Aliphatic thermoplastic polyester elastomer and preparation method thereof
The non-degradable and non-block polymers with "hard"-"soft"-"hard"-"hard"-"hard"-"hard""and"hard")"On-degradable" and "hard"")")"L-polylactic acid and propylene oxide and succinic anhydride" are solved by the preparation of triblock or multi-block polymers with "hard" and "hard" structures")" and "hard"")")")"On-degradable")"On-degradable")""""""""""""""""""""""""""""""""""""""""""""""""""""""""""""""""""""""""""""""""""""""""""""""""""""""""" The problem of waste pollution has achieved biocompatibility and efficient preparation, and expanded the scope of application.
Patent Information
- Application Number
- CN202310050459.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-01
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-02-01
AI Technical Summary
Traditional thermoplastic polyester elastomers are non-degradable, waste pollutes the environment, and the international market is monopolized by foreign companies, which limits its development.
The L-polylactic acid with high melting point is used as the hard segment, and the propylene oxide and succinic anhydride copolyester with adjustable glass transition temperature is used as the soft segment, and the chain transfer method is prepared with "hard"-" softness through chain transfer method or chain extension method. The triblock or multiblock polymer with "-"hard" structure regulates the ratio of soft and hard segments to achieve an efficient and low-energy-consuming preparation process.
The biocompatibility and biodegradability of aliphatic thermoplastic polyester elastomers are achieved, the application scope is expanded, and the preparation route is efficient, low energy consumption, and waste discharge is free, which is suitable for industrial production.
Smart Images

Figure CN116355188B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of polymer materials, and in particular relates to an aliphatic thermoplastic polyester elastomer and a preparation method thereof. Background Art
[0002] Thermoplastic polyester elastomer is commonly known as polyester rubber or polyester thermoplastic elastomer. It is a block polymer containing two different soft and hard segments. It has both the excellent mechanical properties of vulcanized rubber and the good processing properties of thermoplastic plastics. Therefore, it only needs a simple molding process and does not require a vulcanization process. Compared with traditional vulcanized rubber, its production process takes less time and greatly improves production efficiency. The soft segment in the material ensures the low-temperature softness of the material, while the presence of the hard segment can play a role in physical cross-linking, providing a certain strength to the material while plasticizing and molding. In addition, since the waste of thermoplastic polyester elastomer can be recycled and reused for a second time, it also solves the problem that rubber products cannot be recycled to a certain extent. Therefore, thermoplastic polyester elastomer has become a standardized, global, and environmentally friendly material, which meets the requirements of green and environmental protection development.
[0003] Traditional thermoplastic polyester elastomers are block copolymers composed of aromatic polyester hard segments (such as PBT) and aliphatic polyesters (such as PCL) or polyether soft segments (such as PEG, PPG and PTMG). Traditional thermoplastic polyester elastomers have problems such as non-degradability and waste pollution. In the context of large-scale use around the world, increasing resource waste and epoxy environmental pollution also restrict their development. At the same time, the international and domestic high-end markets of thermoplastic polyester elastomers are basically monopolized by foreign companies. Based on this, the present invention provides an aliphatic thermoplastic polyester elastomer and a preparation method thereof. Specifically, L-polylactic acid with a high melting point is used as a hard segment, and propylene oxide and succinic anhydride copolyester with adjustable glass transition temperature is used as a soft segment. The hard segment and the soft segment are prepared by a chain transfer method or a chain extension method to form a triblock or multiblock polymer with a "hard"-"soft"-"hard" structure. This route is efficient, low energy consumption and no waste, and is an atom-economical route. At the same time, aliphatic thermoplastic polyester elastomers have good biocompatibility and biodegradability, and the small molecular compounds released can be reused without polluting the environment, which greatly expands the application scope of such thermoplastic elastomers. Summary of the invention
[0004] The main content of the present invention is to provide an aliphatic thermoplastic polyester elastomer and a preparation method thereof according to the deficiencies of the prior art.
[0005] Technical solution of the present invention
[0006] An aliphatic thermoplastic polyester elastomer, which uses L-polylactic acid with a high melting point as a hard segment and propylene oxide and succinic anhydride copolyester with adjustable glass transition temperature as a soft segment, and the hard segment and the soft segment are prepared by chain transfer method or chain extension method to form a triblock or multiblock polymer with a "hard"-"soft"-"hard" structure. At the same time, the ratio of the soft and hard segments in the triblock or multiblock polymer is adjustable. The "hard"-"soft"-"hard" structure is as follows:
[0007]
[0008] Where:
[0009] x is a natural number from 1 to 10;
[0010] m is a non-zero natural number;
[0011] n is a non-zero natural number.
[0012] The preparation method of the aliphatic thermoplastic polyester elastomer is as follows: propylene oxide, succinic anhydride, a first catalyst, a chain initiator and an organic solvent are added to a reactor to carry out a first polymerization reaction to obtain a soft segment polymer. L-lactide monomer and a second catalyst are added in situ, and a second polymerization reaction is carried out by a chain transfer method to obtain a "hard"-"soft"-"hard" triblock polymer. A chain extender is selectively added to the original solution, and a third polymerization reaction is carried out by a chain extension method to obtain a multi-block polymer.
[0013] In the first polymerization reaction, the first catalyst has the general structural formula M 1 a L 1 b [M 2 (CN) c L 2 d ] e [H 2 O] f .
[0014] Where:
[0015] M 1 Selected from Zn 2+ 、Co 2+ 、Ni 2+ , Fe 2+ , Fe 3+ , Ca 2+ Mg 2+ , Cu 2+ Sn 2+ , Cd2+ or Pb 2+ ;M 2 Selected from Al 3+ 、Co 3+ , Fe3+ Cr 3+ or Mn 3+ ; a, c and e are non-zero natural numbers, b, d and f are natural numbers; L 1 With L 2 The structures may be the same or different, and are specifically one of the following structures:
[0016]
[0017] The chain initiator is one of small molecule alcohols (such as ethylene glycol, glycerol, pentaerythritol, etc.) or macromolecular alcohols (polyethylene glycol 400, polypropylene glycol 600, etc.).
[0018] The mass ratio of the first catalyst to propylene oxide is 1:5000-10000.
[0019] The molar ratio of propylene oxide to succinic anhydride is 1-11:1.
[0020] The molar ratio of propylene oxide to chain initiator is 200-2000:1.
[0021] The organic solvent is any one of toluene, xylene, tetrahydrofuran, dichloromethane, dichloroethane, n-hexane and 1,4-dioxane.
[0022] In the second polymerization reaction, the second catalyst is one of the following catalysts:
[0023]
[0024] Where:
[0025] R is
[0026]
[0027] R 1 H, OH, C 1 ~C 4 Alkyl, C 1 ~C 4 Alkoxy, F, Cl, Br or NO 2 Group;
[0028] R 2 H, C 1 ~C 4 Alkyl, C 1 ~C 4 Alkoxy, F, Cl, Br or NO 2 Group;
[0029] R 3 C 1 ~C4 alkyl;
[0030] R 4 C 1 ~C 4 alkyl;
[0031] R 5 C 1 ~C 4 alkyl;
[0032] X is Cl, NO 3 CF 3 COO、CH 3 COO, BF 4 , CH 3 O、CH 3 CH 2 , or CH 3 CH 2 CH 2 CH 2 Group;
[0033] g = 0, 1, 2, 4, 6 or 8;
[0034] h is a non-zero natural number;
[0035] i is a non-zero natural number;
[0036] y is a non-zero natural number.
[0037] The molar ratio of metal magnesium to L-lactide in the second catalyst is 1:500-20000.
[0038] In the third polymerization reaction, the chain extender is one of toluene-2,4-diisocyanate (TDI), hexamethylene diisocyanate (HDI), 4,4'-methylene diisocyanate (MDI), terephthaloyl chloride (TPC) and adipoyl chloride (HDC).
[0039] The molar ratio of the chain extender to the triblock polymer is 1-1.2:1.
[0040] The first polymerization reaction temperature is 50-120°C.
[0041] The first polymerization reaction time is 2 to 4 hours.
[0042] The second polymerization reaction temperature is 25-120°C.
[0043] The second polymerization reaction time is 1 to 5 hours.
[0044] The third polymerization reaction temperature is 60-120°C.
[0045] The third polymerization reaction time is 0.5 to 2 hours.
[0046] The glass transition temperature of the soft segment polymer in the aliphatic thermoplastic polyester elastic can be adjusted within the range of -8 to -48°C.
[0047] The ratio of the soft segment to the hard segment in the aliphatic thermoplastic polyester elastomer is adjustable, and the content of the hard segment is 20-80wt%.
[0048] The number average molecular weight of the aliphatic thermoplastic polyester elastomer is 30.0-200.0 kg / mol.
[0049] The aliphatic thermoplastic polyester elastomer has a use window temperature of -48 to 170°C, a maximum tensile strength of 10 to 40 MPa, and a breaking elongation of 300 to 1500%.
[0050] Beneficial effects of the present invention:
[0051] (1) The soft segment of the aliphatic thermoplastic polyester elastomer described in the present invention is made of propylene oxide and succinic anhydride as raw materials. By adjusting the ratio of the two, the soft segment structure and glass transition temperature can be adjusted within the range of -8 to -48°C.
[0052] (2) The ratio of soft segment to hard segment in the aliphatic thermoplastic polyester elastomer of the present invention is adjustable, and the content of hard segment is 20-80 wt %, thereby achieving the regulation of thermal and mechanical properties of the aliphatic thermoplastic polyester elastomer.
[0053] (3) The aliphatic thermoplastic polyester elastomer described in the present invention has good biocompatibility and biodegradability, and the released small molecule compounds can be reused without causing pollution to the environment.
[0054] (4) The preparation route of the aliphatic thermoplastic polyester elastomer described in the present invention is efficient, low in energy consumption and waste-free, and is an atom-economical route. At the same time, the catalysts and raw materials used are cheap and readily available, and are suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0055] Figure 1 This is the hydrogen nuclear magnetic resonance spectrum of the elastomer prepared in Example 6;
[0056] Figure 2 This is the hydrogen nuclear magnetic resonance spectrum of the elastomer prepared in Example 10. DETAILED DESCRIPTION
[0057] The technical solution of the present invention is further described below through examples.
[0058] The terms used in the present invention, unless otherwise specified, generally have the meanings commonly understood by those of ordinary skill in the art.
[0059] In the following examples, various processes and methods not described in detail are conventional methods known in the art. At the same time, due to the large number of catalyst types and the diverse polymer structure ratios, not all preparation methods are described in detail, and typical examples are taken to illustrate the specific process steps of the present invention.
[0060] L a CAS:939-23-1;L b CAS:55-22-1;L c CAS:553-26-4;L d CAS:366-18-7;
[0061] L e CAS:937242-26-7;L f CAS:2185841-71-6;L g CAS:1148-79-4;
[0062] Raw material A1-1 CAS: 120-83-2;
[0063] Raw material A1-2 CAS: 1249587-34-5;
[0064] Raw material B1-1 CAS: 20383-23-7;
[0065] Raw material C1-1 CAS: 4543-96-8;
[0066] Example 1-2 is an example of the first catalyst preparation method.
[0067] Examples 3-5 are examples of the preparation methods of the mononuclear magnesium metal A1, binuclear magnesium metal B1 and polymer magnesium metal C1 in the second catalyst.
[0068] Examples 6-10 are examples of preparing aliphatic thermoplastic polyester elastomers using the catalyst of the present invention. The first catalyst and the second catalyst used in the examples are numbered as shown in the following formula.
[0069] First catalyst:
[0070] ZlUT b 2 [Fe(CN) 4 L d ] 2
[0071] Zn 2 L c 2 [Al(CN) 4 L e ]4
[0072] Second catalyst:
[0073]
[0074] Example 1
[0075] Under nitrogen protection, weigh FeCl with a molar ratio of 1:4:1 in the reaction flask at room temperature. 3 (1.62 g, 10.00 mmol), KCN (2.60 g, 40.00 mmol) and L d (1.56 g, 10.00 mmol) was stirred vigorously with deionized water (10.00 g), mixed evenly, heated to 60 °C, stirred for 2 h, and an emulsion was obtained. The temperature was raised to 80 °C and mixed with FeCl 3 Molar ratio of ZnCl:1:2:2 2 (0.68 g, 5.00 mmol) and L b (1.23 g, 10.00 mmol) was mixed with deionized water (10.00 g) and added to the reaction bottle at a uniform speed within 2 h. After the addition was completed, the reaction was kept warm for 2 h. The emulsion was cooled and centrifuged to obtain a solid. The solid was washed three times with deionized water at 50 ° C and dried to obtain the product ZnL b 2 [Fe(CN) 4 L d ] 2 , yield 87%. Elemental analysis (C 40 H 26 N 14 ZnFe 2 O 4 , mass percentage), theoretical value: C 50.90, H 2.76, N 20.78, O 6.79; measured value: C 50.15, H 2.98, N 20.43, O 6.86.
[0076] Example 2
[0077] Under nitrogen protection, weigh AlCl with a molar ratio of 1:4:1 in the reaction flask at room temperature. 3 (1.33 g, 10.00 mmol), KCN (2.60 g, 40.00 mmol) and L e (2.12 g, 10.00 mmol) was stirred vigorously with deionized water (20.00 g), mixed evenly, heated to 80 °C, stirred for 3 h, and an emulsion was obtained. The temperature was raised to 100 °C and mixed with AlCl 3 Molar ratio of ZnCl:1:1:2 2 (0.68 g, 5.00 mmol) and L c(0.78 g, 5.00 mmol) was mixed with deionized water (10.00 g) and added to the reaction bottle at a uniform speed within 3 h. After the addition was completed, the reaction was kept warm for 4 h. The emulsion was cooled and centrifuged to obtain a solid. The solid was washed three times with deionized water at 60 ° C and dried to obtain the product Zn 2 L c 2 [Al(CN) 4 L e ] 4 , yield 81%. Elemental analysis (C 72 H 52 N 44 B 4 Zn 2 Al 4 , mass percentage), theoretical value: C 47.63, H 2.87, N 33.96; measured value: C 47.10, H 3.03, N 33.74.
[0078] Example 3
[0079] The synthesis reaction equation of mononuclear magnesium A1 is:
[0080]
[0081] The specific preparation steps of mononuclear magnesium metal A1 are:
[0082] Under the protection of inert gas, raw material A1-1 (10.00 g, 61.35 mmol), raw material A1-2 (9.59 g, 61.35 mmol) and paraformaldehyde (2.76 g, 92.03 mmol) in a molar ratio of 1:1:1.5 were mixed, dissolved in methanol (47.95 g) in a mass ratio of 5:1 to raw material A1-2, and stirred for reaction at 60 ° C for 12 h. After cooling to room temperature, hydrochloric acid ethanol solution (mass fraction 30%, 8.96 g, 73.62 mmol) in a molar ratio of 1.2:1 to raw material A1-2 was added to obtain a white precipitate. The filter cake was collected by filtration and washed with methanol for 3 times, dried, dissolved in water in a mass ratio of 3:1 to the filter cake, and precipitated with NaHCO 3The pH value of the solution was adjusted to 6-7 with a saturated aqueous solution, and dichloromethane was added in a mass ratio of 5:1 to the filter cake for extraction three times. The organic phase was collected, and a desiccant was added to remove water, and then dichloromethane was removed under reduced pressure to obtain mononuclear magnesium A1 ligand (19.51 g, 58.90 mmol) with a yield of 96%. Under the protection of inert gas, the mononuclear magnesium A1 ligand (10.00 g, 30.18 mmol) was dissolved in n-hexane (50.00 g) at a mass ratio of 5:1 with the mononuclear magnesium A1 ligand, and di-n-butyl magnesium (1M, 30.18 mL, 30.18 mmol) at a molar ratio of 1:1 was added dropwise at 0°C for 3 h. After the addition was completed, the mixture was kept warm for 2 h. HCl (1.10 g, 30.18 mmol) at a molar ratio of 1:1 with the mononuclear magnesium A1 ligand was added, and the mixture was kept warm for 2 h. A white precipitate was precipitated, and the filter cake was collected by filtration. The filter cake was washed with n-hexane 3 times and dried in vacuo to obtain mononuclear magnesium A1 (11.53 g, 29.58 mmol) with a yield of 98%. 1 H NMR (CDCl 3 ,400MHz): δ1.18(m,2H),1.48-1.55(m,4H),2.25(m,2H),2.28(s,6H),2.38(s,3H),2.49-2.57(m,2H),3.71(s,2H),6.93(s,1H),7.29(s,1H).
[0083] Example 4
[0084] The synthesis reaction equation of binuclear magnesium metal B1 is:
[0085]
[0086] The specific preparation steps of binuclear magnesium metal B1 are:
[0087] Under nitrogen protection, 2-methoxyhydroquinone (4.21 g, 30.08 mmol) and triethylamine (3.04 g, 30.08 mmol) in a molar ratio of 1:1 were mixed in dichloromethane (20.00 g), and the temperature was kept at 0°C. Pivaloyl chloride (4.35 g, 36.10 mmol) in a molar ratio of 1.2:1 with 2-methoxyhydroquinone was added dropwise to the reaction solution for 3 hours. After the addition was completed, the mixture was kept warm for 2 hours, filtered, and the filtrate was collected. Dichloromethane was removed by distillation under reduced pressure to obtain a crude intermediate B1-1, which was then purified by column chromatography (developing solvent: petroleum ether: ethyl acetate volume ratio = 5:1) to obtain intermediate B1-1 (5.26 g, 23.46 mmol, yield 78%). Under the protection of inert gas, the raw material intermediate B1-1 (10.00 g, 44.58 mmol), raw material B1-1 (5.80 g, 44.58 mmol) and paraformaldehyde (2.00 g, 66.87 mmol) in a molar ratio of 1:1:1.5 were mixed, dissolved in ethanol (17.40 g) in a mass ratio of 3:1 with the raw material B1-1 (N,N,N'-trimethyl-1,4-butanediamine), and then stirred at 80 ° C for 14 h, and hydrochloric acid ethanol solution (mass fraction 30%, 6.51 g, 53.50 mmol) in a molar ratio of 1.2:1 with the raw material B1-1 was added to obtain a white precipitate, filtered, collected the filter cake, and washed with ethanol. The dried filter cake was dissolved in water in a mass ratio of 3:1 with it, and washed with NaHCO 3The pH value of the solution was adjusted to 6-7 with a saturated aqueous solution, and dichloroethane was added in a mass ratio of 5:1 to the filter cake for extraction three times. The organic phase was collected, a desiccant was added to remove water, and dichloroethane was removed under reduced pressure to obtain intermediate B1-2 (14.46 g, 39.68 mmol) with a yield of 89%. The intermediate B1-2 (10.00 g, 27.43 mmol) was dissolved in methanol (40.00 g) at a mass ratio of 4:1 with the intermediate B1-2. The reaction temperature was controlled at -5°C. An aqueous NaOH solution (30% mass fraction, 14.63 g, 109.72 mmol) at a molar ratio of 4:1 with the intermediate B1-2 was added dropwise. The addition was completed after 3 hours. An aqueous hydrochloric acid solution (15% mass fraction) was added dropwise to adjust the solution pH to 6-7. Dichloroethane was added at a mass ratio of 6:1 with the intermediate B1-2 and extracted three times. After drying, the dichloroethane was removed under reduced pressure to obtain a colorless oily liquid, namely the intermediate B1-3 (6.38 g, 22.77 mmol) with a yield of 83%. Under the protection of inert gas, glutaric acid (5.00 g, 37.85 mmol) was dissolved in dichloroethane (15.00 g) at a mass ratio of 3:1 at room temperature, and then DIC (N, N'-diisopropylcarbodiimide) (9.55 g, 75.70 mmol) at a molar ratio of 2:1 to glutaric acid was added, stirred and mixed for 20 minutes, and intermediate B1-3 (21.22 g, 75.70 mmol) at a molar ratio of 2:1 to glutaric acid was added. The reaction was kept at room temperature for 48 hours to obtain a reddish-brown liquid. The dichloroethane was removed by vacuum distillation to obtain a crude binuclear magnesium metal B1 ligand. Methanol in a mass ratio of 3:1 to the crude binuclear magnesium B1 ligand was added, slurried for 3 hours, filtered, the filter cake was collected, and washed with methanol 3 times, and dried to obtain binuclear magnesium B1 ligand (14.94 g, 22.71 mmol), with a yield of 60%. Under the protection of inert gas, the binuclear magnesium B1 ligand (10.00 g, 15.20 mmol) was dissolved in petroleum ether in a mass ratio of 10:1 to the crude binuclear magnesium B1 ligand, and di-n-butyl magnesium (1M, 30.40 mL, 30.40 mmol) in a molar ratio of 2:1 to the crude binuclear magnesium B1 ligand was added dropwise at 20°C for 6 hours. After the addition was completed, the mixture was kept warm for 2 hours, and CH in a molar ratio of 2:1 to the crude binuclear magnesium B1 ligand was added. 3 COOH (1.82 g, 30.40 mmol) was added and the reaction was kept warm for 2 h. A white precipitate was precipitated. The filter cake was collected by filtration and washed with petroleum ether for 3 times. After vacuum drying, binuclear magnesium B1 (11.29 g, 13.68 mmol) was obtained with a yield of 90%. 1 HNMR (CDCl 3 ,400MHz): δ1.74(m,2H),1.82-1.87(m,8H),2.20(s,12H),2.41-2.46(m,18H),3.73(s,4H),3.81(s,6H),6.86(s,2H),7.25(s,2H).
[0088] Example 5
[0089] The synthetic reaction equation of polymer magnesium metal C1 is:
[0090]
[0091] The specific preparation steps of polymer magnesium metal C1 are:
[0092] Under the protection of inert gas, tert-butylhydroquinone (1.66 g, 10.00 mmol), raw material C1-1 (1.16 g, 10.00 mmol) and paraformaldehyde (0.45 g, 15.00 mmol) in a molar ratio of 1:1:1.5 were mixed, ethanol (5.00 g) was added to dissolve, and the reaction was continued at 80°C for 14 h with stirring, and a hydrochloric acid ethanol solution (mass fraction 30%, 1.46 g, 12.00 mmol) in a molar ratio of 1.2:1 with the raw material C1-1 was added to obtain a white precipitate, which was filtered and the filter cake was collected and washed with ethanol. The dried filter cake was dissolved in water in a mass ratio of 3:1 with water and washed with NaHCO 3The pH value of the solution was adjusted to 6-7 with a saturated aqueous solution, and dichloroethane was added in a mass ratio of 5:1 to the filter cake for extraction three times. The organic phase was collected, and a desiccant was added to remove water, and then the dichloroethane was removed under reduced pressure to obtain the crude intermediate C1-1, which was then purified by column chromatography (the developing solvent was petroleum ether: ethyl acetate, volume ratio = 10:1) to obtain intermediate C1-1 (1.65 g, 5.60 mmol) with a yield of 56%. Under the protection of inert gas, the intermediate C1-1 (10.00 g, 33.97 mmol) was dissolved in toluene (40.00 g), and TEA (triethylamine, 3.78 g, 37.36 mmol) was added in a molar ratio of 1.1:1 to the intermediate C1-1. Then, acryloyl chloride (3.38 g, 37.36 mmol) was diluted with toluene (16.90 g) in a molar ratio of 1.1:1 to the intermediate C1-1. Acryloyl chloride was added dropwise to the solution of the intermediate C1-1 at 0°C for 4 hours. After the addition was completed, the mixture was kept warm for 1 hour, filtered, and the filtrate was collected. The toluene was removed by distillation under reduced pressure to obtain the intermediate C1-2 (11.37 g, 32.61 mmol) with a yield of 96%. AIBN (azobisisobutyronitrile, 28.27 mg, 0.17 mmol) with a molar ratio of 500:1 to methyl acrylate was added to the reaction flask, the temperature was raised to 60°C, the intermediate C1-2 (10.00 g, 28.69 mmol) and methyl acrylate (7.41 g, 86.08 mmol) with a molar ratio of 1:3 were dissolved in toluene (87.05 g), and the mixture was added dropwise to the reaction flask within 10 hours. After the reaction, the toluene was removed by vacuum distillation to obtain the polymer-type magnesium metal C1 ligand (17.41 g), with a yield of 100%. Under the protection of inert gas, the polymer-type magnesium metal C1 ligand (10.00 g) was dissolved in cyclohexane (50.00 g) with a mass ratio of 5:1 to the ligand, and di-n-butyl magnesium (1M, 16.48 mL, 16.48 mmol) with a molar ratio of n:1 to the ligand was added dropwise at 20°C for 3 hours, and the mixture was kept warm for 2 hours after the addition was completed. Then add CF with a molar ratio of n:1 to the polymer magnesium C1 ligand 3 COOH (0.53 g, 16.48 mmol) was added and the reaction was kept warm for 2 h. A white precipitate was precipitated. The filter cake was collected by filtration and washed with cyclohexane for 3 times. After vacuum drying, polymer magnesium metal C1 (10.35 g, 15.66 mmol) was obtained with a yield of 95%. 1 H NMR (CDCl 3 ,400MHz): δ1.48(s,9H),1.50(m,2H),1.55-1.93(m,8H),2.13(s,6H),2.27(m,4H), 2.36(s,3H),2.45-2.53(m,4H),3.66(s,9H),3.74(s,2H),6.85(s,1H),7.22(s,1H).
[0093] Example 6
[0094] In a 100mL reaction bottle equipped with a magnet, dry at 120℃ for more than 12h, evacuate and wait until it cools to room temperature, and flush with nitrogen for use. Under nitrogen protection, weigh propylene oxide (17.4g, 300.00mmol) and succinic anhydride (10.0g, 100.00mmol) at a molar ratio of 3:1 at room temperature, add toluene (40.00g) and heat to 80℃ to dissolve, add to the dropping tank for use. Weigh ZnL with a mass ratio of 1:5000 to propylene oxide. b 2 [Fe(CN) 4 L d ] 2 (3.48mg), add polyethylene glycol 400 (0.60g, 1.50mmol) with a molar ratio of 1:200 to propylene oxide, heat to 90℃, add the solution in the drop-adding tank to the reactor at a uniform rate within 2h, keep warm and react for 10min to obtain a soft segment polymer. Weigh L-lactide (6.85g, 47.57mmol) with a mass ratio of 1:4 to the soft segment polymer, then add mononuclear metal magnesium A1 (37.10mg, 0.095mmol) with a molar ratio of 1:500 to L-lactide, react at 25℃ for 5h to obtain a triblock polymer. Take out a very small amount of the reaction mixture for GPC testing. GPC test shows that the polymerization molecular weight is 33.5kg / mol and the molecular weight distribution is 1.68. The remaining reaction polymer is dissolved in dichloromethane and precipitated in a large amount of methanol, and vacuum dried to obtain an aliphatic thermoplastic polyester elastomer with a hard segment content of 20wt%. Thermal property tests show that the glass transition temperature of the obtained aliphatic thermoplastic polyester elastomer is -20° C. and the melting point is 170° C. Mechanical property tests show that the maximum tensile strength of the obtained aliphatic thermoplastic polyester elastomer is 10 MPa and the elongation at break is 750%.
[0095] Example 7
[0096] In a 100mL reaction bottle equipped with a magnet, dry at 120℃ for more than 12h, evacuate and wait until it cools to room temperature, and flush with nitrogen for use. Under nitrogen protection, weigh propylene oxide (10.00g, 172.41mmol) and succinic anhydride (17.24g, 172.41mmol) in a molar ratio of 1:1 at room temperature, add dichloroethane (40.00g) and heat to 50℃ to dissolve, add to the dropping tank for use. Weigh Zn with a mass ratio of 1:7500 to propylene oxide. 2 L c 2 [Al(CN) 4 L e ] 4(1.33mg), add polypropylene glycol 600 (0.17g, 0.29mmol) with a molar ratio of 1:600 to propylene oxide, heat to 50℃, add the solution in the drop-adding tank to the reactor at a uniform rate within 2h, keep warm and react for 10min to obtain a soft segment polymer. Weigh L-lactide (18.16g, 126.11mmol) with a mass ratio of 2:3 to the soft segment polymer, then add binuclear metal magnesium B1 (52.02mg, 0.063mmol) with a molar ratio of 1:2000 to L-lactide, react at 120℃ for 1h to obtain a triblock polymer. Take out a very small amount of the reaction mixture for GPC testing. GPC test shows that the polymerization molecular weight is 78.5kg / mol and the molecular weight distribution is 1.63. The remaining reaction polymer is dissolved in dichloromethane and precipitated in a large amount of methanol, and vacuum dried to obtain an aliphatic thermoplastic polyester elastomer with a hard segment content of 40wt%. Thermal property tests show that the glass transition temperature of the obtained aliphatic thermoplastic polyester elastomer is -8°C and the melting point is 170°C. Mechanical property tests show that the maximum tensile strength of the obtained aliphatic thermoplastic polyester elastomer is 22 MPa and the elongation at break is 1000%.
[0097] Example 8
[0098] In a 100mL reaction bottle equipped with a magnet, dry at 120℃ for more than 12h, evacuate and wait until it cools to room temperature, and then flush with nitrogen for use. Under nitrogen protection, weigh propylene oxide (10.00g, 172.41mmol) and succinic anhydride (2.87g, 28.74mmol) at a molar ratio of 6:1 at room temperature, add 1,4-dioxane (20.00g), heat to 120℃ to dissolve, and add to the dropping tank for use. Weigh Zn with a mass ratio of 1:5000 to propylene oxide. 2 L c 2 [Al(CN) 4 L e ] 4(2.00mg), add ethylene glycol (10.70mg, 0.17mmol) with a molar ratio of 1:1000 to propylene oxide, heat to 120℃, add the solution in the drop-adding tank to the reactor at a uniform rate within 4h, keep warm and react for 10min to obtain a soft segment polymer. Weigh L-lactide (51.48g, 357.50mmol) with a mass ratio of 4:1 to the soft segment polymer, then add polymer-type metal magnesium C1 (11.80mg, 0.018mmol) with a molar ratio of 1:20000 to L-lactide, react at 120℃ for 5h to obtain a triblock polymer. Take out a very small amount of the reaction mixture for GPC testing. GPC test shows that the polymerization molecular weight is 60.3kg / mol and the molecular weight distribution is 1.59. Then add HDI (215.40 mg, 1.28 mmol) with a molar ratio of 1.2:1 to the triblock, keep warm at 60°C for 1 hour to obtain a multi-block polymer. Take out a very small amount of the reaction mixture for GPC testing. GPC test shows that the polymerization molecular weight is 125.0 kg / mol and the molecular weight distribution is 1.89. The remaining reaction polymer is dissolved in dichloromethane and precipitated in a large amount of methanol, and vacuum dried to obtain an aliphatic thermoplastic polyester elastomer with a hard segment content of 80 wt%. Thermal performance tests show that the glass transition temperature of the obtained aliphatic thermoplastic polyester elastomer is -43°C and the melting point is 170°C. Mechanical property tests show that the maximum tensile strength of the obtained aliphatic thermoplastic polyester elastomer is 40 MPa and the elongation at break is 350%.
[0099] Example 9
[0100] In a 100mL reaction bottle equipped with a magnet, dry at 120℃ for more than 12h, evacuate and wait until it cools to room temperature, and flush with nitrogen for use. Under nitrogen protection, weigh propylene oxide (10.00g, 172.41mmol) and succinic anhydride (1.72g, 17.24mmol) at a molar ratio of 10:1 at room temperature, add n-hexane (20.00g) and heat to 80℃ to dissolve, add to the dropping tank for use. Weigh ZnL with a mass ratio of 1:10000 to propylene oxide. b 2 [Fe(CN) 4 L d ] 2(1.00mg), add polyethylene glycol 400 (34.48mg, 0.086mmol) with a molar ratio of 1:2000 to propylene oxide, heat to 80℃, add the solution in the drop-adding tank to the reactor at a uniform rate within 2.5h, keep warm and react for 10min to obtain a soft segment polymer. Weigh L-lactide (11.72g, 81.39mmol) with a mass ratio of 1:1 to the soft segment polymer, then add binuclear metal magnesium B1 (14.00mg, 0.016mmol) with a molar ratio of 1:5000 to L-lactide, react at 50℃ for 2h to obtain a triblock polymer. Take out a very small amount of the reaction mixture for GPC testing. GPC test shows that the polymerization molecular weight is 89.3kg / mol and the molecular weight distribution is 1.65. Then add MDI (65.62 mg, 0.26 mmol) with a molar ratio of 1:1 to the triblock, keep the temperature at 80°C for 0.5 h to obtain a multi-block polymer. Take out a very small amount of the reaction mixture for GPC testing. The GPC test shows that the polymerization molecular weight is 197.8 kg / mol and the molecular weight distribution is 2.21. The remaining reaction polymer is dissolved in dichloromethane and precipitated in a large amount of methanol, and vacuum dried to obtain an aliphatic thermoplastic polyester elastomer with a hard segment content of 50 wt%. Thermal performance tests show that the glass transition temperature of the obtained aliphatic thermoplastic polyester elastomer is -48°C and the melting point is 170°C. Mechanical property tests show that the maximum tensile strength of the obtained aliphatic thermoplastic polyester elastomer is 32 MPa and the elongation at break is 950%.
[0101] Example 10
[0102] In a 100mL reaction bottle equipped with a magnet, dry at 120℃ for more than 12h, evacuate and wait until it cools to room temperature, and flush with nitrogen for use. Under nitrogen protection, weigh propylene oxide (10.00g, 172.41mmol) and succinic anhydride (4.31g, 43.10mmol) at a molar ratio of 4:1 at room temperature, add toluene (30.00g) and heat to 90℃ to dissolve, add to the dropping tank for use. Weigh ZnL with a mass ratio of 1:7500 to propylene oxide. b 2 [Fe(CN) 4 L d ] 2(1.33mg), add polypropylene glycol 600 (51.72mg, 0.086mmol) with a molar ratio of 1:2000 to propylene oxide, heat to 90℃, add the solution in the drop-adding tank to the reactor at a uniform rate within 3h, keep warm and react for 10min to obtain a soft segment polymer. Weigh L-lactide (7.71g, 53.50mmol) with a mass ratio of 7:13 to the soft segment polymer, then add polymer-type metal magnesium C1 (3.53mg, 0.005mmol) with a molar ratio of 1:10000 to L-lactide, react at 80℃ for 4h to obtain a triblock polymer. Take out a very small amount of the reaction mixture for GPC testing. GPC test shows that the polymerization molecular weight is 75.3kg / mol and the molecular weight distribution is 1.66. Then add HDI (54.11 mg, 0.32 mmol) with a molar ratio of 1:1 to the triblock, keep warm at 120°C for 2 hours to obtain a multi-block polymer. Take out a very small amount of the reaction mixture for GPC testing. GPC test shows that the polymerization molecular weight is 153.5 kg / mol and the molecular weight distribution is 1.80. The remaining reaction polymer is dissolved in dichloromethane and precipitated in a large amount of methanol, and vacuum dried to obtain an aliphatic thermoplastic polyester elastomer with a hard segment content of 35wt%. Thermal performance tests show that the glass transition temperature of the obtained aliphatic thermoplastic polyester elastomer is -34°C and the melting point is 170°C. Mechanical property tests show that the maximum tensile strength of the obtained aliphatic thermoplastic polyester elastomer is 23MPa and the elongation at break is 1500%.
[0103] The above description is only a preferred embodiment of the present invention. All equivalent changes and modifications made according to the scope of the patent application of the present invention should fall within the scope of the present invention.
Claims
1. A method for preparing an aliphatic thermoplastic polyester elastomer, It is characterized in that The aliphatic thermoplastic polyester elastomer is a triblock or multiblock polymer with a "hard"-"soft"-"hard" structure prepared by chain transfer method or chain extension method. The ratio of the soft segment to the hard segment in the triblock or multiblock polymer can be adjusted, and the hard segment content is 20-80wt%; The preparation method of the aliphatic thermoplastic polyester elastomer is as follows: propylene oxide, succinic anhydride, a first catalyst, a chain initiator and an organic solvent are added to a reactor to carry out a first polymerization reaction to obtain a soft segment polymer; L-lactide monomer and a second catalyst are added in situ to carry out a second polymerization reaction by a chain transfer method to obtain a "hard"-"soft"-"hard" triblock polymer; a chain extender is selectively added to the original solution to carry out a third polymerization reaction by a chain extension method to obtain a multi-block polymer; the molar ratio of propylene oxide to succinic anhydride is 1-11:1; The first catalyst has the general structural formula M 1 a L 1 b [M 2 (CN) c L 2 d ] e [H 2 O] f ; Where: M 1 Selected from Zn 2+ 、Co 2+ 、Ni 2+ , Fe 2+ , Fe 3+ , Ca 2+ Mg 2+ , Cu 2+ Sn 2+ 、Cd 2+ or Pb 2+ ;M 2 Selected from Al 3+ 、Co 3+ , Fe 3+ Cr 3+ or Mn 3+ ; a, c and e are non-zero natural numbers, b, d and f are natural numbers; L 1 With L 2 The structures are the same or different, specifically one of the following structures: ; The second catalyst is one of the following catalysts: ; Where: R is ; R 1 H, OH, C 1 ~C 4 Alkyl, C 1 ~C 4 Alkoxy, F, Cl, Br or NO 2 Group; R 2 H, C 1 ~C 4 Alkyl, C 1 ~C 4 Alkoxy, F, Cl, Br or NO 2 Group; R 3 C 1 ~C 4 alkyl; R 4 C 1 ~C 4 alkyl; R 5 C 1 ~C 4 alkyl; X is Cl, NO 3 CF 3 COO、CH 3 COO, BF 4 , CH 3 O、CH 3 CH 2 , or CH 3 CH 2 CH 2 CH 2 Group; g = 0, 1, 2, 4, 6, or 8; h is a non-zero natural number; i is a non-zero natural number; y is a non-zero natural number.
2. The method for preparing an aliphatic thermoplastic polyester elastomer according to claim 1, It is characterized in that In the first polymerization reaction, the chain initiator is one of ethylene glycol, glycerol, pentaerythritol, polyethylene glycol 400, and polypropylene glycol 600; the mass ratio of the first catalyst to propylene oxide is 1:5000-10000; the molar ratio of propylene oxide to the chain initiator is 200-2000:1; and the organic solvent is any one of toluene, xylene, tetrahydrofuran, dichloromethane, dichloroethane, n-hexane, and 1,4-dioxane.
3. The method for preparing an aliphatic thermoplastic polyester elastomer according to claim 1, It is characterized in that In the second polymerization reaction, the molar ratio of metal magnesium to L-lactide in the second catalyst is 1:500-20000.
4. The method for preparing an aliphatic thermoplastic polyester elastomer according to claim 1, It is characterized in that In the third polymerization reaction, the chain extender is one of toluene-2,4-diisocyanate, hexamethylene diisocyanate, 4,4'-methylenebis(phenyl isocyanate), terephthaloyl chloride and adipoyl chloride; and the molar ratio of the chain extender to the triblock polymer is 1-1.2:
1.
5. The method for preparing an aliphatic thermoplastic polyester elastomer according to claim 1, It is characterized in that The first polymerization reaction temperature is 50-120°C, and the first polymerization reaction time is 2-4 hours; The second polymerization reaction temperature is 25-120°C, and the second polymerization reaction time is 1-5 h; The third polymerization reaction temperature is 60-120° C., and the third polymerization reaction time is 0.5-2 h.
6. The method for preparing an aliphatic thermoplastic polyester elastomer according to claim 1, It is characterized in that The glass transition temperature of the soft segment polymer can be adjusted in the range of -8 to -48 °C.
7. The method for preparing an aliphatic thermoplastic polyester elastomer according to claim 1, It is characterized in that The number average molecular weight of the aliphatic thermoplastic polyester elastomer is 30.0-200.0 kg / mol.
8. The method for preparing an aliphatic thermoplastic polyester elastomer according to claim 1, It is characterized in that The aliphatic thermoplastic polyester elastomer has an operating window temperature of -48 to 170°C, a maximum tensile strength of 10 to 40 MPa, and an elongation at break of 300 to 1500%.
Citation Information
Patent Citations
Preparation method of biodegradable block copolymer
CN109776773A
Catalyst system for preparing block polymer and method for catalytic synthesis of block polymer
CN110317332A
Catalytic system and synthesis method of multi-block copolymer
CN114456363A
Biodegradable copolymer for medical use
JP1994298917A
KR20210092180A