] Take 0.45g of cadmium myristic acid and stir it in tetrahydrofuran at 90℃ for 30min to form a transparent solution. Take 0.4g of polyvinyl chloride and dissolve it in the above transparent solution at 90℃. Stir for 30min to form a uniform solution. After the solution is cooled to room temperature, take 80μL of 1mol / L tri-n-octylphosphine selenium and add it to the above mixed solution. Stir for 20min at room temperature to obtain a quantum dot precursor-polymer solution. Heat the above solution at 90℃ for 5min to make it a transparent solution. Take 450 microliters of the above transparent solution on a quartz glass sheet and spin coat it at 1000rpm for 30s to form a transparent quantum dot precursor-polymer film on the glass sheet. The film was heat treated at 160°C in air atmosphere. When treated at 160°C, the film thickness obtained at this spin coating speed was thicker, the thermal conductivity was slower, the activity of the polymer chain and the migration rate of the precursor were slower, so the particle size of the obtained CdSe was smaller, about 1.7nm ( Figure 2 ).
[0043] Example 3: Preparation of polymer luminescent film containing 8nm CdSe quantum dots
[0044] Take 0.45g of cadmium myristic acid and stir it in tetrahydrofuran at 90℃ for 30min to form a transparent solution. Take 0.4g of polyvinyl chloride and dissolve it in the above transparent solution at 90℃. Stir for 30min to form a uniform solution. After the solution is cooled to room temperature, take 80μL of 1mol / L tri-n-octylphosphine selenium and add it to the above mixed solution. Stir at room temperature for 20min to obtain a quantum dot precursor-polymer solution. Heat the above solution at 90℃ for 5min to make it a transparent solution. Take 450 microliters of the above transparent solution on a quartz glass sheet and spin coat it at 5000rpm for 30s to form a transparent quantum dot precursor-polymer film on the glass sheet. The film is heat-treated at 160℃ in an air atmosphere. Since the polymer film obtained under this speed condition is thinner, the polymer molecular chain is active under this temperature condition and the precursor migration rate is faster, the resulting quantum dot particle size is larger, about 8nm ( Figure 3 )
[0045] Comparative Example 1: Preparation of Pure Quantum Dots
[0046] 2.4mmol of cadmium oxide was dissolved in a mixed solution of 2.5mL of octadecene and 2.5mL of oleic acid and placed in a three-necked flask. The reaction mixture was heated to 100℃ under vacuum for 20min, and then heated to 250℃ for 5min in a nitrogen atmosphere to obtain cadmium oleate as a precursor. 1.2mmol of selenium powder was dissolved in 1ml of tri-n-octylphosphine to form tri-n-octylphosphine selenium, which was ultrasonically treated under an inert atmosphere at room temperature. Then, 0.4mL of tri-n-octylphosphine selenium, 0.6mL of tri-n-octylphosphine and 9mL of oleyl ammonia were placed in a three-necked flask, vacuum degassed at 100℃ and stirred for 20 minutes. When the temperature reached 275℃, 1mL of cadmium oleate solution was quickly injected into the reaction mixture under a nitrogen atmosphere, stirred for 4min, and then cooled to room temperature. The obtained CdSe quantum dots were precipitated with methanol, centrifuged at 8000 rpm for 5 min, and redispersed in tetrahydrofuran solution. 300 μL of the solution was spin-coated on a quartz glass sheet at a speed of 100 rpm. After the sample was completely dried, a pure quantum dot film loaded on the quartz glass sheet was obtained.
[0047] Comparative Example 2: Preparation of quantum dot-polymer composite film by physical blending method
[0048] 0.4 g of polyvinyl chloride powder was added to 2 ml of the tetrahydrofuran dispersion of quantum dots prepared in the comparative example, and stirred on a stirrer until dissolved. 300 μL of the dispersion was spin-coated on a quartz glass sheet at a speed of 2000 rpm. After the solvent in the sample was completely evaporated, a quantum dot-polymer film prepared by physical blending was obtained.
[0049] It should be understood that those skilled in the art can make improvements or changes based on the above description, and all these improvements and changes should fall within the scope of protection of the appended claims of the present invention.
Claims
1. A method for in-situ preparation of quantum dot-doped polymer thin film materials by spin coating process, characterized in that: Dissolving and dispersing the precursor components required for preparing quantum dots in the corresponding polymer solution, and regulating the composition, size and appearance of the prepared quantum dot-doped polymer by controlling the concentration and proportion of the precursor in the polymer solution; The steps include: Step 1: dissolving a cadmium precursor in tetrahydrofuran at 90° C., stirring for a period of time to form a transparent solution, adding polyvinyl chloride to the transparent solution, and stirring evenly at the temperature; adding a selenium precursor after the solution returns to room temperature, and stirring to obtain a transparent solution; Step 2: Take a certain amount of the transparent solution in step 1 and drop it on the substrate for spin coating. After the solvent evaporates completely, a quantum dot precursor-polymer pre-coating film can be obtained; Step 3: heat-treating the quantum dot precursor-polymer pre-coating film at a temperature higher than the glass transition temperature of the polymer. The heat treatment process is the process of forming quantum dots from the quantum dot precursor in the polymer matrix. The size and morphology of the quantum dots are regulated by changing the heat treatment time. After the heat treatment, the film is cooled to room temperature to obtain a quantum dot-doped polymer film material. The heat treatment time range is 10-600s.
2. The method according to claim 1, characterized in that In step 1, the metal component precursor in the quantum dot precursor is a cadmium salt of myristic acid, stearic acid, or oleic acid.
3. The method according to claim 1, characterized in that: In step 1, the precursor of the non-metal component in the quantum dot precursor is tri-n-octylphosphine selenide or sodium hydride selenide.
4. The method according to claim 1, characterized in that: In step 1, the concentration of the quantum dot constituent elements contained in the quantum dot precursor is 0.003-0.17 mol / L.
5. The method according to claim 1, characterized in that In step 1, the mass concentration of the polymer is 0.05 g / ml-0.5 g / ml.
6. The method according to claim 1, characterized in that In step 2, the substrate includes a quartz glass sheet and a silicon sheet.