A sulfur-modified magnetite-loaded biochar material and its preparation method and application

By introducing Fe3O4 nanoparticles and sulfonic acid functional groups into biochar, sulfur-modified magnetite-loaded biochar material is formed, which solves the problem of removing tetracycline and arsenic in composite polluted water bodies, and achieves efficient and stable water treatment effect , and has the advantages of recycling and mass production.

CN116393089BActive Publication Date: 2024-11-05ZHEJIANG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310123076.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-16
Publication Date
2024-11-05
Estimated Expiration
2043-02-16

AI Technical Summary

Technical Problem

The prior art is difficult to efficiently remove tetracycline and arsenic in composite contaminated water bodies, and the adsorption capacity of biochar is limited, and the loaded iron nanoparticles may block the porous structure, reducing the water treatment efficiency.

Method used

Using sulfur-modified magnetite-loaded biochar material, the specific surface area and stability are improved to achieve efficient removal of tetracycline and arsenic by introducing the dual active sites of Fe3O4 nanoparticles and sulfonic acid-based ones.

Benefits of technology

It achieves efficient removal of tetracycline and arsenic, minimizing the mutual influence of the two, improving water treatment efficiency, and recyclable materials, suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116393089B_ABST
    Figure CN116393089B_ABST
Patent Text Reader

Abstract

The present invention discloses a sulfur-modified magnetite-loaded biochar material and a preparation method and application thereof. The present invention uses rice husk as a biomass material, first obtains raw biochar by oxygen-limited pyrolysis, then ultrasonically dissolves divalent iron salt and trivalent iron salt and uniformly mixes with biochar, then adjusts pH after heating in a water bath until a precipitate is formed, and the generated solid product is further sulfided after washing and drying to obtain a sulfur-modified magnetite-loaded biochar material. The prepared sulfur-modified magnetite-loaded biochar material has uniform magnetite nanoparticles and sulfonic acid group reaction sites, exhibits excellent tetracycline and trivalent arsenic removal performance, and can be applied to the treatment of composite polluted wastewater.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of environmental restoration materials, and in particular relates to a sulfur-modified magnetite-loaded biochar material and a preparation method and application thereof. Background Art

[0002] With the rapid development of industry and agriculture and the increasing material needs of human beings, water pollution has evolved from single pollution to heavy metal and organic compound pollution. Due to the discharge of animal husbandry and aquaculture waste, tetracycline antibiotics and arsenic are detected in water bodies at the same time. Related studies have shown that the presence of tetracycline will reduce the stability of arsenic in solution, and the presence of arsenic will also affect the removal of tetracycline. The interaction between the two will affect the removal efficiency of compound pollutants. Therefore, it is urgent to develop green and efficient compound polluted water remediation technology.

[0003] Among traditional water treatment technologies, adsorption is one of the simple and efficient methods. In recent years, biochar has been widely used as an adsorption material for heavy metals and antibiotics due to its large specific surface area, developed pore structure, and rich oxygen-containing functional groups. However, the adsorption capacity of raw biochar is limited and it is difficult to recycle from water bodies, which limits its practical application potential. At the same time, complex pollutants easily compete for the active sites of biochar, thereby reducing the efficiency of water treatment. In recent years, iron-modified biochar can effectively increase the specific surface area and oxygen-containing functional groups of biochar, but the loaded iron nanoparticles may also occupy the reaction sites of the original biochar and block the porous structure. To solve the above problems, non-metal modification strategies are used to further regulate the surface properties of biochar and introduce rich functional groups. Summary of the invention

[0004] The present invention aims to provide a sulfur-modified magnetite-loaded biochar material and its preparation method and application. The present invention adopts a simple synthesis method to prepare a material with Fe 3 O 4 The nanoparticles with dual active sites of sulfonic acid groups exhibited high stability and the ability to simultaneously remove tetracycline and arsenic.

[0005] The technical solution adopted by the present invention is as follows:

[0006] 1. A Sulfur-Modified Magnetite-Loaded Biochar Material

[0007] The biochar precursor is rice husk biomass, produced in Hangzhou, Zhejiang. The main components of magnetite are Fe 3 O 4 The materials are mainly composed of biochar, Fe 3 O 4 and sulfur-containing groups.

[0008] Fe 3 O4 The size of the nanoparticles is about 20 nm, and the main component of the sulfur-containing groups is sulfonic acid groups.

[0009] 2. A method for preparing sulfur-modified magnetite-loaded biochar material

[0010] The following steps are involved:

[0011] Step 1) The rice husk biomass raw material is rinsed with deionized water to remove residual minerals, then dried and crushed by a high-speed grinder and sieved for later use. A certain amount of biomass is placed in a ceramic crucible, placed in a programmed temperature muffle furnace for oxygen-limited cracking, taken out after cooling, washed with deionized water for multiple times, and dried to obtain biochar;

[0012] Step 2) ultrasonically dissolving the ferrous iron salt and the ferric iron salt and uniformly mixing them with the biochar obtained in step 1), heating them in a water bath and adjusting the pH until a precipitate is formed, and washing the obtained solid product with deionized water until it is neutral and then drying;

[0013] Step 3) The dried product obtained in step 2) is dissolved in sodium hydroxide and tetraaminobenzenesulfonic acid and stirred and heated continuously. After the acid-base reaction is completed, sodium nitrite and hydrochloric acid solution are added in sequence until the grafting reaction is completed. The remaining product is washed to neutrality and then dried to obtain a sulfur-modified magnetite-loaded biochar material.

[0014] In the step 1), the heating rate is 15°C min -1 ; Reaction temperature is 700℃; Drying temperature is 60~80℃; Drying time is 24h; Screen size is 0.15mm.

[0015] In the step 2), the divalent iron salt and the trivalent iron salt are FeSO 4 7H 2 O and FeCl 3 The molar ratio of the two is 1:2; the water bath temperature is 70°C; the reaction time is 1h; the pH when the precipitate is formed is 10-11; after the reaction, wash with deionized water three times or more, and the drying temperature is 80°C.

[0016] In the step 3), the mass ratio of sodium hydroxide to tetraaminobenzenesulfonic acid is 1:8.3; the reaction temperature is 70° C.; the mass of sodium nitrite added is 1.59 g; the concentration of hydrochloric acid is 4 mol / L; the drying temperature is 80° C.; the drying time is 12 h; the medium for washing the remaining product is deionized water and acetone, and the washing times are at least three times.

[0017] 3. Application of Sulfur-modified Magnetite-loaded Biochar Materials

[0018] Sulfur-modified magnetite-loaded biochar materials are used in the treatment of complex polluted wastewater; sulfur-modified magnetite-loaded biochar materials simultaneously remove tetracycline and trivalent arsenic.

[0019] The key to the technical solution of the present invention is to use metal nanoparticles Fe 3 O 4 Simultaneous modification of biochar with non-metallic sulfur, Fe 3 O 4 The specific surface area of ​​biochar is increased, and sulfur modification introduces more functional groups. This metal- and non-metal-based dual-functional modification strategy provides more active sites for biochar, while also enhancing the stability and reactivity of biochar.

[0020] Beneficial effects of the present invention:

[0021] (1) The sulfur-modified magnetite-loaded biochar material provided by the present invention achieves the dual-functional modification purpose of biochar, which not only increases the specific surface area and magnetic properties of biochar, but also introduces oxidative sulfonic acid functional groups, effectively promoting the removal of tetracycline and arsenic.

[0022] (2) The preparation method of the sulfur-modified magnetite-loaded biochar material provided by the present invention is simple, environmentally friendly, and can be synthesized on a large scale.

[0023] (3) The sulfur-modified magnetite-loaded biochar material provided by the present invention can achieve the simultaneous removal of tetracycline and arsenic through a two-step process in a short period of time, and minimize the mutual influence of tetracycline and arsenic, laying the foundation for its application in the field of complex water pollution remediation. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is the XRD pattern of the sulfur-modified magnetite-loaded biochar material prepared in Example 2;

[0025] Figure 2 This is a SEM image of the sulfur-modified magnetite-loaded biochar material prepared in Example 2;

[0026] Figure 3 This is the FTIR image of the sulfur-modified magnetite-loaded biochar material prepared in Example 2;

[0027] Figure 4 This is a hysteresis curve diagram of the sulfur-modified magnetite-loaded biochar material prepared in Example 2;

[0028] Figure 5 The S 2p XPS graphs of sulfur-modified magnetite-loaded biochar materials before and after the reaction;

[0029] Figure 6This is the removal kinetic diagram of tetracycline and sodium arsenite by the sulfur-modified magnetite-loaded biochar material prepared in Example 2. DETAILED DESCRIPTION

[0030] In order to make the purpose, technical scheme and advantages of the present invention more clear, the present invention is further described in detail in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention, rather than to limit the scope of protection of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0031] Unless otherwise defined, the experimental methods and professional terms described in the following examples have the same meanings as those generally understood in the art. The terms used in the present invention are for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0032] Unless otherwise specified, reagents, materials, instruments, etc. used in the present invention can be obtained from commercial sources.

[0033] Example 1

[0034] (1) The rice husk biomass was washed with deionized water for multiple times, dried at 80° C., crushed by a high-speed crusher, and passed through a 0.15 mm sieve for later use;

[0035] (2) A certain amount of biomass was placed in a ceramic crucible, and the crucible was transferred to a programmed temperature muffle furnace. After pyrolysis at 700 °C for 6 hours, the biomass was taken out, washed with deionized water for multiple times, and then dried to obtain rice husk biochar.

[0036] Example 2

[0037] (1) Put FeSO 4 7H 2 O and FeCl 3 Dissolved in 200 mL of deionized water at a molar ratio of 1:2 to obtain solution A;

[0038] (2) Weigh 5 g of biochar and pour it into solution A and ultrasonicate it for 30 min to obtain mixed solution B;

[0039] (3) The mixed solution B was heated in a water bath at 70°C for 1 h, and then 5 mol / L NaOH solution was added dropwise until the pH was 11. The resulting black solid product was centrifuged, washed with deionized water until neutral, and then dried at 80°C to obtain Fe 3 O 4 @BC;

[0040] (4) Weigh 1.0 g Fe 3 O 4@BC, 0.48 g NaOH and 4.0 g tetraaminobenzenesulfonic acid were dissolved in 120 mL deionized water and stirred continuously at 70 °C to obtain a mixed solution C. Then, 1.59 g NaNO 2 Add to solution C, and then add 8 mL of 4 mol / L HCl solution dropwise. After the reaction is completed, the residual solid is washed with deionized water and acetone for several times and then dried at 80°C for 12 h to obtain sulfur-modified magnetite-loaded biochar material.

[0041] Figure 1 Fe prepared in Example 2 3 O 4 @BC and sulfur-modified magnetite-loaded biochar materials. It can be seen from the figure that: Fe 3 O 4 The diffraction peak of Fe 3 O 4 of the crystal structure.

[0042] Figure 2 Fe prepared in Example 2 3 O 4 @BC and SEM images of sulfur-modified magnetite-loaded biochar materials. It can be seen from the figure that: Fe 3 O 4 The nanoparticles are evenly dispersed on the biochar surface, and sulfur modification does not affect Fe 3 O 4 Spherical structure of nanoparticles and porous structure of biochar.

[0043] Figure 3 Fe prepared in Example 2 3 O 4 @BC and FTIR images of sulfur-modified magnetite-loaded biochar materials. It can be seen from the figure that: Fe 3 O 4 @BC contains Fe–OH groups, while sulfur in sulfur-modified magnetite-loaded biochar materials mainly exists in the form of sulfonic acid groups.

[0044] Figure 4 This is the hysteresis curve of the sulfur-modified magnetite-loaded biochar material prepared in Example 2. It can be seen from the figure that the sulfur-modified magnetite-loaded biochar material has strong magnetism and can be quickly separated and recovered under the action of an external magnetic field.

[0045] Figure 5 This is the S 2p XPS graph of the sulfur-modified magnetite-loaded biochar material before and after the reaction. It can be seen from the figure that after the reaction, some sulfonic acid groups are converted into sulfhydryl groups.

[0046] Application Example 1

[0047] Tetracycline and arsenic were used as target pollutants for removal kinetic tests. 0.2 g / L of the sulfur-modified magnetite-loaded biochar material prepared in Example 2 was placed in 22 mL of 1 mg / L and 5 mg / L tetracycline and sodium arsenite solutions (initial pH 5), and oscillated continuously at room temperature for 240 min. 1 mL of sample was extracted with a disposable syringe at regular intervals, filtered, and the concentrations of tetracycline and arsenic were determined using high performance liquid chromatography or hydride generation-atomic fluorescence spectrophotometer. The results are shown in Figure 6 .

[0048] Depend on Figure 6 It can be seen that the sulfur-modified magnetite-loaded biochar material prepared in Example 2 of the present invention can simultaneously remove about 85% of arsenic and tetracycline within 120 minutes at a concentration of 0.2 g / L. The entire removal process includes two stages: adsorption and oxidation. It can be seen that the sulfur-modified magnetite-loaded biochar material prepared in the present invention has a high removal efficiency for tetracycline and arsenic.

[0049] In addition, it should be understood that although this specification is described according to implementation methods, not every implementation method contains only one independent technical solution. This narrative method of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in the embodiments may also be appropriately combined to form other implementation methods that can be understood by those skilled in the art, which all belong to the scope of protection of the present invention.

Claims

1. A method for preparing a sulfur-modified magnetite-loaded biochar material, characterized in that: The sulfur-modified magnetite-loaded biochar material is obtained by modifying biochar with magnetite and sulfur-containing groups; the magnetite includes Fe3O4 nanoparticles with a size of 20 nm; the sulfur-containing groups include sulfonic acid groups; and the biochar precursor is rice husk biomass; The method for preparing the sulfur-modified magnetite-loaded biochar material comprises the following steps: Step 1) The rice husk biomass raw material is rinsed with deionized water to remove residual minerals, and then dried and ground with a high-speed grinder and sieved for later use; The sieved biomass is placed in a ceramic crucible, put into a programmed temperature muffle furnace for oxygen-limited cracking, taken out after cooling, washed with deionized water for multiple times, and then dried to obtain biochar; Step 2) ultrasonically dissolving the divalent iron salt and the trivalent iron salt and uniformly mixing them with the biochar obtained in step 1), heating them in a water bath and adjusting the pH until a precipitate is formed, and washing the obtained solid product with deionized water until it is neutral and then drying; Step 3) dissolving the dried product obtained in step 2) in sodium hydroxide and tetraaminobenzenesulfonic acid and continuously stirring and heating, and after the acid-base reaction is completed, adding sodium nitrite and hydrochloric acid solution in sequence until the grafting reaction is completed; washing the remaining product to neutrality and then drying to obtain a sulfur-modified magnetite-loaded biochar material; Sulfur-modified magnetite-loaded biochar material is used in the treatment of complex polluted wastewater to simultaneously remove tetracycline and trivalent arsenic.

2. The preparation method according to claim 1, characterized in that: In the step 1): The heating rate in the muffle furnace was 15 °C min -1 , the reaction temperature is 700 °C; Drying temperature is 60~80 o C, drying time is 24 h; The mesh size of the sieve is 0.15 mm.

3. The preparation method according to claim 1, characterized in that: In the step 2): The ferrous and ferric salts are FeSO4·7H2O and FeCl3, respectively, with a molar ratio of 1:2; The mass ratio of biochar to total iron salts was 1:

1.

4. The preparation method according to claim 1, characterized in that: In the step 2): The water bath temperature was 70 °C and the reaction time was 1 h; The pH when the precipitate is formed is 10-11; The obtained solid product was washed with deionized water for three times or more and dried at 80 o C.

5. The preparation method according to claim 1, characterized in that: In the step 3): The mass ratio of sodium hydroxide to tetraaminobenzenesulfonic acid is 1:8.3; The mass of sodium nitrite added was 1.59 g and the concentration of hydrochloric acid was 4 mol / L.

6. The preparation method according to claim 1, characterized in that: In the step 3): The reaction temperature of the acid-base reaction is 70 o C; Drying temperature is 80 o C, drying time is 12 h; The remaining product is washed with deionized water and acetone for at least three times.