Inorganic slurry, N-type battery slurry and preparation method thereof

By using inorganic additives in inorganic slurry in N-type battery slurry to promote the precipitation of silver grains, the problem of obstruction of silver grain growth control and current transmission is solved, and the conversion efficiency of solar cell cells and the dispersion of slurry is improved. sex.

CN116364331BActive Publication Date: 2024-11-08NANTONG AISHENG NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310569998.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-19
Publication Date
2024-11-08
Estimated Expiration
2043-05-19

AI Technical Summary

Technical Problem

In N-type battery paste, the prior art is difficult to effectively control the growth size and quantity of silver grains, resulting in high contact resistance and excessive glass powder content and hinder current transmission, poor dispersion, affecting the conversion efficiency of solar cell cells.

Method used

Using an inorganic slurry, including an organic carrier, an inorganic additive and a dispersant, the Ag ions dissolved in the glass phase are reduced to silver micelles in the intermediate sintering stage through a redox reaction, and the size and number of silver grains are controlled, and Mix in the battery paste to improve the sintering effect and adhesion of the silver powder.

Benefits of technology

Effectively reduce contact resistance, increase the number of silver grains, improve the ohmic contact between metal and semiconductors, improve the conversion efficiency of solar cell cells, reduce dependence on glass powder, improve the dispersion and printing of slurry performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116364331B_ABST
    Figure CN116364331B_ABST
Patent Text Reader

Abstract

The present invention proposes an inorganic slurry, an N-type battery slurry and a preparation method thereof, which belong to a conductive slurry for solar cells. The inorganic slurry includes: 50 to 90 parts by mass of an organic carrier; 0.1 to 30 parts by mass of an inorganic additive; 0.1 to 10 parts by mass of a dispersant; and 5 to 40 parts by mass of a solvent. When the inorganic slurry of the present invention is used in an N-type battery slurry, in the intermediate sintering stage, the inorganic additive can reduce the Ag ions dissolved in the glass phase to silver micelles through an oxidation-reduction reaction, thereby controlling the size and quantity of silver in the silver micelles, that is, promoting the precipitation of silver grains, so as to further improve the metal semiconductor ohmic contact, reduce metal recombination, and improve the conversion efficiency of solar cells.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of conductive paste for solar cells, and in particular relates to an inorganic paste, an N-type battery paste and a preparation method thereof. Background Art

[0002] The working principle of solar cells is based on the photovoltaic effect of semiconductor PN junction. When pure silicon is mixed with phosphorus atoms, only a small amount of energy is needed to make a "redundant" electron of the phosphorus atom (five electrons in the outermost layer) escape. When phosphorus atoms are used for doping, the resulting silicon is called N-type ("n" means negative electricity). Injecting boron into N-type semiconductor materials to form a p+ / n-type solar cell is called an n-type silicon wafer. N-type silicon wafers usually have a longer minority carrier lifetime and higher battery efficiency.

[0003] Conductive paste for N-type crystalline silicon solar cells mainly includes front silver aluminum paste and back fine grid silver paste. Conductive paste is mainly composed of metal filler, inorganic binder, organic carrier, etc.

[0004] However, in N-type battery paste, the metal filler is mainly silver powder, which is the main body of the conductive function. Its quality will directly affect the bulk resistance and contact resistance of the electrode material. Among them, the recrystallized silver particles deposited on silicon are considered to be the only channel for current transmission. The silver particles form a good metal semiconductor ohmic contact with the underlying silicon, which is directly responsible for the transmission of current from the silicon emitter area to the silver grid line, and has a very low contact resistance with the silicon emitter area.

[0005] At present, the main component that promotes the deposition of silver powder on silicon is an inorganic binder, such as glass powder. The mechanism of action of the inorganic binder glass powder is as follows: ① Initial sintering stage: Ag shrinks rapidly, and due to the presence of O, silver turns into silver ions and dissolves in the glass; due to the capillary attraction, the glass phase carries the Ag ions and penetrates downward along the channel. The lower the glass viscosity, the faster it reaches and corrodes the SiNx anti-reflection film layer; ② Intermediate sintering stage: Silver particles become more and more dense, and there are continuous pore channels. The glass phase with low viscosity can quickly pass through to the SiNx layer, while the glass phase with high viscosity has no time to pass through and is retained in isolated holes. The Ag ions in the glass phase will react with SiNx to generate Ag atoms. ③ Final sintering stage (<730℃): Ag shrinks slowly, and only a small amount of glass phase is retained in the glass system with low viscosity, and the corrosion reaction is uniform; in the glass system with high viscosity, a large amount of glass phase will be retained, and the corrosion reaction is uneven. As the temperature rises, the silver precipitation at the glass phase interface decreases, and Ag crystals appear in the Si layer.

[0006] Based on the above mechanism, it can be known that the number and size of silver grains are related to the contact resistance, but the more recrystallized silver grains there are, the larger their size, and the lower their contact resistance. The contact resistance also depends on the thickness of the glass layer deposited on the silicon surface. In other words, the number of silver grains does not directly determine the contact resistance. When the glass content is very low, the number of precipitated silver grains is very small, which is not conducive to reducing the contact resistance. When the glass content is high, although the number of generated silver grains increases, the thickness of the glass layer between the recrystallized silver grains and the silver thick film will also increase, resulting in obstruction of current transmission, which is also not conducive to reducing the contact resistance.

[0007] Therefore, when only glass powder is included in the N-type battery paste, the growth size of the silver grains cannot be controlled, and when the glass powder content is low, the number of precipitated silver grains is small. When the glass powder content is high, problems such as current transmission obstruction and metal composite occur, which is not conducive to reducing contact resistance. In addition, the current preparation method of the N-type battery paste is to directly mix the components together, and the dispersibility of the inorganic powder is poor, and the conversion efficiency of the battery cell is low. Summary of the invention

[0008] The present invention aims to solve at least one of the technical problems existing in the prior art, and provides an inorganic slurry, an N-type battery slurry and a preparation method thereof.

[0009] In one aspect of the present invention, an inorganic slurry is provided for N-type battery slurry, wherein the inorganic slurry comprises: 50 to 90 parts by mass of an organic carrier;

[0010] 0.1 to 30 parts by mass of an inorganic additive;

[0011] 0.1 to 10 parts by mass of a dispersant;

[0012] 5 to 40 parts by mass of solvent.

[0013] Optionally, the inorganic additive includes at least one of graphene, indium powder, silicon powder, boron powder and zinc powder.

[0014] Optionally, the particle size D50 of the inorganic additive is in the range of 0.05 μm to 2 μm.

[0015] Optionally, the organic vehicle includes 3 to 5 parts by mass of PVB resin and 5 to 10 parts by mass of acrylic resin.

[0016] Optionally, the dispersant includes at least one of a pigment group copolymer, a highly branched polyester, a fatty acid, a polyamide, and an acidic group-containing copolymer.

[0017] Optionally, the solvent includes at least one of diethylene glycol butyl ether, polyoxymethylene dimethyl ether, butyl carbitol, dibutyl phthalate, and diethylene glycol butyl ether acetate.

[0018] Another aspect of the present invention provides an N-type battery slurry, comprising:

[0019] 80-90 parts by mass of conductive silver powder;

[0020] 4 to 10 parts by weight of an organic carrier;

[0021] 0.1 to 5 parts by mass of aluminum powder;

[0022] 1 to 6 parts by mass of glass powder;

[0023] 0.1 to 2 parts by mass of additives;

[0024] 0.1 to 5 parts by weight of inorganic slurry, wherein the inorganic slurry is the inorganic slurry described above.

[0025] Another aspect of the present invention provides a method for preparing the N-type battery slurry as described above, the preparation method comprising:

[0026] obtaining an inorganic slurry;

[0027] The inorganic slurry is mixed evenly with conductive silver powder, organic carrier, aluminum powder, glass powder and additives, and subjected to grinding and dispersion treatment to obtain N-type battery slurry.

[0028] Optionally, obtaining the inorganic slurry comprises:

[0029] The inorganic additive, dispersant and solvent are mixed, and the mixture is dispersed and homogenized by stirring to obtain an intermediate slurry;

[0030] Resin is added to the intermediate slurry, and the mixture is stirred and dispersed to obtain an inorganic slurry.

[0031] Optionally, the mass ratio of the inorganic additive to the dispersant is in the range of (70-87.5): (12.5-30);

[0032] The mass ratio of the inorganic additive to the solvent is in the range of (10-40): (60-90);

[0033] The mass ratio of the intermediate slurry to the organic carrier is in the range of (10-50): (50-90).

[0034] The present invention provides an inorganic slurry, an N-type battery slurry and a preparation method thereof, wherein the inorganic slurry comprises: 50 to 90 parts by mass of an organic carrier; 0.1 to 30 parts by mass of an inorganic additive; 0.1 to 10 parts by mass of a dispersant; and 5 to 40 parts by mass of a solvent. When the inorganic slurry of the present invention is used in the N-type battery slurry, in the intermediate sintering stage, the inorganic additive can reduce the Ag ions dissolved in the glass phase to silver micelles through an oxidation-reduction reaction, thereby controlling the size and quantity of the silver in the silver micelles, that is, promoting the precipitation of silver grains, so as to further improve the metal semiconductor ohmic contact, reduce metal recombination, and improve the conversion efficiency of solar cells. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 This is a powder SEM image of an inorganic slurry according to an embodiment of the present invention;

[0036] Figure 2 This is a SEM image of an N-type battery slurry with an inorganic additive added after sintering according to another embodiment of the present invention;

[0037] Figure 3 This is a SEM image of an N-type battery slurry without inorganic additives after sintering according to another embodiment of the present invention;

[0038] Figure 4 This is a flowchart of a method for preparing N-type battery slurry according to another embodiment of the present invention. DETAILED DESCRIPTION

[0039] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and specific implementation methods. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the described embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative work are within the scope of protection of the present invention.

[0040] Unless otherwise specified, the technical terms or scientific terms used in the present invention should be understood by people with ordinary skills in the field to which the present invention belongs. "Including" or "comprising" used in the present invention neither limits the shapes, numbers, steps and / or their groups mentioned, nor excludes the presence or addition of one or more other different shapes, numbers, steps and / or their groups.

[0041] In one aspect of the present invention, an inorganic slurry is provided for N-type battery slurry, wherein the inorganic slurry comprises: 50 to 90 parts by mass of an organic carrier, preferably 50 to 70 parts by mass of an organic carrier, which is beneficial to improving the printing performance of the slurry; 0.1 to 30 parts by mass of an inorganic additive, preferably 3 to 10 parts of an inorganic additive, which is beneficial to improving the photoelectric conversion efficiency of the battery and the printing performance of the slurry; 0.1 to 10 parts by mass of a dispersant, preferably 2 to 5 parts of a dispersant, which is beneficial to improving the dispersion uniformity of the inorganic additive, improving the photoelectric conversion efficiency of the battery and the printing performance of the slurry; 5 to 40 parts by mass of a solvent, preferably 30 to 40 parts of a solvent, which is beneficial to improving the printing performance of the slurry.

[0042] Combined Figure 1 As shown, according to the powder SEM image of the inorganic slurry, it can be seen that the particle size of the inorganic powder is mostly between 0.1μm and 0.2μm. The particle size of the inorganic powder in this range can improve the contact between the metal and the semiconductor, control the size and quantity of the silver micelles formed, and thus improve the conversion efficiency of the solar cell.

[0043] In this embodiment, when the inorganic slurry is used in the N-type battery slurry, in the intermediate sintering stage, the inorganic additive can reduce the Ag ions dissolved in the glass phase to silver micelles through redox reactions, thereby controlling the size and quantity of silver micelle silver, that is, promoting the precipitation of silver grains, so as to further improve the metal semiconductor ohmic contact, reduce metal recombination, and improve the conversion efficiency of solar cells. At the same time, the inorganic additive can also serve as a high-temperature bonding phase to play a role in the adhesion of the N-type battery slurry to the silicon wafer.

[0044] Specifically, the inorganic additive includes at least one of graphene, indium powder, silicon powder, boron powder and zinc powder.

[0045] In this embodiment, when the above-mentioned inorganic additives are used in N-type battery paste, based on the reducing property of each powder, the number of silver grains generated can be increased, the growth size of silver grains can be controlled, and metal composites can be reduced, which plays an important role in the sintering of silver powder and whether silver silicon can form a good ohmic contact.

[0046] Furthermore, the particle size D50 of the inorganic additive is in the range of 0.05 μm to 2 μm. When the median particle size D50 is within the above preferred range, the melting state is good, and the Ag ions dissolved in the glass phase can be reduced to silver micelles through redox reactions during the sintering process, thereby controlling the size and amount of silver micelles, and giving full play to the role of the inorganic additive, and the performance of the slurry is optimized.

[0047] In some preferred embodiments, the content of the above-mentioned inorganic additives may preferably be 0.1 parts by mass, 1 parts by mass, 5 parts by mass, 10 parts by mass, and 30 parts by mass, and the particle size D50 may preferably be 0.05 μm, 1 μm, and 2 μm. The higher the content of the inorganic additive and the smaller the particle size, the stronger its reducing property is, the more silver grains are generated, the ohmic contact is formed, the growth size of the silver grains is controlled, and the metal composite is reduced.

[0048] Furthermore, the organic carrier includes a resin with a molecular weight of 1000-90000, preferably 30000-60000, which is beneficial to improving the stability and printing performance of the N-type battery paste. Specifically, it includes 3 to 5 parts by mass of polyvinyl butyral (PVB resin) and 5 to 10 parts by mass of acrylic resin, that is, the above two resins are mixed to form a main resin. Of course, in this embodiment, the organic carrier may also include other resins, which are not specifically limited.

[0049] In some preferred embodiments, the PVB resin content may be preferably 3 parts by mass, 4 parts by mass, or 5 parts by mass. Within the above preferred content range, the battery slurry has good dispersant and wettability, and is also well compatible with other resins. During the printing process, alcohol and ester solvents evaporate. The acrylic resin content may be preferably 5 parts by mass, 8 parts by mass, or 10 parts by mass. Within the above preferred content range, the molecular weight of the resin is relatively large, and the macromolecules are easily aggregated into a film after the solvent evaporates, thereby improving printability. Moreover, as the temperature rises, the gradient evaporates with less residue.

[0050] It should be noted that, in the present embodiment, the organic carrier system volatilizes 15wt% at 150-200°C, 85wt% at 200-240°C, and 100wt% at 240-300°C. The above-mentioned organic carrier has a layered structure rather than being concentrated in a small temperature range to avoid concentrated volatilization leading to pores and cracks in the electrode grid lines; secondly, the slurry formed based on the organic carrier has good storage stability.

[0051] Furthermore, the dispersant includes at least one of a pigment group copolymer, a highly branched polyester, a fatty acid, a polyamide, and an acid group-containing copolymer.

[0052] In this embodiment, the block copolymer dispersant with pigment affinity group has the effect of wetting and reducing viscosity; the highly branched polyester dispersant has good film-forming property and can be used as a plasticizer to reduce viscosity; the fatty acid dispersant has the advantages of good thermal toughness and low viscosity; the polyamide dispersant is a series of polymers containing amide segments (-CONH-), which have the characteristics of hydrophilicity, high water absorption, hygroscopicity and quick drying, low gelling property, and good adhesion, tensile strain and ductility; the copolymer dispersant containing acidic group has wettability and dispersion stability for other inorganic pigments, reduces viscosity, and improves gloss and leveling.

[0053] In some preferred embodiments, the content of the above-mentioned dispersant may be preferably 0.1 parts by mass, 0.5 parts by mass, 2 parts by mass, 5 parts by mass, and 10 parts by mass. The higher the dispersant content, the more obvious the viscosity reduction effect. Among them, 5 parts by mass of dispersant corresponds to the best viscosity reduction effect.

[0054] Furthermore, the solvent includes at least one of diethylene glycol butyl ether, polyoxymethylene dimethyl ether, butyl carbitol, dibutyl phthalate, and diethylene glycol butyl ether acetate, and the above solvents have good solubility for components such as resins.

[0055] The present invention uses an inorganic slurry including an inorganic additive in an N-type battery slurry. Based on its reducibility, the inorganic slurry can promote the precipitation of Ag in the intermediate sintering stage, increase the number of silver grains, and control the size of the silver grains. Even when the glass material content is very low, a large number of silver grains can still be precipitated to improve the ohmic contact between the metal and the semiconductor, which is beneficial to reducing the contact resistance.

[0056] On the other hand, the present invention provides an N-type battery paste, comprising: 80 to 90 parts by mass of conductive silver powder; 4 to 10 parts by mass of an organic carrier; 0.1 to 5 parts by mass of aluminum powder; 1 to 6 parts by mass of glass powder; 0.1 to 2 parts by mass of an auxiliary agent (including a thixotropic agent, a defoaming agent, etc.); 0.1 to 5 parts by mass of the inorganic paste described above, preferably 2 to 4 parts by mass (for example, 2 parts by mass, 2.5 parts by mass, 3 parts by mass, 3.5 parts by mass and 4 parts by mass, etc.) of the aforementioned inorganic paste, which is beneficial to improving the photoelectric conversion efficiency of the battery while reducing the impact on the printing performance of the paste.

[0057] In the present embodiment, the N-type battery paste is an N-type silver paste. Based on the reducing property of the inorganic additive, the number of silver grains generated can be increased to form ohmic contact, the growth size of the silver grains can be controlled, and metal composites can be reduced. There is no need to add more glass powder. Only 1 to 6 parts by mass of glass powder are needed to precipitate a large number of silver grains, which can solve the problem of increased thickness of the glass layer between the recrystallized silver grains and the silver thick film caused by adding more glass powder.

[0058] like Figure 2As shown in Figure 2, in the battery slurry with inorganic additive powder added, a large amount of Ag is precipitated during the intermediate sintering stage, such as Figure 3 As shown, in the battery slurry without the addition of inorganic additive powder, Ag is wrapped in the glass phase during the intermediate sintering stage.

[0059] It should be noted that the organic carrier may also include 3 to 5 parts by mass of PVB resin and 5 to 10 parts by mass of acrylic resin, that is, a mixture of the above two resins as the main resin. Of course, in this embodiment, the organic carrier may also include other resins, which is not specifically limited.

[0060] In this embodiment, aluminum powders of different particle sizes have different activities. For example, the aluminum powder particle size D50 may preferably be 1.5-2.5 μm. Aluminum powder within this particle size range can effectively improve conductivity. Glass powder can use Pb-Zn-B-Si-In system as an inorganic bonding phase, which can fully wet the silver powder and the silicon substrate, so that the silver powder and the silicon substrate maintain good adhesion. Additives can promote sintering and help improve functionality.

[0061] Furthermore, in order to illustrate the performance of the battery slurry, it is necessary to print it into a battery cell and test the IV characteristics of the battery cell to illustrate the battery conversion efficiency, and further evaluate the impact of different inorganic additives on the performance of the battery cell. Combined with Table 3, it can be seen that compared with the slurry without adding inorganic additive powder, adding different inorganic additive powders will improve the conversion efficiency of the battery cell to varying degrees, and the conversion efficiency range is 24.56% to 24.76%.

[0062] like Figure 4 As shown, another aspect of the present invention provides a method S100 for preparing N-type battery slurry, comprising steps S110 to S120:

[0063] S110, obtaining an inorganic slurry, including the following process:

[0064] Step S1101, weigh a certain amount of inorganic additive powder and dispersant, the mass ratio of the two is in the range of (70-87.5): (12.5-30);

[0065] Step S1102, weighing a certain amount of solvent, the weight ratio of the inorganic additive powder weighed in step S1101 to the solvent is in the range of (10-40): (60-90);

[0066] Step S1103, mixing the inorganic additive and dispersant of step S1101 with the solvent of step S1102, and stirring and dispersing with a dispersing paddle for 30 to 90 minutes;

[0067] Step S1104, homogenizing the stirred slurry by (one or more of ultrasound, ball milling, and homogenization) to obtain a uniform intermediate slurry;

[0068] Step S1105, weigh the resin according to the mass ratio of the intermediate slurry to the organic carrier of (10-50): (50-90), and add the weighed resin to the intermediate slurry, and stir and disperse for 30-90 minutes to obtain an inorganic slurry.

[0069] S120, the inorganic slurry obtained in step S110 is evenly mixed with 80-90 parts by mass of conductive silver powder, 4-10 parts by mass of organic carrier, 0.1-5 parts by mass of aluminum powder, 1-6 parts by mass of glass powder and 0.1-2 parts by mass of additives, and then ground to a slurry fineness of ≤10 μm to obtain an electrode slurry, i.e., an N-type battery slurry.

[0070] The preparation method of the present invention adopts a step-by-step method to prepare battery slurry, first forming an inorganic slurry, dissolving the inorganic additive powder and components such as an organic carrier together, and then mixing the inorganic slurry with other materials to form an electrode slurry, so as to give full play to the role of the inorganic additive powder, achieve better mixing effect, and improve the dispersibility of the slurry.

[0071] The following will further illustrate the preparation method of inorganic slurry and N-type battery slurry in combination with several specific examples:

[0072] Example 1

[0073] The preparation method of the inorganic slurry in this example, the components and contents are shown in Table 1, and the specific steps include:

[0074] S1. Weigh 5 parts by mass of graphene, 1 part by mass of highly branched polyester, and 1 part by mass of polyamide;

[0075] S2, weighing 33 parts by mass of diethylene glycol butyl ether;

[0076] S3, mixing the inorganic additive and dispersant of step S1 with the solvent of step S2, and stirring and dispersing with a dispersing paddle for 30 to 90 minutes;

[0077] S4, homogenizing the stirred slurry by (one or more of ultrasound, ball milling, and homogenization) to obtain a uniform intermediate slurry;

[0078] S5. Weigh 60 parts by mass of an organic carrier, add the organic carrier to the intermediate slurry, and stir and disperse for 30 to 90 minutes to obtain an inorganic slurry.

[0079] Example 2

[0080] The preparation method of the inorganic slurry in this example, the components and contents are shown in Table 1, and the specific steps include:

[0081] S1. Weigh 5 parts by mass of indium powder, 1 part by mass of highly branched polyester, and 1 part by mass of polyamide;

[0082] S2, weighing 33 parts by mass of diethylene glycol butyl ether;

[0083] S3, mixing the inorganic additive and dispersant of step S1 with the solvent of step S2, and stirring and dispersing with a dispersing paddle for 30 to 90 minutes;

[0084] S4, homogenizing the stirred slurry by (one or more of ultrasound, ball milling, and homogenization) to obtain a uniform intermediate slurry;

[0085] S5. Weigh 60 parts by mass of an organic carrier, add the organic carrier to the intermediate slurry, and stir and disperse for 30 to 90 minutes to obtain an inorganic slurry.

[0086] Example 3

[0087] The preparation method of the inorganic slurry in this example, the components and contents are shown in Table 1, and the specific steps include:

[0088] S1, weighing 5 parts by mass of silicon powder, 1 part by mass of highly branched polyester, and 1 part by mass of polyamide;

[0089] S2, weighing 33 parts by mass of diethylene glycol butyl ether;

[0090] S3, mixing the inorganic additive and dispersant of step S1 with the solvent of step S2, and stirring and dispersing with a dispersing paddle for 30 to 90 minutes;

[0091] S4, homogenizing the stirred slurry by (one or more of ultrasound, ball milling, and homogenization) to obtain a uniform intermediate slurry;

[0092] S5. Weigh 60 parts by mass of an organic carrier, add the organic carrier to the intermediate slurry, and stir and disperse for 30 to 90 minutes to obtain an inorganic slurry.

[0093] Example 4

[0094] The preparation method of the inorganic slurry in this example, the components and contents are shown in Table 1, and the specific steps include:

[0095] S1. Weigh 5 parts by mass of boron powder, 1 part by mass of highly branched polyester, and 1 part by mass of polyamide;

[0096] S2, weighing 33 parts by mass of diethylene glycol butyl ether;

[0097] S3, mixing the inorganic additive and dispersant of step S1 with the solvent of step S2, and stirring and dispersing with a dispersing paddle for 30 to 90 minutes;

[0098] S4, homogenizing the stirred slurry by (one or more of ultrasound, ball milling, and homogenization) to obtain a uniform intermediate slurry;

[0099] S5. Weigh 60 parts by mass of an organic carrier, add the organic carrier to the intermediate slurry, and stir and disperse for 30 to 90 minutes to obtain an inorganic slurry.

[0100] Example 5

[0101] The preparation method of the inorganic slurry in this example, the components and contents are shown in Table 1, and the specific steps include:

[0102] S1. Weigh 5 parts by mass of zinc powder, 1 part by mass of highly branched polyester, and 1 part by mass of polyamide;

[0103] S2, weighing 33 parts by mass of diethylene glycol butyl ether;

[0104] S3, mixing the inorganic additive and dispersant of step S1 with the solvent of step S2, and stirring and dispersing with a dispersing paddle for 30 to 90 minutes;

[0105] S4, homogenizing the stirred slurry by (one or more of ultrasound, ball milling, and homogenization) to obtain a uniform intermediate slurry;

[0106] S5. Weigh 60 parts by mass of an organic carrier, add the organic carrier to the intermediate slurry, and stir and disperse for 30 to 90 minutes to obtain an inorganic slurry.

[0107] Example 6

[0108] The components and contents of the battery slurry in this embodiment are shown in Table 2. The specific steps include:

[0109] 3 parts by mass of the inorganic slurry obtained in Example 1 were uniformly mixed with 85 parts by mass of conductive silver powder, 6 parts by mass of organic carrier, 1.5 parts by mass of aluminum powder, 3.5 parts by mass of glass powder and 1 part by mass of auxiliary agent, and then ground to a slurry fineness of ≤10 μm to obtain N-type battery slurry.

[0110] Furthermore, after the battery paste of this embodiment was printed into a battery cell, the IV battery cell efficiency was tested. According to Table 3, the conversion efficiency was 24.56%.

[0111] Combined Figure 2 It can be seen that a large amount of Ag is precipitated from the battery slurry during the sintering stage, the silver grains increase, and the inorganic additive powder can promote the precipitation of Ag.

[0112] Example 7

[0113] The components and contents of the battery slurry of this embodiment are shown in Table 2, the inorganic slurry is 3.5 parts by mass, the organic carrier is 5.5 parts by mass, the other components and contents are the same as those in Example 6, and the preparation method is also the same as that in Example 6.

[0114] Furthermore, after the battery paste of this embodiment was printed into a battery cell, the IV battery cell efficiency was tested. According to Table 3, the conversion efficiency was 24.63%.

[0115] Combined Figure 2 It can be seen that a large amount of Ag is precipitated from the battery slurry during the sintering stage, the silver grains increase, and the inorganic additive powder can promote the precipitation of Ag.

[0116] Example 8

[0117] The components and contents of the battery slurry in this embodiment are shown in Table 2. The specific steps include:

[0118] 3 parts by mass of the inorganic slurry obtained in Example 2 were uniformly mixed with 85 parts by mass of conductive silver powder, 6 parts by mass of organic carrier, 1.5 parts by mass of aluminum powder, 3.5 parts by mass of glass powder and 1 part by mass of auxiliary agent, and then ground to a slurry fineness of ≤10 μm to obtain N-type battery slurry.

[0119] Furthermore, after the battery paste of this embodiment was printed into a battery cell, the IV battery cell efficiency was tested. According to Table 3, the conversion efficiency was 24.75%.

[0120] Combined Figure 2 It can be seen that a large amount of Ag is precipitated from the battery slurry during the sintering stage, the silver grains increase, and the inorganic additive powder can promote the precipitation of Ag.

[0121] Example 9

[0122] The components and contents of the battery slurry of this embodiment are shown in Table 2, the inorganic slurry is 3.5 parts by mass, the organic carrier is 5.5 parts by mass, and the other components and contents are the same as those in Example 8, and the preparation method is also the same as that in Example 8.

[0123] Furthermore, after the battery paste of this embodiment was printed into a battery cell, the IV battery cell efficiency was tested. According to Table 3, the conversion efficiency was 24.76%.

[0124] Combined Figure 2 It can be seen that a large amount of Ag is precipitated from the battery slurry during the sintering stage, the silver grains increase, and the inorganic additive powder can promote the precipitation of Ag.

[0125] Example 10

[0126] The components and contents of the battery slurry in this embodiment are shown in Table 2. The specific steps include:

[0127] 3 parts by mass of the inorganic slurry obtained in Example 3 were uniformly mixed with 85 parts by mass of conductive silver powder, 6 parts by mass of organic carrier, 1.5 parts by mass of aluminum powder, 3.5 parts by mass of glass powder and 1 part by mass of auxiliary agent, and then ground to a slurry fineness of ≤10 μm to obtain N-type battery slurry.

[0128] Furthermore, after the battery paste of this embodiment was printed into a battery cell, the IV battery cell efficiency was tested. According to Table 3, the conversion efficiency was 24.72%.

[0129] Combined Figure 2 It can be seen that a large amount of Ag is precipitated from the battery slurry during the sintering stage, the silver grains increase, and the inorganic additive powder can promote the precipitation of Ag.

[0130] Embodiment 11

[0131] The components and contents of the battery slurry in this embodiment are shown in Table 2, the inorganic slurry is 3.5 parts by mass, the organic carrier is 5.5 parts by mass, the other components and contents are the same as those in Example 10, and the preparation method is also the same as that in Example 10.

[0132] Furthermore, after the battery paste of this embodiment was printed into a battery cell, the IV battery cell efficiency was tested. According to Table 3, the conversion efficiency was 24.76%.

[0133] Combined Figure 2 It can be seen that a large amount of Ag is precipitated from the battery slurry during the sintering stage, the silver grains increase, and the inorganic additive powder can promote the precipitation of Ag.

[0134] Example 12

[0135] The components and contents of the battery slurry in this embodiment are shown in Table 2. The specific steps include:

[0136] 3 parts by mass of the inorganic slurry obtained in Example 4 were uniformly mixed with 85 parts by mass of conductive silver powder, 6 parts by mass of organic carrier, 1.5 parts by mass of aluminum powder, 3.5 parts by mass of glass powder and 1 part by mass of auxiliary agent, and then ground to a slurry fineness of ≤10 μm to obtain N-type battery slurry.

[0137] Furthermore, after the battery paste of this embodiment was printed into a battery cell, the IV battery cell efficiency was tested. According to Table 3, the conversion efficiency was 24.71%.

[0138] Combined Figure 2 It can be seen that a large amount of Ag is precipitated from the battery slurry during the sintering stage, the silver grains increase, and the inorganic additive powder can promote the precipitation of Ag.

[0139] Embodiment 13

[0140] The components and contents of the battery slurry in this embodiment are shown in Table 2, the inorganic slurry is 3.5 parts by mass, the organic carrier is 5.5 parts by mass, and the other components and contents are the same as those in Example 12, and the preparation method is also the same as that in Example 12.

[0141] Furthermore, after the battery paste of this embodiment was printed into a battery cell, the IV battery cell efficiency was tested. According to Table 3, the conversion efficiency was 24.71%.

[0142] Combined Figure 2 It can be seen that a large amount of Ag is precipitated from the battery slurry during the sintering stage, the silver grains increase, and the inorganic additive powder can promote the precipitation of Ag.

[0143] Embodiment 14

[0144] The components and contents of the battery slurry in this embodiment are shown in Table 2. The specific steps include:

[0145] 3 parts by mass of the inorganic slurry obtained in Example 5 were uniformly mixed with 85 parts by mass of conductive silver powder, 6 parts by mass of organic carrier, 1.5 parts by mass of aluminum powder, 3.5 parts by mass of glass powder and 1 part by mass of auxiliary agent, and then ground to a slurry fineness of ≤10 μm to obtain N-type battery slurry.

[0146] Furthermore, after the battery paste of this embodiment was printed into a battery cell, the IV battery cell efficiency was tested. According to Table 3, the conversion efficiency was 24.76%.

[0147] Combined Figure 2 It can be seen that a large amount of Ag is precipitated from the battery slurry during the sintering stage, the silver grains increase, and the inorganic additive powder can promote the precipitation of Ag.

[0148] Embodiment 15

[0149] The components and contents of the battery slurry in this embodiment are shown in Table 2, the inorganic slurry is 3.5 parts by mass, the organic carrier is 5.5 parts by mass, and the other components and contents are the same as those in Example 14, and the preparation method is also the same as that in Example 14.

[0150] Furthermore, after the battery paste of this embodiment was printed into a battery cell, the efficiency of the IV battery cell was tested. According to Table 3, the conversion efficiency was 24.78%.

[0151] Combined Figure 2 It can be seen that a large amount of Ag is precipitated from the battery slurry during the sintering stage, the silver grains increase, and the inorganic additive powder can promote the precipitation of Ag.

[0152] Comparative Example 1

[0153] The components and contents of the battery slurry in this embodiment are shown in Table 2. The specific steps include:

[0154] 85 parts by mass of conductive silver powder, 9 parts by mass of organic carrier, 1.5 parts by mass of aluminum powder, 3.5 parts by mass of glass powder and 1 part by mass of auxiliary agent were mixed evenly, and then ground to a slurry fineness of ≤10 μm to obtain N-type battery slurry.

[0155] Furthermore, after the battery paste of the comparative example was printed into a battery cell, the IV battery cell efficiency was tested. According to Table 3, the conversion efficiency was 24.45%.

[0156] Comparative Example 2

[0157] The components and contents of the battery slurry of this embodiment are shown in Table 2, the inorganic slurry is 1.5 parts by mass, the organic carrier is 7.5 parts by mass, the other components and contents are the same as those in Example 6, and the preparation method is also the same as that in Example 6.

[0158] Furthermore, after the battery paste of the comparative example was printed into a battery cell, the IV battery cell efficiency was tested. According to Table 3, the conversion efficiency was 24.52%.

[0159] Comparative Example 3

[0160] The components and contents of the battery slurry of this embodiment are shown in Table 2, the inorganic slurry is 5 parts by mass, the organic carrier is 4 parts by mass, the other components and contents are the same as those in Example 6, and the preparation method is also the same as that in Example 6.

[0161] Furthermore, after the battery paste of the comparative example was printed into a battery cell, the IV battery cell efficiency was tested. According to Table 3, the conversion efficiency was 24.54%.

[0162] Comparative Example 4

[0163] The components and contents of the battery slurry of this embodiment are shown in Table 2, the inorganic slurry is 1.5 parts by mass, the organic carrier is 7.5 parts by mass, and the other components and contents are the same as those in Example 8, and the preparation method is also the same as that in Example 8.

[0164] Furthermore, after the battery paste of the comparative example was printed into a battery cell, the IV battery cell efficiency was tested. According to Table 3, the conversion efficiency was 24.65%.

[0165] Comparative Example 5

[0166] The components and contents of the battery slurry of this embodiment are shown in Table 2, the inorganic slurry is 5 parts by mass, the organic carrier is 4 parts by mass, the other components and contents are the same as those in Example 8, and the preparation method is also the same as that in Example 8.

[0167] Furthermore, after the battery paste of the comparative example was printed into a battery cell, the IV battery cell efficiency was tested. According to Table 3, the conversion efficiency was 24.64%.

[0168] Comparative Example 6

[0169] The components and contents of the battery slurry of this embodiment are shown in Table 2, the inorganic slurry is 1.5 parts by mass, the organic carrier is 7.5 parts by mass, the other components and contents are the same as those in Example 10, and the preparation method is also the same as that in Example 10.

[0170] Furthermore, after the battery paste of the comparative example was printed into a battery cell, the IV battery cell efficiency was tested. According to Table 3, the conversion efficiency was 24.69%.

[0171] Comparative Example 7

[0172] The components and contents of the battery slurry of this embodiment are shown in Table 2, the inorganic slurry is 5 parts by mass, the organic carrier is 4 parts by mass, the other components and contents are the same as those in Example 10, and the preparation method is also the same as that in Example 10.

[0173] Furthermore, after the battery paste of the comparative example was printed into a battery cell, the IV battery cell efficiency was tested. According to Table 3, the conversion efficiency was 24.64%.

[0174] Comparative Example 8

[0175] The components and contents of the battery slurry in this embodiment are shown in Table 2, the inorganic slurry is 1.5 parts by mass, the organic carrier is 7.5 parts by mass, and the other components and contents are the same as those in Example 12, and the preparation method is also the same as that in Example 12.

[0176] Furthermore, after the battery paste of the comparative example was printed into a battery cell, the IV battery cell efficiency was tested. According to Table 3, the conversion efficiency was 24.64%.

[0177] Comparative Example 9

[0178] The components and contents of the battery slurry in this embodiment are shown in Table 2, the inorganic slurry is 5 parts by mass, the organic carrier is 4 parts by mass, the other components and contents are the same as those in Example 12, and the preparation method is also the same as that in Example 12.

[0179] Furthermore, after the battery paste of the comparative example was printed into a battery cell, the IV battery cell efficiency was tested. According to Table 3, the conversion efficiency was 24.60%.

[0180] Comparative Example 10

[0181] The components and contents of the battery slurry in this embodiment are shown in Table 2, the inorganic slurry is 1.5 parts by mass, the organic carrier is 7.5 parts by mass, and the other components and contents are the same as those in Example 14, and the preparation method is also the same as that in Example 14.

[0182] Furthermore, after the battery paste of the comparative example was printed into a battery cell, the IV battery cell efficiency was tested. According to Table 3, the conversion efficiency was 24.65%.

[0183] Comparative Example 11

[0184] The components and contents of the battery slurry in this embodiment are shown in Table 2, the inorganic slurry is 5 parts by mass, the organic carrier is 4 parts by mass, and the other components and contents are the same as those in Example 14, and the preparation method is also the same as that in Example 14.

[0185] Furthermore, after the battery paste of the comparative example was printed into a battery cell, the IV battery cell efficiency was tested. According to Table 3, the conversion efficiency was 24.64%.

[0186] According to Table 3, the conversion efficiency of the battery slurry of Comparative Example 1 is 24.45%. Compared with the above embodiments, the conversion efficiency of the battery is lower, which shows that adding the above inorganic additives to the battery slurry can improve the conversion efficiency of the battery. Combining the results of Examples 6-15 and Comparative Examples 2-11, it can be seen that when the amount of inorganic slurry added is 2 to 4 parts by mass, the photoelectric conversion efficiency of the prepared battery is higher. When the amount of inorganic slurry added is less than 2 parts by mass, or greater than 4 parts by mass, the photoelectric conversion efficiency of the battery decreases.

[0187] Combined Figure 2 It can be seen that the battery slurry formed in Examples 6-15 precipitates a large amount of Ag during the sintering stage, the silver grains increase, and the inorganic additive powder can promote the precipitation of Ag. At the same time, the printability of the slurry is also good, and there is no problem of network blocking. Figure 3 It can be seen that during the sintering stage of the battery slurries formed in Comparative Examples 1-11, a large amount of Ag is retained in the glass phase, the precipitated silver grains are significantly reduced, and network blocking occurs.

[0188] Table 1 Components and contents in inorganic slurry of Examples 1-5

[0189]

[0190] Table 2 Components and contents in N-type battery slurries of Examples 6-15 and Comparative Examples 1-11

[0191]

[0192]

[0193] Table 3 Battery conversion efficiency results of Examples 6-15 and Comparative Examples 1-11

[0194] Slurry formula Photoelectric conversion efficiency / % Example 6 24.56 Example 7 24.63 Example 8 24.75 Example 9 24.76 Example 10 24.72 Embodiment 11 24.76 Example 12 24.71 Embodiment 13 24.71 Embodiment 14 24.76 Embodiment 15 24.78 Comparative Example 1 24.45 Comparative Example 2 24.52 Comparative Example 3 24.54 Comparative Example 4 24.65 Comparative Example 5 24.64 Comparative Example 6 24.69 Comparative Example 7 24.64 Comparative Example 8 24.64 Comparative Example 9 24.60 Comparative Example 10 24.65 Comparative Example 11 24.64

[0195] The present invention provides an inorganic slurry, an N-type battery slurry and a preparation method thereof, which have the following beneficial effects: the inorganic functional additive of the present invention can promote the precipitation of silver grains in the intermediate sintering stage of the battery slurry, increase the number of silver grains, and can also control the growth size of the silver grains to improve the ohmic contact between the metal and the semiconductor, reduce metal composite, and help reduce contact resistance and improve the conversion efficiency of solar cells without adding more glass powder. In addition, the preparation method of the present invention can improve the mixing effect of the slurry and increase the dispersibility.

[0196] It is to be understood that the above embodiments are merely exemplary embodiments used to illustrate the principles of the present invention, but the present invention is not limited thereto. For those of ordinary skill in the art, various modifications and improvements can be made without departing from the spirit and essence of the present invention, and these modifications and improvements are also considered to be within the scope of protection of the present invention.

Claims

1. An N-type battery slurry, characterized in that: include: 80-90 parts by mass of conductive silver powder; 4 to 10 parts by weight of an organic carrier; 0.1 to 5 parts by mass of aluminum powder; 1 to 6 parts by mass of glass powder; 0.1 to 2 parts by mass of additives; 2 to 4 parts by mass of an inorganic slurry, wherein: The inorganic slurry comprises: 50 to 90 parts by mass of an organic carrier; 3 to 10 parts by mass of an inorganic additive; the inorganic additive comprises at least one of indium powder, boron powder and zinc powder; the particle size D50 of the inorganic additive is in the range of 0.05 μm to 2 μm; 0.1 to 10 parts by mass of a dispersant; 5 to 40 parts by mass of solvent.

2. The N-type battery slurry according to claim 1, characterized in that: The organic carrier comprises 3 to 5 parts by mass of PVB resin and 5 to 10 parts by mass of acrylic resin.

3. The N-type battery slurry according to claim 1, characterized in that: The dispersant includes at least one of a pigment group copolymer, a highly branched polyester, a fatty acid, a polyamide, and an acid group-containing copolymer.

4. The N-type battery slurry according to claim 1, characterized in that: The solvent includes at least one of diethylene glycol butyl ether, polyoxymethylene dimethyl ether, butyl carbitol, dibutyl phthalate, and diethylene glycol butyl ether acetate.

5. A method for preparing an N-type battery slurry according to any one of claims 1 to 4, characterized in that: The preparation method comprises: obtaining an inorganic slurry; The inorganic slurry is mixed evenly with conductive silver powder, organic carrier, aluminum powder, glass powder and additives, and subjected to grinding and dispersion treatment to obtain N-type battery slurry.

6. The preparation method according to claim 5, characterized in that: The step of obtaining the inorganic slurry comprises: The inorganic additive, dispersant and solvent are mixed, and the mixture is dispersed and homogenized by stirring to obtain an intermediate slurry; Resin is added to the intermediate slurry, and the mixture is stirred and dispersed to obtain an inorganic slurry.

7. The preparation method according to claim 6, characterized in that: The mass ratio of the inorganic additive to the dispersant is in the range of (70-87.5): (12.5-30); The mass ratio of the inorganic additive to the solvent is in the range of (10-40): (60-90); The mass ratio of the intermediate slurry to the organic carrier is in the range of (10-50): (50-90).