A method for purifying Ag from precipitates obtained by washing OLED silver target with hydrochloric acid
The drying, crushing and iron block reduction reaction of the precipitate obtained by rinsing hydrochloric acid of OLED silver target, combined with deionized water and hydrochloric acid to adjust the pH value, solve the problem of high energy consumption, complex process and unenvironmental purified silver in the prior art. The problem is that high-grade, low-energy consumption and environmentally friendly silver purification effect has been achieved.
Patent Information
- Application Number
- CN202310444455.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-23
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-04-23
AI Technical Summary
The prior art method of purified silver has high energy consumption, complex process and is not environmentally friendly, and the hydrazine hydrate used poses a threat to the environment and human health, resulting in low silver grade.
The precipitate obtained by rinsing hydrochloric acid with OLED silver target material is dried, crushed, and reacted with deionized water and iron blocks, adjust the pH value and heated it. The iron blocks are used as reducing agent to achieve silver purification, avoiding the unreacted iron. Contamination of products and adjusting pH and deionized water through low concentration of hydrochloric acid, reducing energy consumption and solvent consumption.
The purification of 99.99 purity silver is achieved, providing an environmentally friendly, low-energy consumption, easy operation and good cost control method, avoiding the use of hydrazine hydrate, and reducing environmental pollution and human body harm.
Smart Images

Figure BDA0004195104020000051 
Figure BDA0004195104020000061 
Figure HDA0004195104030000011
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of hydrometallurgy, and in particular to a method for purifying Ag from a precipitate obtained by washing an OLED silver target with hydrochloric acid. Background Art
[0002] At present, the traditional process of extracting silver from silver chloride is mainly divided into two types: pyrolysis and wet process. Among them, the pyrolysis is to extract silver from silver chloride by adding sodium carbonate. The basic principle of the pyrolysis is: The advantages are simple process and basically no impurities generated. The disadvantages are high energy consumption and the generation of CO 2 It does not conform to the current carbon emission reduction and carbon peak policy; the wet method includes silver chloride plus iron to replace silver, ammonia leaching silver, hydrazine hydrate precipitation to extract silver and silver chloride directly using hydrazine hydrate to extract silver. The principle of silver chloride plus iron powder to replace silver is In order to prevent the iron salt from hydrolyzing to produce hydroxide precipitation and mixing it into silver chloride and silver powder during the reaction, excessive concentrated hydrochloric acid needs to be added. At the same time, if the iron powder does not react fully, it is easy to enter the product and is difficult to separate, resulting in a decrease in the product quality. A refining step is often required. In fact, two steps are required to prepare high-grade silver. In the second step, the crude silver produced in the first step needs to be dissolved with solvents such as nitric acid, filtered, and then reduced with copper. The second step takes a long time and is complicated. The cost of using raw materials copper and nitric acid is high, and there are also serious environmental pollution problems. The principle of ammonia leaching silver and hydrazine hydrate precipitation silver extraction is as follows: Silver chloride is directly extracted with hydrazine hydrate based on the principle of 2AgCl+2N 2 H 4 ·H 2 O→2Ag+N 2 +2NH 4 Cl+2H 2 O, both methods require the use of hydrazine hydrate, which is an explosive and dangerous chemical that can cause harm to the human body through absorption or inhalation of the eyes and skin. In addition, it is highly toxic to aquatic organisms and may cause long-term adverse effects in the aquatic environment. Therefore, there is an urgent need for an environmentally friendly, low-energy, simple-to-operate and high-quality silver extraction method. Summary of the invention
[0003] In order to solve the above technical problems, the purpose of the present invention is to provide a method for purifying Ag from the precipitate obtained by washing OLED silver target with hydrochloric acid, so as to solve the problems of high energy consumption, complex technology, environmental pollution and low grade in the prior art of purifying Ag.
[0004] The technical solution of the present invention to solve the above technical problem is as follows: a method for purifying Ag from a precipitate obtained by washing an OLED silver target with hydrochloric acid is provided, comprising the following steps:
[0005] (1) drying and crushing the precipitate obtained by washing the OLED silver target with hydrochloric acid in sequence to obtain a pretreated raw material;
[0006] (2) The pretreated raw material obtained in step (1) is mixed evenly with deionized water, the pH value is adjusted to 1.5-2.5, heated and stirred, and then an iron block is added. When the solution completely changes from white to gray, the solid phase is collected, washed and dried to obtain Ag.
[0007] On the basis of the above technical solution, the present invention can also be improved as follows:
[0008] Furthermore, in step (1), the drying process is completed by drying at 100-110°C.
[0009] Furthermore, in step (1), the drying process is completed by drying at 105°C.
[0010] Furthermore, in step (1), a vibration ball mill is used to grind the product to a fineness of 280 mesh with a mass fraction of ≥95%.
[0011] Furthermore, in step (2), the mass ratio of the pretreated raw material obtained in step (1) to the deionized water solution is 1:9-11.
[0012] Furthermore, in step (2), the mass ratio of the pretreated raw material obtained in step (1) to the deionized water solution is 1:10.
[0013] Furthermore, in step (2), concentrated hydrochloric acid is used to adjust the pH value to 1.5-2.5.
[0014] Furthermore, in step (2), concentrated hydrochloric acid is used to adjust the pH value to 2.5.
[0015] Furthermore, in step (2), concentrated hydrochloric acid is used to adjust the pH value to 1.5.
[0016] Furthermore, in step (2), the mass ratio of the pretreated raw material to the iron block is 5:1-3.
[0017] Furthermore, in step (2), heating is performed to 25-45°C.
[0018] Furthermore, in step (2), heating is performed to 45°C.
[0019] Furthermore, in step (2), after the iron block is added, the gas generated by the reaction is washed with water and then discharged.
[0020] The present invention also provides Ag prepared by a method for purifying Ag from a precipitate obtained by washing the above-mentioned OLED silver target with hydrochloric acid.
[0021] The present invention has the following beneficial effects:
[0022] 1. The present invention uses the precipitate obtained by washing the OLED silver target with hydrochloric acid as raw material, and prepares 99.99% pure Ag by reduction method, providing an environmentally friendly, low-energy, simple and controllable method for purifying Ag.
[0023] 2. The present invention uses iron blocks as reducing agents, which effectively prevents the unreacted iron from contaminating the product.
[0024] 3. The present invention uses deionized water and then adds hydrochloric acid to adjust the pH. The concentration is low. The solution only needs to add hydrochloric acid to adjust the pH and can be reused. The solvent consumption is small, and the exhaust gas has no pollutants and can be directly discharged. The reaction temperature is 25-45°C, which is basically at room temperature, with low energy consumption and can effectively control costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 The morphology of the pretreated raw material in Example 1;
[0026] Figure 2 The morphology of the product obtained in Example 1;
[0027] Figure 3 The morphology of the product obtained in Example 2;
[0028] Figure 4 The morphology of the product obtained in Example 3;
[0029] Figure 5 The morphology of the product obtained in Example 4;
[0030] Figure 6 The morphology of the product obtained in Example 5;
[0031] Figure 7 The morphology of the product obtained in Example 6;
[0032] Figure 8 The morphology of the product obtained in Example 7;
[0033] Fig. 9 is the element content of the raw material and the product obtained from 1-4;
[0034] Fig.10 It is the element content of the product obtained in Examples 5-7. DETAILED DESCRIPTION
[0035] The principles and features of the present invention are described below in conjunction with the accompanying drawings. The examples are only used to explain the present invention and are not used to limit the scope of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0036] Embodiment 1:
[0037] A method for purifying Ag from a precipitate obtained by washing an OLED silver target with hydrochloric acid, comprising the following steps:
[0038] (1) drying the precipitate obtained by washing the OLED silver target with hydrochloric acid at 105° C., and crushing the precipitate by a vibration ball mill to a fineness of 280 mesh with a mass fraction of 95%, thereby obtaining a pre-treated raw material;
[0039] (2) The pretreated raw material obtained in step (1) and deionized water are mixed uniformly in a mass ratio of 1:10, concentrated hydrochloric acid is added to adjust the pH to 2.5, the mixture is heated to 40°C, and then an iron block is added (the mass ratio of the pretreated raw material to the iron block is 5:2), and the mixture is continuously stirred. The generated gas is washed with water and then discharged. When the solution completely changes from white to gray, the solid phase is collected, washed and dried to obtain Ag.
[0040] Embodiment 2:
[0041] A method for purifying Ag from a precipitate obtained by washing an OLED silver target with hydrochloric acid, comprising the following steps:
[0042] In step (1), concentrated hydrochloric acid is added to adjust the pH to 2, and the rest is the same as in Example 1.
[0043] Embodiment 3:
[0044] A method for purifying Ag from a precipitate obtained by washing an OLED silver target with hydrochloric acid, comprising the following steps:
[0045] In step (1), concentrated hydrochloric acid was added to adjust the pH to 1.5, and the rest was the same as in Example 1.
[0046] Embodiment 4:
[0047] A method for purifying Ag from a precipitate obtained by washing an OLED silver target with hydrochloric acid, comprising the following steps:
[0048] In step (1), concentrated hydrochloric acid is added to adjust the pH to 2, the mass ratio of the pretreated raw material to the iron block is 5:1, and the rest is the same as in Example 1.
[0049] Embodiment 5-7:
[0050] A method for purifying Ag from a precipitate obtained by washing an OLED silver target with hydrochloric acid, comprising the following steps:
[0051] In step (1), concentrated hydrochloric acid is added to adjust the pH to 2. In step (2), the temperature is heated to 30° C., 35° C., and 45° C., respectively. The rest is the same as in Example 1.
[0052] Test example
[0053] 1. The Ag prepared in Examples 1-7 and the pre-treated raw material in Example 1 were subjected to electron microscopy and EDS characterization tests, and the results are shown in Figure 1-10 .
[0054] 2. The Ag prepared in Examples 1-7 and the pre-treated raw material components in Example 1 were tested respectively, and the reaction time and yield were statistically analyzed. The results are shown in Table 1.
[0055] Table 1 Example - Ag composition obtained
[0056]
[0057]
[0058] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for purifying Ag from a precipitate obtained by washing an OLED silver target with hydrochloric acid, characterized in that: The following steps are involved: (1) drying and crushing the precipitate obtained by washing the OLED silver target with hydrochloric acid in sequence to obtain a pretreated raw material; (2) mixing the pretreated raw material obtained in step (1) and deionized water uniformly, adjusting the pH value to 1.5-2.5, heating and stirring, and then adding iron blocks. When the solution completely changes from white to gray, collecting the solid phase, washing and drying, and obtaining Ag; In step (1), the drying process is completed at 100-110° C. In step (1), the product is crushed by a vibration ball mill to a fineness of 280 mesh with a mass fraction of ≥95%; In step (2), concentrated hydrochloric acid is used to adjust the pH value to 1.5-2.5; In step (2), the mass ratio of the pretreated raw material to the iron block is 5:1-3; In step (2), heating to 25-45°C.
2. The method for purifying Ag from the precipitate obtained by washing the OLED silver target with hydrochloric acid according to claim 1, characterized in that: In step (2), the mass ratio of the pretreated raw material obtained in step (1) to the deionized water solution is 1:9-11.
3. The method for purifying Ag from the precipitate obtained by washing the OLED silver target with hydrochloric acid according to claim 1, characterized in that: In step (2), after the iron block is added, the gas generated by the reaction is washed with water and then discharged.
4. Ag obtained by the method of purifying Ag from the precipitate obtained by washing the OLED silver target with hydrochloric acid as described in any one of claims 1 to 3.