A method for preparing high mechanical strength carbon particles by activating biomass with sulfuric acid and its application
Through low-temperature hydrolysis and high-temperature pyrolysis of sulfuric acid activated biomass, spherical carbon particles with high mechanical strength and large specific surface area were prepared, which solved the problem of insufficient mechanical strength of biochar materials, applied to microbial electrochemical systems, and improved the production of the system Electrical performance and reduce costs.
Patent Information
- Application Number
- CN202310249243.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-15
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-03-15
AI Technical Summary
The existing biochar materials have insufficient mechanical strength, which is difficult to be stable in wastewater treatment and microbial electrochemical systems, and the preparation process is complex and the cost is high.
The low-temperature hydrolysis of sulfuric acid activated biomass is used to form self-bonded spherical carbon particles. Through low-temperature drying and high-temperature pyrolysis processes, carbon particles with high mechanical strength and large specific surface area are prepared as electrode materials for microbial electrochemical systems.
The preparation of carbon particles with high mechanical strength and low cost is achieved, which improves the stability and performance of carbon particles, enhances the electrical production performance of microbial electrochemical systems, and reduces the cost of preparation and application.
Smart Images

Figure CN116395690B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of biomass, and specifically relates to a method for preparing high mechanical strength carbon particles by activating biomass with sulfuric acid and an application thereof. Background Art
[0002] Biochar is a black solid substance rich in carbon formed by the pyrolysis of various biomass under oxygen-limited conditions. The raw materials for the preparation of biochar are very wide, including coconut shells, reeds, sawdust, agricultural and forestry waste, sludge, etc. Biochar has a large specific surface area and contains a large number of functional groups such as carboxyl, carbonyl, lactone, hydroxyl, and ketone on its surface, which makes biochar have good adsorption, ion exchange and electrochemical activity. In addition, biochar has a low cost and is increasingly receiving widespread attention in the field of environmental remediation. It is used as a water treatment adsorbent and soil remediation improver. However, in general, compared with the activated carbon used in the market, biochar has a relatively low adsorption capacity for pollutants. In addition, due to the low density and small particle size of biochar, it is difficult to separate it from the water body during sewage treatment. After being applied to the soil, it is easy to migrate and infiltrate with water, which may cause secondary environmental pollution, which greatly limits the promotion and application of biochar technology. Therefore, it is very necessary to carry out research on high-density and high-strength molded biochar materials for the promotion and application of biochar.
[0003] In terms of the application of biochar materials, some studies have used biochar materials as electrodes in microbial electrochemical systems. Microbial electrochemical technology can use organic matter in wastewater to convert chemical energy into electrical energy, and has great application potential in water treatment. The high cost of electrode materials is one of the factors that limit its application. Compared with activated carbon, graphite, etc., the cost of biochar is greatly reduced, but the performance of the microbial electrochemical system constructed by biochar electrodes is comparable to that of activated carbon and graphite electrode systems, so biochar has advantages as an electrode material. Carbonizing natural materials such as plants such as kenaf, grapefruit peel, and Xanthium sibiricum as three-dimensional electrode materials, the mechanical strength of natural materials after direct carbonization is insufficient, and they are easy to break, resulting in unstable performance. The preparation process of making biochar into powder and then adding a binder to roll or press it into an electrode is cumbersome. Based on this, the application form of biochar materials in microbial electrochemical systems also needs to be expanded.
[0004] At present, there are three common methods for preparing shaped biochar materials: the first method is to use natural biomass raw materials as precursors and directly carbonize them to obtain shaped biochar; the second method is to first add a binder to extrude the biomass raw materials into shape, and then pyrolyze the shaped raw materials; the third method is to first prepare biochar powder, and then add an organic binder (such as humic acid and its sodium salt, phenolic resin, cellulose-based binder, coal tar pitch and polyvinyl alcohol, etc.) or an inorganic binder (bentonite, montmorillonite, kaolinite and diatomaceous earth, etc.) to extrude them. All three methods have certain limitations: the compressive strength and hardness of the shaped biochar prepared by the first method are very poor; the binder of the second method is easily deactivated under the high temperature (<500℃) of the carbonization or activation process, which makes the compressive strength and density of the final product decrease, and it is easy to break during use; the binder of the third method is directly added to the biochar, which will destroy the pore structure, reduce the specific surface area, and reduce the active adsorption sites. The additional binder also increases the preparation cost of biochar.
[0005] In addition, when biochar is used in water treatment processes such as pollutant adsorption and microbial carrier, the mechanical strength, specific surface area, and content of surface active sites (including pore size, edge defects, topological defects, and surface functional groups) of the material directly affect the cost performance of the material. Therefore, in the process of material preparation, it is very meaningful to study how to effectively prepare biochar particles with high specific surface area, high mechanical properties, and low cost. Summary of the invention
[0006] The present invention relates to a method for preparing high mechanical strength biochar particles using biomass precursors and its application, and specifically to a method for forming self-bonding shaped carbon particles by hydrolyzing waste biomass with sulfuric acid activation, and its application in electrode materials of microbial electrochemical systems. The technical solution of the present invention is as follows:
[0007] A method for preparing high mechanical strength carbon particles by activating biomass with sulfuric acid comprises the following steps:
[0008] (1) crushing clean and dry biomass to obtain biomass powder, adding sulfuric acid and stirring evenly, and activating to obtain slurry;
[0009] (2) placing the slurry into a strip making machine to make strips, then rolling them into spherical particles, and then drying them at low temperature to achieve surface hardening;
[0010] (3) In an inert gas atmosphere, the surface-hardened spherical particles are placed in a tubular furnace for pyrolysis after heating, and then cooled to room temperature, washed, and dried to obtain carbon particles with high mechanical strength.
[0011] Preferably, the biomass includes industrial by-products, agricultural wastes and urban wastes containing lignin, cellulose and hemicellulose, such as one or more of sludge, rice husks, straw, wood scraps, bamboo chips, leaves and the like.
[0012] Preferably, in step (1), the mass ratio of sulfuric acid volume to biomass powder is (2-4):1 in ml / g.
[0013] Preferably, in step (1), the mass fraction of sulfuric acid is 30-65%. If the mass fraction or volume of sulfuric acid is too small, the purpose of activating biomass to dehydrate and hydrolyze to produce sticky substances cannot be achieved. On the contrary, if the amount of sulfuric acid is too much, the yield of spherical carbon particles will be greatly reduced.
[0014] Preferably, in step (1), the activation temperature is 80-120° C. and the activation time is 1-2 h.
[0015] Preferably, in step (2), the drying temperature is 50-70° C. and the drying time is 7-12 hours to prevent the spherical particles from sticking to the surface due to softening.
[0016] Preferably, in step (3), the heating rate is 1-5°C / min, the pyrolysis temperature is 400-1000°C, and the pyrolysis time is 0.5-5h. If the heating rate is too fast, the carbon particles will break and cannot maintain a spherical shape; the higher the pyrolysis temperature, the higher the carbonization degree, specific surface area, carbon content, and electrical conductivity of the particles, and the mechanical strength will also be affected.
[0017] The invention also provides carbon particles with high mechanical strength prepared by the preparation method.
[0018] The present invention also provides application of high mechanical strength carbon particles prepared by the preparation method in a microbial electrochemical system.
[0019] The present invention also provides a microbial electrochemical system, in which the high mechanical strength carbon particles prepared by the preparation method are wrapped with a current collector as an anode electrode.
[0020] Preferably, the microbial electrochemical system uses a titanium mesh or a stainless steel mesh as the anode current collector.
[0021] When the system is operated in batch mode, the carbon particles are in good contact with the electrolyte and are not limited by mass transfer, which can better test the performance of the carbon particles as anode.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] 1. After being activated by sulfuric acid with a high mass fraction, biomass can be hydrolyzed to produce a sticky substance, which can be self-adhesive and formed without adding additional binders. The prepared spherical carbon particles have high compressive strength, stable performance, and reduced production costs.
[0024] 2. The present invention first activates at low temperature and then pyrolyzes at high temperature, ensuring that the biomass raw material first reacts with sulfuric acid to produce a viscous substance, and then pyrolyzes at high temperature to form spherical carbon particles, so as to prevent the high-temperature pyrolysis from directly generating carbon powder. During this period, the heating rate of the carbon pyrolysis process is adjusted to ensure that the carbon pyrolysis proceeds slowly, so as to ensure that the carbon particles are stably formed, and the carbon pyrolysis temperature and pyrolysis time are regulated to increase the yield of biomass components converted into fixed carbon, and at the same time adjust the pore structure distribution to obtain carbon particles with high mechanical strength and high specific surface area.
[0025] 3. The shaped carbon particles with a certain strength (compressive strength of about 1.03±0.24 to 2.58±0.62MPa) prepared by the present invention are not only easy to transport, but also not easily affected by external forces such as mechanical stirring during the actual process of addition, not easy to break, and easy to recycle.
[0026] 4. The three-dimensional carbon particles with high specific surface area prepared by the present invention (particle size of about 2 to 15 mm, specific surface area of about 580 to 1713 m 2 / g) provides sufficient active sites for the attachment of functional microorganisms, and good conductivity ensures the power generation performance of the microbial electrochemical system. The maximum output power of the microbial electrochemical system constructed with the carbon particles as electrode materials can reach about 883-2067 mW / cm 2 . BRIEF DESCRIPTION OF THE DRAWINGS
[0027] The accompanying drawings, which are incorporated in and constitute a part of the specification, illustrate embodiments consistent with the present invention and, together with the description, serve to explain the principles of the present invention, in which:
[0028] Figure 1 Stress-strain curves in compression tests of carbon particles;
[0029] Figure 2 The power generation performance of the microbial electrochemical system constructed with the bioanode of the net bag carbon particles. DETAILED DESCRIPTION
[0030] The disclosure below provides many different embodiments or examples to implement different structures of the present invention. In order to simplify the disclosure of the present invention, the parts and settings of specific examples are described below. Of course, they are only examples, and the purpose is not to limit the present invention. In addition, the present invention can repeat reference numbers and / or reference letters in different examples, and this repetition is for the purpose of simplification and clarity, which itself does not indicate the relationship between the various embodiments and / or settings discussed.
[0031] The present invention uses sulfuric acid to activate biomass for low-temperature hydrolysis and degradation, forming a system in which a binder, a plasticizer and an antioxidant act together, so as to promote the self-bonding molding of the raw materials of biomass powder without adding any additional adhesive substances, and then obtains spherical granular biochar with high mechanical strength through pyrolysis under inert gas lower limit oxygen. The obtained carbon particles have high conductivity, large surface area and good biocompatibility, and can be used as water treatment adsorbents or microbial carrier fillers. Using them as electrode materials for microbial electrochemical systems can also achieve the enrichment of functional microorganisms, resulting in good electricity generation performance.
[0032] Embodiment 1:
[0033] In this embodiment, corn cobs were used as biomass raw materials, carbon particles were prepared according to the preparation method of the present invention, and the carbon particles were used as anode materials of the microbial electrochemical system to achieve stable electrical energy output.
[0034] 1) crushing the dried corncobs into 80 mesh corncob powder;
[0035] 2) Weigh 50 g corncob powder into a beaker, then add 150 mL of 35% sulfuric acid, stir and mix well, then place in an oven at 120° C. for 2 h to obtain a black slurry;
[0036] 3) Put the black slurry into a strip making machine, make it into long strips, put it on a pill rolling board, and roll it into spherical particles with a diameter of 8 mm;
[0037] 4) placing the spherical particles in an oven at 65°C overnight to harden their surface;
[0038] 5) Take the spherical particles out of the oven, put them in a crucible, and heat them to 900°C at a rate of 3°C / min in a tube furnace under argon atmosphere, and pyrolyze them at 900°C for 2h;
[0039] 6) After the pyrolysis is completed, the mixture is naturally cooled to room temperature, the spherical carbon particles are washed with deionized water, soaked in anhydrous ethanol, ultrasonicated in deionized water for 30 minutes, and dried in an oven to finally obtain spherical carbon particles with a diameter of about 3 mm.
[0040] 7) Using a 10-mesh titanium mesh to make a net bag, filling the carbon particles prepared above into the net bag to form a net bag particle anode with a projected area of about 2 cm×2 cm, and using titanium wire to extract electrons;
[0041] 8) Double-chamber cubic microbial electrochemical system, the inner dimensions of the anode are 4cm×4cm×2cm, the electrode material is a net bag particle anode, the inner dimensions of the cathode are 4cm×4cm×4cm, the cathode electrode is a carbon fiber brush with a diameter of 3cm and a length of 3cm, and the cathode and anode are separated by a cation exchange membrane. The anode is inoculated with domestic sewage, the anode liquid is artificial water, the substrate is 1g / L sodium acetate, added to 50mM phosphate buffer (Na2HPO4·12H2O: 13.32g / L; NaH2PHO4·2H2O: 3.36g / L; NH4Cl: 0.31g / L; KCl: 0.13g / L), and vitamin and trace element solutions are added, and the cathode liquid is 50mM potassium ferrocyanide and 50mM phosphate buffer.
[0042] 9) The compressive strength of carbon particles (BC900) obtained by pyrolysis at 900°C is as follows Figure 1 The surface area is 1712.8m 2 / g, the maximum output power of the microbial electrochemical system constructed using the particles as electrode materials is as follows Figure 2 As shown, it reaches 2066.7mW / cm 2 .
[0043] Embodiment 2:
[0044] The present embodiment is different from Example 1 in that: in step (5), the temperature is raised to 800°C at a rate of 3°C / min in an argon atmosphere in a tube furnace, and pyrolysis is performed at 800°C for 2h. The rest is the same as Example 1. The compressive strength of the carbon particles (BC800) obtained by pyrolysis at 800°C is 1.93±0.49MPa, and the specific surface area is 928.8m 2 / g, and the maximum output power of the microbial electrochemical system constructed using the particles as electrode materials reached 1624.8mW / cm 2 .
[0045] Embodiment 3:
[0046] The present embodiment is different from Example 1 in that: in step (5), the temperature is raised to 700°C at a rate of 3°C / min in an argon atmosphere in a tube furnace, and pyrolysis is performed at 700°C for 2 hours. The rest is the same as Example 1. The compressive strength of the carbon particles (BC700) obtained by pyrolysis at 700°C is 2.58±0.62MPa, and the specific surface area is 580.7m 2 / g, and the maximum output power of the microbial electrochemical system constructed using the particles as electrode materials reached 883.6mW / cm 2 .
[0047] Embodiment 4:
[0048] The present embodiment is different from Example 1 in that the biomass raw material used in steps (1) and (2) is corn stalks, and in step (5), the temperature is raised to 500°C at a rate of 3°C / min in an argon atmosphere in a tube furnace, and pyrolyzed at 500°C for 2h. The rest is the same as Example 1. The compressive strength of the carbon particles (BC500) obtained by pyrolysis at 500°C is 1.55±0.37MPa.
[0049] Embodiment 5:
[0050] The present embodiment is different from Example 1 in that in step (5), the temperature is raised to 400°C at a rate of 3°C / min in an argon atmosphere in a tube furnace, and pyrolysis is performed at 400°C for 2 hours. The rest is the same as Example 1. The compressive strength of the carbon particles (BC400) obtained by pyrolysis at 400°C is 1.35±0.27MPa.
[0051] Embodiment 6:
[0052] The present embodiment is different from Example 1 in that: in step (5), the temperature is raised to 600°C at a rate of 3°C / min in an argon atmosphere in a tube furnace, and pyrolysis is performed at 600°C for 2h. The rest is the same as Example 1. The compressive strength of the carbon particles (BC600) obtained by pyrolysis at 600°C is 2.14±0.77MPa.
[0053] Principle of the present invention:
[0054] The main components of biomass include lignin, cellulose and hemicellulose. After the biomass raw materials are impregnated with sulfuric acid, the dehydration and hydrolysis of high-polysaccharides such as hemicellulose and cellulose are promoted, and the aromatic groups of lignin are promoted to break. During the pyrolysis process, viscous substances such as tar, oligosaccharides or polycyclic aromatic hydrocarbons are produced in situ. Through diffusion, polycondensation, cross-linking and curing, a system of binders, plasticizers and antioxidants is formed, which promotes the self-forming of raw materials without adding additional adhesive substances. At the same time, during the pyrolysis process, the carbon aromatic ring forms graphite-like microcrystals and carbon skeleton structures, and the release of various volatile substances and gases can create more pore structures and increase porosity.
[0055] Application of the above spherical carbon particles as electrode materials in microbial electrochemical systems:
[0056] (1) The carbon particles prepared by the present invention have good stability in water and a compressive strength of 1.03±0.24 to 2.58±0.62 MPa.
[0057] (2) The carbon particle anode uses titanium mesh as an electron collector. The prepared carbon particles are accumulated in a mesh bag made of titanium mesh, and the electrons are conducted out through titanium wire.
[0058] (3) Domestic sewage is used as a bacterial source to inoculate the anode. After the system is successfully started, the carbon particle bioanode degrades the organic matter in the anode liquid and simultaneously conducts the generated electrons through an external circuit, thereby generating current.
[0059] (4) Carbon particles have a large surface area and can adsorb pollutants in water. As microbial carriers, carbon particles provide sufficient sites for microbial attachment. As electrode materials, carbon particles receive electrons transferred to the extracellular space by electroactive microorganisms and then conduct them to the external circuit. The microbial electrochemical system constructed by carbon particle electrodes can achieve the degradation of organic matter in water and generate electricity.
[0060] Those skilled in the art will readily appreciate other embodiments of the invention after considering the specification and practicing the invention herein. The invention is intended to cover any variations, uses or adaptations of the invention that follow the general principles of the invention and include common knowledge or customary techniques in the art of the invention. The specification and examples are to be considered exemplary only, and the true scope and spirit of the invention are indicated by the claims.
[0061] It should be understood that the present invention is not limited to the exact construction that has been described above and shown in the drawings and that various modifications and changes may be made without departing from the scope thereof. The scope of the present invention is limited only by the appended claims.
Claims
1. A method for preparing high mechanical strength carbon particles by activating biomass with sulfuric acid, characterized in that: The following steps are involved: (1) crushing clean and dry biomass to obtain biomass powder, adding sulfuric acid and stirring evenly, and activating to obtain slurry; The activation temperature is 80-120°C, and the activation time is 1-2h; (2) placing the slurry into a strip making machine to make strips, then rolling them into spherical particles, and then drying them at low temperature to achieve surface hardening; The drying temperature is 50-70°C, and the drying time is 7-12h; (3) In an inert gas atmosphere, the surface-hardened spherical particles are placed in a tubular furnace for pyrolysis after heating, and then cooled to room temperature, washed, and dried to obtain the high mechanical strength carbon particles.
2. The method for preparing high mechanical strength carbon particles by activating biomass with sulfuric acid according to claim 1, characterized in that: In step (1), the volume ratio of the sulfuric acid to the mass ratio of the biomass powder is (2-4):1 in ml / g.
3. The method for preparing high mechanical strength carbon particles by activating biomass with sulfuric acid according to claim 1, characterized in that: In step (1), the mass fraction of the sulfuric acid is 30-65%.
4. The method for preparing high mechanical strength carbon particles by activating biomass with sulfuric acid according to claim 1, characterized in that: In step (3), the heating rate is 1-5°C / min, the pyrolysis temperature is 400-1000°C, and the pyrolysis time is 0.5-5h.
5. Carbon particles with high mechanical strength prepared by the method according to any one of claims 1 to 4.
6. Use of high mechanical strength carbon particles prepared by the method according to any one of claims 1 to 4 in a microbial electrochemical system.
7. A microbial electrochemical system, characterized in that: The high mechanical strength carbon particles prepared by the method described in any one of claims 1 to 4 are wrapped with a current collector as an anode electrode.
8. The microbial electrochemical system according to claim 7, characterized in that: The microbial electrochemical system uses a titanium mesh or a stainless steel mesh as an anode current collector.