Glass ceramic mold and preparation method thereof
By adopting the design and preparation process of glass ceramic molds, the problems of high thermal expansion, poor oxidation resistance and insufficient thermal shock resistance of existing thermal bending mold materials are solved, and efficient and low-cost 3D glass mass production is achieved, which has expanded the The scope of application of the mold and the accuracy and flatness of the blank after hot bending.
Patent Information
- Application Number
- CN202111679663.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-31
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2041-12-31
AI Technical Summary
Existing thermal bending mold materials, such as metals and graphite, have problems such as high thermal expansion, poor oxidation resistance, and insufficient thermal shock resistance, resulting in low yield, low efficiency, high cost of mass production of 3D glass, and a narrow range of thermal expansion coefficient. , the scope of application is limited.
The glass ceramic mold is used, and its main crystal phase includes β-quartz, β-spentazole and β-lithiumite. Combined with MgAl2Si3O10, MgAl2O4, ZnAl2O4 and other components, the thermal expansion coefficient is controlled to be -1.0×10-6~3.0×10-5 Within the range of /K, the thermal conductivity is greater than or equal to 1W/(m·k), and through specific preparation processes such as mixing, melting, forming, microcrystalization and annealing, it is prepared with high thermal conductivity, high temperature resistance, A mold that resists heat shock.
It realizes the high thermal conductivity, high temperature resistance and high thermal shock resistance of the mold, extends the service life, has a wide range of application, significantly improves the yield and efficiency of mass production of 3D glass, reduces costs, and avoids the blank after thermal bending. dimensional accuracy and roughness improvement.
Smart Images

Figure CN116409936B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of forming and processing mold preparation, and in particular to a glass ceramic mold and a preparation method thereof. Background Art
[0002] Heat-bent glass is made by heating and softening a flat glass blank, forming it in a mold, and then annealing it to make a curved glass. During the heat bending process, the glass needs to be heated and force-transmitted by the mold without affecting the accuracy and characteristics of the glass. Therefore, the material of the mold needs to have the characteristics of easy processing, high thermal conductivity, high temperature resistance, low expansion, high softening point and high thermal shock resistance.
[0003] Most traditional hot bending molds are made of metal and graphite. Metal materials are easily deformed at high temperatures, have a long heat transfer time, and have high thermal expansion, which may cause defects or dimensional deviations in the glass after hot bending. Graphite molds have poor oxidation resistance and are easily oxidized at high temperatures, resulting in a shortened mold life and increased costs. They also have poor thermal shock resistance and are not suitable for long-term use, which can easily lead to deviations in the dimensional accuracy of the blanks. Due to the characteristics of metal molds and graphite molds, the yield rate of mass production of 3D glass is currently very low, the efficiency is very low, and the cost is very high.
[0004] In order to achieve low-cost, high-yield, and high-efficiency mass production of 3D glass, technicians are working hard to find a hot bending mold with excellent performance. In the communication with experts in the glass forming mold industry, it was found that they ruled out the use of glass or glass ceramic materials as glass forming molds. Because of the many complex physical, chemical, and mechanical processes that occur in hot glass forming and the final product, the demanding requirements for mold materials are difficult to meet with existing glass or glass ceramic materials. Stringent requirements include: easy machining, resistance to cracking; heat resistance and wear resistance; good thermal conductivity; small thermal expansion coefficient; dense and uniform; high adhesion temperature; good surface finish of the molding, etc.
[0005] Moreover, existing hot bending molds often have the problem of a narrow range of thermal expansion coefficients under the condition of meeting low expansion properties, which limits their scope of application. Summary of the invention
[0006] (I) Purpose of application
[0007] Based on this, in order to realize the application of glass-ceramic materials in the field of hot bending molds, make the glass-ceramic molds meet the requirements of hot bending molds, improve the service life of hot bending molds, and expand the application scope of hot bending molds, this application discloses the following technical solutions.
[0008] (II) Technical solution
[0009] The present application discloses a glass-ceramic mold, wherein the main crystalline phase of the glass-ceramic mold includes one or more of β-quartz, β-spodumene and β-eucryptite, and the mass fraction of the β-quartz + the mass fraction of the β-spodumene + the mass fraction of the β-eucryptite is in the range of 0.1% to 70.0%.
[0010] In a possible implementation manner, the main crystalline phase further includes MgAl2Si3O 10 , MgAl2O4, ZnAl2O4 and mullite.
[0011] In a possible implementation, the thermal expansion coefficient of the glass-ceramic mold is -1.0×10 -6 ~3.0×10 -5 / K.
[0012] In a possible implementation manner, the glass-ceramic mold comprises Li2O in a mass fraction range of 0.50% to 10.00%.
[0013] In a possible implementation, the components of the glass-ceramic mold further include Na2O and K2O, the mass ratio of Na2O, K2O and Li2O is required to be as follows: (Na2O+K2O) / Li2O<1.00, and the total mass fraction of Na2O and K2O is ≤8.00%.
[0014] In a possible embodiment, the following raw materials are included in weight portions: SiO2: 40.00-80.00 parts; Al2O3: 18.00-40.00 parts; ZrO2: 0.50-10.00 parts; Li2O: 0.50-10.00 parts; Na2O: 0.00-2.00 parts; B2O3: 0.00-5.00 parts; K2O: 0.00-5.00 parts; MgO: 0.00-20.00 parts; CaO: 0.00-5.00 parts; P2O5: 0.00-5.00 parts; TiO2: 0.00-5.00 parts; BaO: 0.00-2.00 parts; ZnO: 0.00-10.00 parts.
[0015] In a possible implementation manner, the glass transition temperature of the glass-ceramic mold is greater than or equal to 700°C.
[0016] In a possible implementation, the thermal conductivity of the glass-ceramic mold is greater than or equal to 1 W / (m·K) within a temperature range of 25 to 1000° C.
[0017] As a second aspect of the present application, the present application also discloses a method for preparing a glass ceramic mold, which is characterized by comprising the following steps:
[0018] In the mixing process, each raw material is weighed and mixed evenly to prepare a basic mixture, wherein each raw material includes the following parts by weight:
[0019] SiO2: 40.00-80.00 parts; Al2O3: 18.00-40.00 parts; ZrO2: 0.50-10.00 parts; Li2O: 0.50-10.00 parts; Na2O: 0.00-2.00 parts; B2O3: 0.00-5.00 parts; K2O: 0.00-5.00 parts; MgO: 0.00-20.00 parts; CaO: 0.00-5.00 parts; P2O5: 0.00-5.00 parts; TiO2: 0.00-5.00 parts; BaO: 0.00-2.00 parts; ZnO: 0.00-10.00 parts;
[0020] A melting step, melting the basic mixture and pouring it into a mold to form a basic glass piece;
[0021] A molding process, in which the basic glass piece is made into a glass mold piece of a desired shape;
[0022] A microcrystallization treatment step, wherein the glass mold piece is subjected to nucleation and crystallization treatments in sequence to form the microcrystallized mold piece;
[0023] The cooling step is to cool the microcrystallized mold to room temperature to form a glass ceramic mold.
[0024] In a possible implementation manner, the melting temperature is 1500-1700° C., and the melting time is 3-16 hours.
[0025] In a possible implementation manner, the nucleation temperature is 650-1000° C., and the nucleation time is 1-6 hours; the crystallization temperature is 900-1400° C., and the crystallization time is 0-15 hours.
[0026] In a possible implementation, the molding process is hot bending molding, and the microcrystallization treatment process and the hot bending molding are performed simultaneously.
[0027] In a possible implementation, the forming process is cold carving.
[0028] In a possible implementation, an annealing process is further included before the cold carving process, and the annealing process is to anneal the basic glass piece and cool it to room temperature.
[0029] In a possible implementation manner, the annealing temperature in the annealing process is 600-900° C., the annealing time is 30-1200 hours, and the material is cooled to room temperature at a cooling rate of 5-20° C. / h.
[0030] In a possible implementation manner, the cooling rate in the cooling step is 5 to 40° C. / h.
[0031] In a possible implementation manner, after the cooling process, a polishing process of the glass-ceramic mold is further included.
[0032] (III) Beneficial effects
[0033] The glass ceramic mold provided by the present application has the advantages of high thermal conductivity, high temperature resistance, high softening point and high thermal shock resistance, excellent resistance to cracking, long service life, easy machining, and can meet the demanding use requirements of hot bending molds. At the same time, the glass ceramic mold of the present application has a wide adjustable thermal expansion coefficient range while meeting the requirements of the low thermal expansion coefficient of the mold, and has a wide application range, which greatly improves the applicability of the hot bending mold. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain and illustrate the present application, but should not be construed as limiting the scope of protection of the present application.
[0035] Figure 1 It is a schematic flow chart of the method for preparing a glass ceramic mold disclosed in the present application. DETAILED DESCRIPTION
[0036] In order to make the purpose, technical solutions and advantages of the implementation of this application clearer, the technical solutions in the embodiments of this application are described in more detail below.
[0037] The present application provides a glass-ceramic mold, wherein the main crystal phase of the glass-ceramic mold includes one or more of β-quartz, β-spodumene and β-eucryptite, and the mass fraction of the β-quartz + the mass fraction of the β-spodumene + the mass fraction of the β-eucryptite is in the range of 0.1% to 70.0%.
[0038] In one embodiment, the main crystalline phase further comprises MgAl2Si3O 10 , one or more of MgAl2O4 (magnesium spinel), ZnAl2O4 (zinc spinel) and mullite.
[0039] Specifically, a X-ray diffractometer was used with the instrument settings of 40 mV voltage, 30 mA current, 10-50° test range, 1° / min scan speed, and 0.02° / step step. The X-ray diffraction data after detection were analyzed to confirm the proportion of each crystalline phase.
[0040] The glass-ceramic mold includes the following raw materials in parts by weight: SiO2: 40.00-80.00 parts; Al2O3: 18.00-40.00 parts; ZrO2: 0.50-10.00 parts; Li2O: 0.50-10.00 parts; Na2O: 0.00-2.00 parts; B2O3: 0.00-5.00 parts; K2O: 0.00-5.00 parts; MgO: 0.00-20.00 parts; CaO: 0.00-5.00 parts; P2O5: 0.00-5.00 parts; TiO2: 0.00-5.00 parts; BaO: 0.00-2.00 parts; ZnO: 0.00-10.00 parts.
[0041] The functions of the raw materials of the glass ceramic mold provided in this application are as follows:
[0042] The addition of Li2O will accelerate the precipitation of β-quartz, β-quartz solid solution crystals, β-spodumene and β-eucryptite with low thermal expansion coefficients, significantly reducing the thermal expansion coefficient of glass ceramics. It is also possible to control the mass fraction of β-quartz, β-spodumene and β-eucryptite with negative expansion coefficients in the glass ceramic mold after the base glass is crystallized. However, too much lithium will lead to the transformation of the precipitated crystal phase, which will increase the thermal expansion coefficient of the glass ceramic. Controlling the mass fraction of Li2O to 0.50% to 10.00% is convenient for controlling the glass ceramic mold to obtain a suitable range of thermal expansion coefficients.
[0043] In some embodiments, the mass fraction of Li2O includes 0.50 wt% to 10.00 wt% and all ranges and sub-ranges therebetween, such as 0.50 wt%-7.50 wt%, 0.50 wt%-5.00 wt%, 0.50 wt%-2.50 wt%, 2.00 wt%-10.00 wt%, 2.00 wt%-7.50 wt%, 2.00 wt%-5.00 wt%, 5.00 wt%-10.00 wt%, 5.00 wt%-7.50 wt%, 7.50 wt%-10.00 wt%, etc. In some embodiments, the content of Li2O can be controlled at 0.00 wt%, 0.50 wt%, 1.00 wt%, 2.00 wt%, 3.00 wt%, 4.00 wt%, 5.00 wt%, 6.00 wt%, 7.00 wt%, 8.00 wt%, 9.00 wt%, 10.00 wt%, etc.
[0044] The addition of Na2O and K2O can reduce the upper crystallization temperature of microcrystalline glass, thereby reducing the production and molding difficulty of base glass (uncrystallized glass, referred to as base glass). Na and K are generally enriched in the glass phase after the base glass is crystallized. Excessive Na2O and K2O will significantly increase the thermal expansion coefficient and reduce the glass transition temperature of glass ceramics. In order to control the thermal expansion coefficient and reduce the glass transition temperature of glass ceramics, the content of Na2O and K2O is controlled. It is necessary to control the mass ratio of Na2O, K2O and Li2O to meet the following requirements: (Na2O+K2O) / Li2O<1.00, and the total mass fraction of Na2O and K2O ≤8.00%.
[0045] In some embodiments, the mass fraction of Na2O includes 0.00 wt% to 2.00 wt% and all ranges and sub-ranges therebetween, such as 0.25 wt%-2.00 wt%, 0.25 wt%-1.50 wt%, 0.25 wt%-1.00 wt%, 1.00 wt%-2.00 wt%, 1.00 wt%-1.50 wt%, etc. In some embodiments, the content of Na2O can be controlled at 0.00 wt%, 0.25 wt%, 1.00 wt%, 1.25 wt%, 1.50 wt%, 1.75 wt%, 2.00 wt%, etc.
[0046] In some embodiments, the mass fraction of K2O includes 0.00 wt% to 5.00 wt% and all ranges and sub-ranges therebetween, for example, it can be controlled at 0.80 wt%-5.00 wt%, 0.80 wt%-4.00 wt%, 0.80 wt%-3.00 wt%, 0.80 wt%-2.00 wt%, 0.80 wt%-1.00 wt%, 1.00 wt%-5.00 wt%, 2.00 wt%-5.00 wt%, 3.00 wt%-5.00 wt%, 4.00 wt%-5.00 wt%, 2.00 wt%-4.00 wt%, 2.00 wt%-3.00 wt%, etc. In some embodiments, the content of K2O can be controlled at 0.00 wt%, 0.80 wt%, 1.00 wt%, 1.50 wt%, 2.00 wt%, 2.50 wt%, 3.00 wt%, 3.50 wt%, 4.00 wt%, 4.50 wt%, 5.00 wt%, etc.
[0047] The addition of B2O3 can reduce the thermal expansion coefficient of the glass phase in glass ceramics (glass ceramics contain glass phase and crystal phase), but too much B2O3 will reduce the strength of glass ceramics.
[0048] In some embodiments, the mass fraction of B2O3 includes 0.00 wt% to 5.00 wt% and all ranges and sub-ranges therebetween, such as 0.75 wt%-5.00 wt%, 0.75 wt%-4.00 wt%, 0.75 wt%-3.00 wt%, 0.75 wt%-2.00 wt%, 0.75 wt%-1.00 wt%, 1.00 wt%-5.00 wt%, 2.00 wt%-5.00 wt%, 3.00 wt%-5.00 wt%, 4.00 wt%-5.00 wt%, 2.00 wt%-4.00 wt%, 2.00 wt%-3.00 wt%, etc. In some embodiments, the mass fraction of B2O3 can be controlled at 0.00 wt%, 0.50 wt%, 0.75 wt%, 1.00 wt%, 1.50 wt%, 2.00 wt%, 2.50 wt%, 3.00 wt%, 3.50 wt%, 4.00 wt%, 4.50 wt%, 5.00 wt%, etc.
[0049] MgO and ZnO participate in the glass ceramic MgAl2Si3O 10 , the formation of magnesium-containing crystals such as ZnAl2O4, MgAl2O4, mullite, cordierite, β-quartz, β-quartz solid solution, β-spodumene and β-eucryptite.
[0050] In some embodiments, the mass fraction of MgO includes 0.00 wt% to 20.00 wt% and all ranges and sub-ranges therebetween, for example, it can be controlled within the range of 0.00 wt%-19.00 wt%, 0.00 wt%-18.70 wt%, 0.00 wt%-16.00 wt%, 0.00 wt%-14.00 wt%, 0.00 wt%-13.30 wt%, 0.00 wt%-11.00 wt%, 0.00 wt%-9.00 wt%, 10.00 wt%-20.00 wt%, 13.30 wt%-20.00 wt%, 15.00 wt%-20.00 wt%, 17.00 wt%-20.00 wt%, 18.70 wt%-20.00 wt%, and the like. In some embodiments, the mass fraction of MgO can be controlled at 0.00 wt%, 1.00 wt%, 2.00 wt%, 3.00 wt%, 4.00 wt%, 5.00 wt%, 6.00 wt%, 7.00 wt%, 8.00 wt%, 9.00 wt%, 10.00 wt%, 11.00 wt%, 12.00 wt%, 13.00 wt%, 14.00 wt%, 15.00 wt%, 16.00 wt%, 17.00 wt%, 18.00 wt%, 19.00 wt%, 20.00 wt%, etc.
[0051] ZrO2 and P2O5 are effective nucleating agents, mainly used to control the crystal growth rate on the surface and inside of the base glass to be consistent. The mass fraction of ZrO2 should be controlled between 0.50 and 10.00%, and the mass fraction of P2O5 should be controlled between 0.00 and 5.00%.
[0052] In some embodiments, the mass fraction of ZrO2 includes 0.50 wt% to 10.00 wt% and all ranges and sub-ranges therebetween, such as 0.50 wt%-10.00 wt%, 0.50 wt%-7.50 wt%, 0.50 wt%-4.00 wt%, 0.80 wt%-10.00 wt%, 0.80 wt%-4.00 wt%, 4.00 wt%-10.00 wt%, 4.00 wt%-8.00 wt%, 4.00 wt%-6.00 wt%, etc. In some embodiments, the content of ZrO2 can be controlled at 0.00 wt%, 0.50 wt%, 0.80 wt%, 1.00 wt%, 2.00 wt%, 3.00 wt%, 4.00 wt%, 5.00 wt%, 6.00 wt%, 7.00 wt%, 8.00 wt%, 9.00 wt%, 10.00 wt%, etc.
[0053] In some embodiments, the mass fraction of P2O5 includes 0.00 wt% to 5.00 wt% and all ranges and sub-ranges therebetween, such as 1.00 wt%-5.00 wt%, 1.00 wt%-4.00 wt%, 1.00 wt%-3.00 wt%, 1.00 wt%-2.00 wt%, 2.00 wt%-5.00 wt%, 3.00 wt%-5.00 wt%, 4.00 wt%-5.00 wt%, 2.00 wt%-4.00 wt%, 2.00 wt%-3.00 wt%, etc. In some embodiments, the mass fraction of P2O5 can be controlled at 0.00 wt%, 0.50 wt%, 0.75 wt%, 1.00 wt%, 1.50 wt%, 2.00 wt%, 2.50 wt%, 3.00 wt%, 3.50 wt%, 4.00 wt%, 4.50 wt%, 5.00 wt%, etc.
[0054] The addition of TiO2 as an effective nucleating agent can control the size of the precipitated crystals of the base glass to less than 2μm, reducing the risk of cracks in the base glass due to the formation of large crystals.
[0055] In some embodiments, the mass fraction of TiO2 includes 0.00 wt% to 5.00 wt% and all ranges and sub-ranges therebetween, for example, it can be controlled at 1.00 wt%-5.00 wt%, 1.00 wt%-4.70 wt%, 1.00 wt%-4.60 wt%, 1.00 wt%-4.00 wt%, 1.00 wt%-3.00 wt%, 1.00 wt%-2.00 wt%, 2.00 wt%-5.00 wt%, 2.00 wt%-4.00 wt%, 3.00 wt%-5.00 wt%, 3.00 wt%-4.00 wt%, 2.00 wt%-3.00 wt%, etc. In some embodiments, the mass fraction of TiO2 can be controlled at 0.00 wt%, 0.50 wt%, 0.75 wt%, 1.00 wt%, 1.50 wt%, 2.00 wt%, 2.50 wt%, 3.00 wt%, 3.50 wt%, 4.00 wt%, 4.60 wt%, 4.70 wt%, 5.00 wt%, etc.
[0056] The addition of CaO can effectively reduce the liquidus viscosity of the base glass, thereby reducing the difficulty of forming. However, too much CaO will cause crystallization during the forming process of the base glass. In this application, the mass fraction of CaO is 0.00-5.00%.
[0057] In some embodiments, the mass fraction of CaO includes 0.00 wt% to 5.00 wt% and all ranges and sub-ranges therebetween, such as 1.00 wt%-5.00 wt%, 1.50 wt%-5.00 wt%, 2.00 wt%-5.00 wt%, 3.00 wt%-5.00 wt%, 4.00 wt%-5.00 wt%, 2.00 wt%-4.00 wt%, 2.00 wt%-3.00 wt%, etc. In some embodiments, the content of KO can be controlled at 0.00 wt%, 1.00 wt%, 1.50 wt%, 2.00 wt%, 2.50 wt%, 3.00 wt%, 3.50 wt%, 4.00 wt%, 4.50 wt%, 5.00 wt%, etc.
[0058] In the present application, the material of the blank to be hot-bent is glass or glass ceramic, and its thermal expansion coefficient has a wide range. If the thermal expansion coefficients of the hot-bending mold and the blank to be hot-bent are greatly different, the roughness of the blank after hot-bending will be greatly increased, so the mold is required to have a wide range and adjustable thermal expansion coefficient.
[0059] When the absolute value of the ratio of the thermal expansion coefficient A1 of the glass-ceramic mold to the thermal expansion coefficient A2 of the blank to be hot-bent is between 0.2 and 1.4, the average roughness of the blank after hot bending only increases by 12% to 40% compared with that before hot bending. Furthermore, when the absolute value of the ratio of the thermal expansion coefficient A1 of the glass-ceramic mold to the thermal expansion coefficient A2 of the blank to be hot-bent is between 0.3 and 0.7, the average roughness of the blank after hot bending only increases by 15% to 30% compared with that before hot bending.
[0060] When the absolute value of the ratio of the thermal expansion coefficient A1 of the mold to the thermal expansion coefficient A2 of the blank to be hot-bent is between 0 and 0.2, the average roughness of the blank after hot-bending is only increased by 70% to 95% compared with that before hot-bending.
[0061] Compared with the 400% increase in the average roughness of the blank after hot bending in a metal mold or a graphite mold, the increase in the average roughness of the blank after hot bending in the glass-ceramic mold of the present invention has been greatly improved, and the problem of a significant increase in roughness caused by the difference in expansion coefficient between the traditional hot bending mold and the glass / glass ceramic to be hot bent has also been solved.
[0062] In the present application, the thermal expansion coefficient of the glass-ceramic mold is tested at 25-1000° C. using a Linseth DIL-L76 thermal expansion instrument, and the size of the glass-ceramic mold test sample is 5 mm*5 mm*50 mm.
[0063] Therefore, in the present application, the mass fraction of Li2O is controlled within the range of 0.50% to 10.00%, and the mass ratio of Na2O, K2O, and Li2O in the raw material satisfies: (Na2O+K2O) / Li2O<1.00, the total mass fraction of Na2O and K2O is ≤8.00%, Na and K are generally enriched in the glass phase after the base glass is crystallized, and excessive Na2O and K2O will significantly increase the thermal expansion coefficient and reduce the glass transition temperature of the glass ceramic. At the same time, the mass fractions of β-quartz, β-spodumene, and β-eucryptite are controlled within the range of 0.1% to 70.0%. β-quartz, β-spodumene, and β-eucryptite are three crystals with low thermal expansion coefficients. Controlling their total mass ratio can contribute to the adjustment of the thermal expansion coefficient of the entire glass-ceramic mold, thereby achieving that the thermal expansion coefficient of the glass-ceramic mold is adjustable within the temperature range of 25 to 1000°C, and the adjustment range is -1.0×10 -6 ~3.0×10 -5 / K.
[0064] While meeting the requirement of low thermal expansion coefficient, the glass-ceramic mold of the present application also has a wide adjustable thermal expansion coefficient range, so that the mold has a wider application range and improves the applicability of the mold.
[0065] The glass transition temperature of the glass ceramic mold of the present application is greater than or equal to 700°C. The glass transition temperature of the glass ceramic mold is relatively high, that is, the softening point is relatively high, which can adapt to the high temperature during the hot bending process and avoid deformation of the hot bending blank and reduction of dimensional accuracy. At the same time, the transition temperature of the residual glass phase after the mold is crystallized will also increase, which can reduce the deformation of the glass phase of the mold when the mold is in use.
[0066] It should be noted that β-quartz includes two types: β-quartz solid solution and β-quartz. When the mass fraction of β-quartz, β-spodumene and β-eucryptite in glass ceramics is greater than 70.0%, the thermal expansion coefficient of the glass ceramic mold as a whole will be significantly reduced, resulting in a significant reduction and narrowing of the thermal expansion coefficient range of the glass ceramic mold in the temperature range of 25 to 1000°C, especially weakening the upper limit of its thermal expansion coefficient range.
[0067] In some embodiments, the sum of the mass fractions of β-quartz, β-spodumene and β-eucryptite in the glass-ceramics of the present application includes all ranges and sub-ranges between 0.1% and 70.0%, for example, it can be controlled within 0.1%-70.0%, 5.0%-70.0%, 5.0%-60.0%, 5.0%-50.0%, 5.0%-47.0%, 5.0%-37.0%, 5.0%-35.0%, 5.0%-33.0%, 5.0%-30.0%, 5.0%-25.0%, 5.0%-16.0%, 16.0%-60.0%, 16.0%-50.0%, 16.0%-47.0%, 16.0%-35.0%, 16.0%-20.0%, 33.0%-70.0%, 33.0%-60.0%, 33.0%-50.0%, 33.0%-47.0%, etc. In some embodiments, the sum of the mass fractions of β-quartz, β-spodumene and β-eucryptite in the glass-ceramic of the present application can be controlled at 10.0 wt.%, 11.0 wt.%, 12.0 wt.%, 13.0 wt.%, 14.0 wt.%, 15.0 wt.%, 16.0 wt.%, 17.0 wt.%, 18.0 wt.%, 19.0 wt.%, 20.0 wt.%, 21.0 wt.%, 22.0 wt.%, 23.0 wt.%, 24.0 wt.%, 25.0 wt.%, 26.0 wt.%, 27.0 wt.%, 28.0 wt.%, 29.0 wt.%, 30.0 wt.%, 31.0 wt.%, 32.0 wt.%, 33.0 wt.%, 34.0 wt.%, 35.0 wt.%, 36.0 wt.%, 37.0 wt. %, 38.0 weight%, 39.0 weight%, 40.0 weight%, 41.0 weight%, 42.0 weight%, 43.0 weight%, 44.0 weight%, 45.0 weight%, 46.0 weight%, 47.0 weight%, 48.0 weight%, 49.0 weight%, 50.0 weight%, 51.0 weight%, 52.0 weight%, 53.0 weight%, 54.0 weight%, 55.0 weight%, 56.0 weight%, 57.0 weight%, 58.0 weight%, 59.0 weight%, 60.0 weight%, 61.0 weight%, 62.0 weight%, 63.0 weight%, 64.0 weight%, 65.0 weight%, 66.0 weight%, 67.0 weight%, 68.0 weight%, 69.0 weight%, 70.0 weight% and so on.
[0068] In the present application, a Mettler-Toledo DSC-3 differential scanning calorimeter was used to test the glass transition temperature of the glass-ceramic mold. The glass-ceramic mold was ground in advance using an agate mortar and then passed through a 200-mesh sieve, and the sieved powder was tested.
[0069] In at least one embodiment, the thermal conductivity of the glass-ceramic mold provided by the present application is greater than or equal to 1 W / (m·k) in the temperature range of 25 to 1000° C. In this way, the mold can be heated up quickly, and the heat can be better transferred to the hot-bent blank, ensuring that the temperature of the mold and the blank quickly reaches consistency, and also ensuring the consistency of the temperature of each part of the mold.
[0070] The present application also provides a method for preparing a glass ceramic mold, as shown below Figure 1 The present invention describes in detail the method for preparing the glass ceramic mold disclosed in the present application. Figure 1 As shown, the method disclosed in this embodiment mainly includes the following steps S100 to S500.
[0071] Step S100, a mixing process, weighing and mixing the raw materials uniformly to form a basic mixture, wherein the raw materials include the following weight parts:
[0072] SiO2: 40.00~80.00 parts; Al2O3: 18.00~40.00 parts; ZrO2: 0.50~10.00 parts; Li2O: 0.50~10.00 parts; Na2O: 0.00~2.00 parts; B2O3: 0.00~5.00 parts; K2O: 0.00~5.00 parts; MgO: 0.00~20.00 parts; CaO: 0.00~5.00 parts; P2O5: 0.00~5.00 parts; TiO2: 0.00~5.00 parts; BaO: 0.00~2.00 parts; ZnO: 0.00~10.00 parts.
[0073] Specifically, the above raw materials and the clarifier are accurately weighed, fully mixed and loaded into a corundum crucible. The clarifier is selected from one or more of As2O3, Sb2O3, SnO2, chloride, fluoride, SO3-containing compounds, and NO3-containing compounds, preferably selected from one or more of SnO2, SO3-containing compounds, chloride, and NO3-containing compounds; the clarifier content is preferably 0-2 weight%.
[0074] Step S200 is a melting process, in which the basic mixture is melted and poured into a mold to form a basic glass piece.
[0075] Specifically, the corundum crucible containing the uniformly mixed raw materials is placed in a silicon-molybdenum rod electric furnace and melted at 1500-1700° C. for 3-16 hours. After the glass liquid is clarified and homogenized, it is poured into a mold to form a basic glass part.
[0076] It should be noted that the mold described here is used to hold a molten mixture of glass raw materials, and then cool it down to obtain a basic glass part.
[0077] Step S300, a molding process, wherein the basic glass component is formed into a glass mold component of a desired shape.
[0078] Specifically, the forming process is cold carving or hot bending.
[0079] Furthermore, when the forming process is hot bending, a 3D hot bending machine on the market is used to perform hot bending to obtain a glass mold part, such as a DTK commercially available model, a Mirley commercially available model, etc. In some embodiments, a DTK-DGP-3D12S3D hot bending machine, or a Mirley CG07-4222 hot bending machine, etc. can be selected.
[0080] Furthermore, when the forming process is cold carving, an annealing process is also included before the forming process, and the annealing process is to anneal the basic glass piece and cool it to room temperature. Glass annealing is to reheat the glass product with permanent stress to a temperature at which the particles inside the glass can move, and use the displacement of the particles to disperse the stress to eliminate or weaken the permanent stress, thereby improving the thermal expansion uniformity and mechanical strength of the glass product.
[0081] The annealing range of glass is generally between the annealing point and the strain point, and the corresponding glass viscosity is 1013dPa·s to 1014.7dPa·s. When the temperature is higher than the annealing point, the glass will soften and deform; when the temperature is lower than the lower limit of the annealing temperature, the glass structure can actually be considered fixed, and the internal particles can no longer move, so it is impossible to disperse or eliminate stress. The internal stress of the glass can be eliminated within a few hours near the strain point. In theory, the longer the annealing time, the smaller the stress of the glass and the higher the uniformity. In addition, new stress will be newly generated during the annealing and cooling process of the glass. The slower the cooling rate, the smaller the stress generated, the higher the stress uniformity of the internal and external glass, and the higher the uniformity of the thermal expansion coefficient of the glass.
[0082] Specifically, the obtained basic glass parts are annealed at 600-900°C for 30-1200h. Furthermore, in order to control the consistency of the expansion coefficients of different parts of the mold, the annealing time is preferably more than 120h. In this application, the annealing point of the glass is confirmed in accordance with the standard GB / T 28196-2011 "Test Method for Annealing Point and Strain Point of Glass", and the strain point is determined by extrapolating the annealing point data. The strain point is the temperature when the viscous deflection velocity is 0.0316 times the annealing viscous deflection velocity. The annealing temperature of this application is the temperature when the annealing viscous deflection velocity of the glass is 0.02-0.0316 times. Within this temperature range, a better annealing effect can be obtained, that is, the higher the uniformity of the thermal expansion coefficient.
[0083] Then it is cooled to room temperature at a cooling rate of 5 to 20°C / h, and then the base glass is ground by CNC cold engraving to remove the excess, and the base glass is chamfered and drilled by a drill to meet the requirements of the final product to obtain a glass mold part.
[0084] Step S400, a microcrystallization process, performing nucleation and crystallization treatments on the glass mold piece in sequence to produce the microcrystallized mold piece;
[0085] Specifically, the nucleation temperature is 650-1000° C., and the nucleation time is 1-6 hours; the crystallization temperature is 900-1400° C., and the crystallization time is 0-15 hours.
[0086] In one embodiment, when the molding process is hot bending molding, the microcrystallization process can be performed simultaneously with the hot bending molding. Specifically, the microcrystallization process can be performed while the glass mold piece is hot bending molding.
[0087] Among them, the nucleation treatment process is: by introducing a suitable nucleating agent into the glass component, during the subsequent heat treatment process, the viscosity of the glass is reduced, and a large number of uniform tiny crystals, namely nuclei, will precipitate (nucleate and grow) in the glass.
[0088] The crystallization process: the required crystals grow on the surface of the precipitated crystal nuclei, so that the internal composition of the glass changes into crystal phase and glass phase.
[0089] Appropriate nucleation temperature and time are conducive to the precipitation of uniform and fine crystal nuclei, and further the growth of uniform and fine crystals during the crystallization process.
[0090] Confirmation of nucleation temperature in this application: The glass transition temperature Tg of the glass is tested by differential scanning calorimetry (DSC), and the nucleation temperature is (Tg-20) to (Tg+130)°C. The specific test conditions are as follows: the glass is annealed and ground, and passed through a 200-mesh sieve. After the sieved glass powder is dried at 300°C for 60 minutes, 20 mg of the glass powder is dried at a heating rate of 10°C / min, and the DSC data from room temperature to 1500°C is tested, and the maximum slope of the first endothermic peak of the DSC curve is taken as the Tg point.
[0091] Crystallization is the process of growing crystals in glass ceramics or glass with formed crystal nuclei through heat treatment.
[0092] Confirmation of the crystallization temperature in this application: Use differential scanning calorimetry (DSC) to test the first crystallization peak temperature Tc of the glass, and the crystallization temperature is (Tc-50) ~ (Tc+50) ° C. The specific test conditions are as follows: grind the glass after annealing, pass through a 200 mesh sieve, dry the sieved glass powder at 300 ° C for 60 minutes, take 20 mg of the glass powder and dry it at a heating rate of 10 ° C / min, test the DSC data from room temperature to 1500 ° C, and take the minimum slope of the first exothermic peak of the DSC curve as the Tc point.
[0093] Effect of crystallization on thermal expansion coefficient: Different degrees of crystallinity can be obtained by controlling the crystallization temperature and crystallization time of the blank. The thermal expansion coefficients of glass-ceramics with different crystalline phases are quite different. Therefore, the thermal expansion coefficient of glass-ceramics can be controlled by adjusting the composition, crystallization temperature and crystallization time.
[0094] Effect of crystallization on thermal shock resistance: When cracks extend along the boundaries of different particles with greatly different thermal expansion coefficients, the thermal shock resistance of the material is improved because the cleavage planes within the crystals can be bent, passivated and branched. Therefore, glass-ceramics with high thermal shock resistance can be obtained by adjusting the raw material composition, crystallization temperature and crystallization time.
[0095] Specifically, the glass mold part is nucleated at 650-1000° C. for 1-6 h, and then crystallized at 900-1400° C. for 0-15 h. Further, the crystallization time includes 0-15 h and all ranges and sub-ranges therebetween, for example, 1 h-2 h, 1 h-3 h, 1 h-4 h, 1 h-5 h, 2 h-3 h, 2 h-4 h, 2 h-5 h, 5 h-15 h, 10 h-11 h, 10 h-12 h, 10 h-13 h, 10 h-14 h, 10 h-15 h, 14 h-15 h, etc., preferably 5 h-15 h, including 6 h-15 h, 7 h-12 h, 7 h-14 h, 7 h-15 h, etc.
[0096] Step S500, a cooling process, annealing and cooling the microcrystallized mold part to room temperature to generate a glass ceramic mold.
[0097] Specifically, the mold is cooled to room temperature at a cooling rate of 5 to 40° C. / h. To control the uniformity of the expansion coefficients of different parts of the mold, a cooling rate of 5 to 20° C. / h is preferred.
[0098] In at least one embodiment, after the cooling process, a polishing process of the glass ceramic mold is also included. After the mold is prepared, when the hot-bending blank is hot-bent, the hot-bending blank is placed in the above mold, and then placed in a hot bending machine, the hot bending process is set, and the hot bending mold is taken out after cooling. The hot bending mold has the advantages of high thermal conductivity, high temperature resistance, high softening point and high thermal shock resistance, and the dimensional accuracy of the glass after hot bending does not change. It is also resistant to oxidation at high temperatures and has a long service life, which is suitable for mass production of 2.5D or 3D glass.
[0099] In at least one embodiment, the expansion coefficient uniformity test method is: on the prepared basic mold, take A and B samples with a diameter of 6 mm and a thickness of 10 mm, and test the thermal expansion coefficient respectively. If A / B is between 0.995 and 1.005, it meets the uniformity requirement of the annealing expansion coefficient. The test instrument is a German NETZSCH-DIL402C high temperature thermal expansion coefficient instrument.
[0100] The thermal conductivity test method of glass ceramic mold is as follows: the test sample size is 100mm*100*1mm in length, width and thickness. The test instrument is the heat flow method thermal conductivity tester HFM436.
[0101] The method for testing the average roughness is: use a chemical mineral TR200 roughness meter to test the sample surface three times, each sampling length is 20 mm, and the average value of the three measured roughness is taken as the average roughness of the sample.
[0102] The performance parameters of the glass-ceramic mold prepared in the present application are explained below through specific examples and comparative examples.
[0103] The following Table 1-1 is a raw material composition table of the base glass of each glass-ceramic mold in Examples 1-6 and Comparative Example 1, Table 1-2 is a specific process parameter table of the preparation process of each glass-ceramic mold in Examples 1-6 and Comparative Example 1, and Table 1-3 is a main crystal phase and performance parameter table of each glass-ceramic mold prepared in Examples 1-6 and Comparative Example 1.
[0104] Table 1-1 Basic glass composition of glass ceramic molds
[0105]
[0106]
[0107] Table 1-2 Glass ceramic mold preparation process parameters
[0108]
[0109]
[0110] Taking Example 1 as an example, the preparation process of the glass ceramic mold is specifically described according to the data in Tables 1-1 and 1-2:
[0111] Accurately weigh the raw materials: SiO2: 47.10 parts; Al2O3: 28.50 parts; ZrO2: 0.80 parts; Li2O: 2.50 parts; Na2O: 0.00 parts, B2O3: 0.00 parts, K2O: 0.80 parts, MgO: 13.30 parts, CaO: 0.00 parts, P2O5: 0.00 parts, TiO2: 4.70 parts, BaO: 0.00 parts, ZnO: 2.30 parts. Fully mix the raw materials, put them into a corundum crucible, add a clarifier, place the corundum crucible in a silicon-molybdenum rod electric furnace and melt at 1640°C for 5 hours, and after the glass liquid is clarified and homogenized, pour it into the mold to form a basic glass part. The obtained basic glass parts are annealed at 720°C for 120h, and then cooled to room temperature at a cooling rate of 6°C / h, followed by CNC cold engraving, and the basic glass is edged to remove the excess, and the basic glass is chamfered and drilled by a drill to meet the requirements of the final product to obtain a glass mold part. The glass mold part is nucleated at 830°C for 2h, then crystallized at 1200°C for 3h, and then cooled to room temperature at a cooling rate of 7°C / h, and then polished to complete the preparation process of the glass ceramic mold.
[0112] Examples 2-6 and Comparative Example 1 also refer to the data requirements of Table 1-1 and Table 1-2 and are the same as the preparation process of Example 1, which will not be repeated here. Table 1-3 is a table of main crystal phases and performance parameters of glass hot bending molds prepared based on Table 1-1 and Table 1-2.
[0113] Table 1-3 Glass ceramic mold crystal phase and performance parameters
[0114]
[0115]
[0116] Taking Example 1 as an example, the prepared hot bending mold is described according to Tables 1-3:
[0117] The main crystal phases of the prepared glass-ceramic mold include: cordierite, β-quartz solid solution, β-quartz, and the mass fraction of the sum of β-quartz solid solution, β-quartz, β-spodumene and β-eucryptite in the crystal phase is 16wt.0%, and the glass transition temperature of the crystallized glass-ceramic mold is 760°C; the thermal expansion coefficient at 25-1000°C is 2.2×10 -6 / K; On the prepared basic mold, samples A and B with a diameter of 6 mm and a thickness of 10 mm were taken, and the thermal expansion coefficients of samples A and B were tested respectively using a German NETZSCH-DIL402C high-temperature thermal expansion coefficient instrument, and the result showed that A / B was 0.996, which met the uniformity requirements of the annealing expansion coefficient;
[0118] When testing the thermal conductivity, a sample with a length, width and thickness of 100mm*100*1mm was obtained from the glass ceramic mold, and the thermal conductivity was tested using the heat flow method thermal conductivity tester HFM436. The thermal conductivity was 2.81W / (m·k). When testing the average roughness of the glass ceramic mold, the chemical mineral TR200 roughness meter was used to test the surface of the glass ceramic mold of Example 1 three times, each sampling length was 20mm, and the average value of the three measured roughness was used as the average roughness of the sample. The average roughness of the glass ceramic mold of Example 1 was measured to be 0.008μm. Examples 2-6 and Comparative Example 1 are the same as above, and will not be repeated here.
[0119] Among them, the raw material composition of Comparative Example 1 is the same as that of Example 3, the crystallization temperature in the preparation process is 1450 degrees, which is greater than 1400 degrees, the crystallization time is 30, which is greater than 15 hours, and the main crystal phase of the prepared hot bending mold is β-quartz solid solution, and the mass fraction of the β-quartz solid solution, β-quartz, β-spodumene and β-eucryptite of the prepared hot bending mold is 73wt%, which is greater than 70wt%, thereby reducing the overall thermal expansion coefficient of the glass-ceramic mold.
[0120] The glass or glass ceramic blanks were hot bent using the glass ceramic molds prepared in the above Examples 1-6. Five blanks AE to be hot bent were selected. The raw material composition and performance parameters of each blank to be hot bent are shown in Tables 1-4.
[0121] Table 1-4 Composition and properties of raw materials for hot bending blanks
[0122]
[0123] According to Tables 1-4, blanks B and C are glass, and blanks A, D and E are glass ceramics. First, blanks A from different batches are selected and hot-bending is performed using the hot-bending mold prepared in Example 1-6. The roughness of blanks A produced from different batches is different. The performance of the blanks after hot bending is shown in Table 1-5.
[0124] Table 1-5 Performance parameters of blank A after hot bending
[0125]
[0126] According to Tables 1-5, the average roughness of the blanks A after hot bending of different batches of blanks A prepared by the glass-ceramic molds of Examples 1-6 is improved slightly, which is much less than the 400% increase in the average roughness of the blanks after hot bending in metal molds or graphite molds, and when the absolute value of the ratio of the thermal expansion coefficient A1 of the glass-ceramic mold to the thermal expansion coefficient A2 of the blank to be hot-bent is in the range of 0.2 to 1.4, the average roughness of the blank after hot bending is in the range of 12% to 40%. As mentioned above, the glass-ceramic mold of this application has good applicability for blanks of the same glass system but different roughness.
[0127] Furthermore, the glass-ceramic mold prepared in Example 1 was selected to perform hot bending processing on the blanks A and E in Tables 1-4 above, and the properties of the blanks after processing are shown in Tables 1-6.
[0128] Table 1-6 Performance parameters of blank after AE hot bending
[0129]
[0130] According to Tables 1-6, the hot bending mold prepared in Example 1 is used to hot bend blanks A-E of different systems. The blank system after hot bending does not change, and the average roughness improvement is small. When the absolute value of the ratio of the thermal expansion coefficient A1 of the glass-ceramic mold and the thermal expansion coefficient A2 of the blank to be hot-bent is in the range of 0.2 to 1.4, the average roughness of the blank after hot bending is in the range of 12% to 40%. It can be seen that the glass-ceramic mold of the present application has good applicability for blanks of different glass systems.
[0131] For the process parameter range provided in Example 1, a set of comparative examples is provided for annealing time, nucleation time, crystallization time and annealing temperature, respectively. The obtained hot bending die performance and the blank condition after hot bending are shown in Tables 1-7:
[0132] Table 1-7 Process parameter comparison table
[0133]
[0134]
[0135] According to Tables 1-7, when the annealing time is less than 30h, the thermal expansion coefficient of 25-1000℃ is large, and the uniformity of the thermal expansion coefficient is relatively unstable, and the average roughness of the blank after hot bending is greatly improved; when the nucleation time is less than 1h, due to the short nucleation time, the glass undergoes non-uniform crystallization during crystallization, and the glass breaks after crystallization and cannot be used; when the crystallization time is greater than 15h, the thermal expansion coefficient of 25-1000℃ is large, and the uniformity of the thermal expansion coefficient is relatively unstable, and the average roughness of the blank after hot bending is greatly improved; when the annealing temperature is greater than 900℃, the thermal expansion coefficient of 25-1000℃ is large, and the uniformity of the thermal expansion coefficient is relatively unstable, and the average roughness of the blank after hot bending is greatly improved; it can be seen that the annealing time, nucleation time, crystallization time and annealing temperature specified in this application can produce a glass-ceramic mold with a suitable thermal expansion coefficient, good uniformity, and low average roughness of the blank after hot bending.
[0136] The present application also provides a pair of comparisons, which are common graphite hot bending molds on the market. The graphite mold of comparison 1 and the glass ceramic mold of Example 1 are used to hot bend the same blank to be hot bent. The performance is compared with that of Example 1, as shown in the following table:
[0137] Table 1-8 Performance parameter comparison table
[0138] Performance parameters Example 1 Graphite mold <![CDATA[Coefficient of thermal expansion (25 to 1000 °C) / (×10 -6 / K)]]> 2.2 4.0 Thermal conductivity (25~1000℃) / [W / (m·k)] 2.81 4.18 Bending temperature (℃, air atmosphere) 760 760 Normal hot bending temperature (℃, air atmosphere) 700-1100 <350 Average roughness of mold (μm) 0.008 0.009 Average roughness of the hot-bending blank before hot bending (μm) 0.0076 0.0076 The average roughness of the hot-bent blank after hot bending is improved 23% 320% Increase percentage of mold roughness after hot bending 4% 450% Mold mass reduction after hot bending 0% 12%
[0139] According to the above Tables 1-1 to 1-8, the prepared glass ceramic mold has good performance through the coordination and adjustment of the raw material ratio and the strict control of the preparation process. By controlling (Na2O+K2O) / Li2O<1.00 in the raw material and the total mass fraction of Na2O and K2O≤8.00%, the thermal expansion coefficient of the glass ceramic is controlled within the range of -1.0×10-6 to 3.0×10-5 / K, and its glass transition temperature is greater than or equal to 700°C, and the mass fraction of Li2O in the raw material is controlled within the range of 0.50 to 10.00%, so that the mass fraction of the sum of crystallized β-quartz, β-spodumene and β-eucryptite is within the range of 0.1% to 70.0%, thereby achieving that the thermal expansion coefficient of the glass ceramic mold can be adjusted within the temperature range of 25 to 1000°C (the adjustment range is -1.0×10 -6 ~3.0×10 -5 / K).
[0140] Therefore, since the glass-ceramic mold has a widely adjustable thermal expansion coefficient, it can adapt to the thermal expansion coefficient of the blank, improve the large thermal expansion coefficient difference, and thus avoid the problem of a large increase in roughness.
[0141] In addition, the glass transition temperature of the glass-ceramic mold is relatively high, that is, the softening point is relatively high, which can adapt to the high temperature during the hot bending process and avoid deformation of the hot-bending blank and reduction in dimensional accuracy.
[0142] On the other hand, the thermal conductivity of the prepared glass-ceramic mold is greater than or equal to 1 W / (m·k) in the temperature range of 25 to 1000°C, has good thermal conductivity, and can achieve rapid heat transfer. Furthermore, by controlling the annealing time, annealing temperature, nucleation time, and crystallization time in the process parameters within a reasonable range, the uniformity of the expansion coefficient of different parts of the glass-ceramic mold can be controlled, and the low roughness of the blank after hot bending can be ensured.
[0143] Further, according to the comparison between the comparative examples in Tables 1-8 and Example 1, under the conditions that the hot bending temperature is 760°C, the average roughness of the hot-bending blanks before hot bending is 0.0076μm, and the average roughness of the molds is similar, the improvement in the average roughness of the glass-ceramic mold provided in the present application after hot bending the blank is much smaller than that of the traditional graphite mold, and the reduction in mold mass of the glass-ceramic mold after hot bending the blank is 0%, while the reduction in the graphite mold is 12%, and the operating temperature of the glass-ceramic mold provided in the present application is much higher than that of the traditional graphite mold.
[0144] Therefore, the glass ceramic mold provided by the present application overcomes the shortcomings of traditional graphite molds such as lack of oxidation resistance, short life and low operating temperature, and achieves the advantages of high thermal conductivity, high temperature resistance, high softening point and high thermal shock resistance, and the dimensional accuracy of the glass does not change after hot bending.
[0145] The above is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application shall be based on the protection scope of the claims.
Claims
1. A glass ceramic mold for hot bending of glass or glass ceramic blanks, characterized in that: The main crystalline phase of the glass-ceramic mold includes one or more of β-quartz, β-spodumene and β-eucryptite, and the mass fraction of the β-quartz + the mass fraction of the β-spodumene + the mass fraction of the β-eucryptite is in the range of 0.1% to 70.0%; the thermal expansion coefficient of the glass-ceramic mold is -1.0×10 -6 ~3.0×10 -5 / K; the components of the glass-ceramic mold include Li2O, which is in the range of 0.50% to 10.00% by mass fraction; the components of the glass-ceramic mold also include Na2O and K2O, and the mass ratio of Na2O, K2O and Li2O is required to be as follows: (Na2O+K2O) / Li2O<1.00, and the total mass fraction of Na2O and K2O is ≤8.00%; the absolute value of the ratio of the thermal expansion coefficient of the glass-ceramic mold to the thermal expansion coefficient of the blank to be hot-bent is between 0.2 and 1.4, and the average roughness of the blank after hot bending is increased by 12% to 40% relative to that before hot bending.
2. The glass ceramic mold according to claim 1, characterized in that: The main crystalline phase also includes MgAl2Si3O 10 , MgAl2O4, ZnAl2O4 and mullite.
3. The glass ceramic mold according to claim 1 or 2, characterized in that: The components of the glass-ceramic mold include the following raw materials in weight percentage: SiO2: 40.00~80.00%; Al2O3: 18.00~40.00%; ZrO2: 0.50~10.00%; Li2O: 0.50~10.00%; Na2O: 0.00~2.00%; B2O3: 0.00~5.00%; K2O: 0.00~5.00%; MgO: 0.00~20.00%; CaO: 0.00~5.00%; P2O5: 0.00~5.00%; TiO2: 0.00~5.00%; BaO: 0.00~2.00%; ZnO: 0.00~10.00%.
4. The glass-ceramic mold according to claim 3, characterized in that: The glass transition temperature of the glass-ceramic mold is greater than or equal to 700°C.
5. The glass-ceramic mold according to any one of claims 1 to 2, characterized in that: The thermal conductivity of the glass ceramic mold is greater than or equal to 1 W / (m·k) within a temperature range of 25 to 1000° C.
6. A method for preparing a glass-ceramic mold as claimed in any one of claims 1 to 5, characterized in that: The steps include: In the mixing process, each raw material is weighed and mixed evenly to form a basic mixture. The components of the glass-ceramic mold include the following raw materials in percentage by weight: SiO2: 40.00~80.00%; Al2O3: 18.00~40.00%; ZrO2: 0.50~10.00%; Li2O: 0.50~10.00%; Na2O: 0.00~2.00%; B2O3: 0.00~5.00%; K2O : 0.00~5.00%; MgO: 0.00~20.00%; CaO: 0.00~5.00%; P2O5: 0.00~5.00%; TiO2: 0.00~5.00%; BaO: 0.00~2.00%; ZnO: 0.00~10.00%; A melting step, melting the basic mixture and pouring it into a mold to form a basic glass piece; A molding process, in which the basic glass piece is made into a glass mold piece of a desired shape; A microcrystallization treatment step, wherein the glass mold piece is subjected to nucleation and crystallization treatments in sequence to form a microcrystallized mold piece; The cooling step is to cool the microcrystallized mold to room temperature to form a glass ceramic mold.
7. The method according to claim 6, characterized in that The melting temperature is 1500-1700° C., and the melting time is 3-16 hours.
8. The method according to claim 6, characterized in that The nucleation temperature is 650-1000° C., and the nucleation time is 1-6 hours; the crystallization temperature is 900-1400° C., and the crystallization time is 0-15 hours.
9. The method according to claim 6, characterized in that The forming process is hot bending forming, and the microcrystallization process is performed simultaneously with the hot bending forming.
10. The method according to claim 6, characterized in that The forming process is cold carving.
11. The method according to claim 10, characterized in that An annealing process is also included before the cold carving process, and the annealing process is to anneal the basic glass piece and cool it to room temperature.
12. The method according to claim 11, characterized in that The annealing temperature in the annealing process is 600-900° C., the annealing time is 30-1200 hours, and the material is cooled to room temperature at a cooling rate of 5-20° C. / h.
13. The method according to claim 6, characterized in that The cooling rate in the cooling step is 5 to 40° C. / h.
14. The method according to claim 6, characterized in that After the cooling process, the method further includes a polishing process for the glass ceramic mold.
Citation Information
Patent Citations
Forming method for glass and glass-ceramic
CN1495134A
Class ceramic mold for resin lens
JP1987182134A
Mold for molding resin and method of manufacturing the same
JP2001150452A
Method of forming sagging mold from a glass ceramic
US4059428A
Method for casting glass-plastic lenses comprising allyl diglycol carbonate plastic
US4246207A