A transmission electron microscope magnetic sample pretreatment method and system
By dispersing magnetic samples in volatile solvents in transmission electron microscopes to form suspension, drying and coating with ultra-thin carbon films, the problem of adsorption of magnetic samples on pole boots is solved, and high-resolution transmission electron microscope imaging is achieved , suitable for batch processing of nanoscale magnetic particles.
Patent Information
- Application Number
- CN202310170104.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-27
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-02-27
AI Technical Summary
The prior art When processing magnetic samples in transmission electron microscopes, the sample is easily adsorbed to the pole boots, resulting in a decrease in the resolution of the electron microscope. Common methods such as demagnetization, magnet removal and dual network wrapping destroy material activity, complex operation and difficult to batch processing. The problem.
The magnetic sample of transmission electron microscope is dispersed in volatile solvents to form a suspension. After drying, the ultra-thin support film without holes is covered on the loading net, and the carbon-plated film with a thickness of 5~35nm is plated on the surface of the loading net to fix the sample. To avoid adsorption.
Effectively fix nanomagnetic particles, avoid adsorption on pole boots, obtain clear high-resolution transmission electron microscope photos, and the carbon coating thickness can be adjusted to suit samples of different sizes, suitable for batch processing.
Smart Images

Figure CN116413291B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electron microscope sample pretreatment, and in particular to a transmission electron microscope magnetic sample pretreatment method and system. Background Art
[0002] With the continuous development of nanotechnology, the application of transmission electron microscope in the field of materials has become increasingly widespread. As a very unique type of functional materials, the demand for transmission electron microscope testing of nanomagnetic materials is increasing. The imaging system of the transmission electron microscope is composed of multiple magnetic lenses, among which the objective lens is composed of lens coils, magnetic circuits and pole shoes. The sample to be tested is placed between the upper and lower pole shoes of the objective lens. During the test, the objective lens pole shoe has a large excitation current. If the sample to be tested is a magnetic sample that has not been specially treated, the micro-nano particles can easily break away from the carrier grid and adsorb onto the objective lens pole shoe, permanently contaminating the optical path of the lens barrel, causing the electron microscope resolution to be greatly reduced and difficult to recover.
[0003] Therefore, magnetic samples need to be pretreated before TEM testing to minimize the risk of magnetic samples adsorbing to the pole piece. Currently, the following methods are commonly used: (1) demagnetizing the sample using a demagnetizer; (2) using a magnet close to the grid to simulate the magnetic field environment in the lens and pre-remove particles that are easy to detach; (3) using a commercially available double-net to wrap the magnetic sample.
[0004] However, the above common methods have some shortcomings. For example, although the demagnetizer can temporarily reduce the magnetism of part of the sample, the sample is easily re-magnetized under the magnetic field generated by the objective lens; and the method of using a magnet to pre-remove some magnetic particles is easy to destroy the active components and functional structure of the material, making the characterization lose its authenticity and comprehensiveness. The method of clamping the magnetic sample with a double network is more reasonable than the first two. Both sheets of the double network are covered with a layer of Fanghua film and a carbon film. When using it, the magnetic material is dispersed on one of the sheets and dried, and then the other sheet is buckled with tweezers. However, the double network still has obvious shortcomings. First, the support film used in the current commercial double network is generally thick, and the two sides of the support film add up to about 60nm. If it is too thin, it is very easy to break in the process of merging the two sheets with tweezers; for smaller nanomagnetic particles, this thickness will cause background interference, making it difficult to obtain clear high-resolution images. On the other hand, the process of buckling the two support films of the double network is easy to cause the support film to break, and it is impossible to ensure the full fixation of the magnetic nanoparticles, and this operation cannot be done in batches. Summary of the invention
[0005] In view of the shortcomings of the existing pretreatment technology, the present invention provides a method and system for pretreatment of magnetic samples for transmission electron microscopy.
[0006] In a first aspect, the present invention provides a method for pretreating a magnetic sample for a transmission electron microscope, wherein the average size of the magnetic sample for a transmission electron microscope is 10 to 100 nm, and the pretreating method comprises the following steps:
[0007] The transmission electron microscope magnetic sample is dispersed in a volatile solvent to prepare a suspension; the suspension is dispersed on a grid and dried to obtain a grid sample; the support frame of the grid is covered with an ultra-thin support film without holes;
[0008] A 5-35 nm thick carbon film is coated on the surface of the grid sample to obtain a sample that can be directly observed under a transmission electron microscope.
[0009] The pretreatment method provided by the present invention can ensure that the nano-magnetic particles with an average size of 10-100nm are not adsorbed onto the pole piece, and the treated sample can obtain a clear high-resolution transmission electron microscope photo. Similarly, the carbon-plated film with a thickness of less than 5nm obtained by the pretreatment method is easy to break, and the transmission electron microscope magnetic sample is easy to be sucked away; the carbon-plated film with a thickness of more than 40nm will produce very obvious background interference.
[0010] In some embodiments provided by the present invention, the thickness of the carbon coating is 10-20 nm. The carbon coating of this thickness has high clarity and can ensure that the magnetic sample of the transmission electron microscope is not sucked away.
[0011] In some embodiments provided by the present invention, the average size of the transmission electron microscopy magnetic sample is 30-60 nm. The transmission electron microscopy magnetic sample is Pt-Co bimetallic nanocrystalline magnetic powder. When the particle size is too small, the carbon coating has a high background interference on the sample, and the clarity of the transmission electron microscopy photo is reduced.
[0012] In some embodiments provided by the present invention, the volatile solvent is one or more of anhydrous ethanol, water, cyclohexane, acetone, and chloroform, preferably anhydrous ethanol.
[0013] In some embodiments provided by the present invention, the support skeleton is one or more of copper, molybdenum, and nickel, preferably copper. The present invention requires that the support film on the surface of the support skeleton has no holes (for example, the micro-grid film has holes), otherwise the magnetic particles cannot be fixed. The type of support film is selected according to the sample. Generally, a support film of ordinary thickness (about 30nm) is selected for micron-level samples, which is not easy to be damaged when carrying the sample. In order to obtain a clear high-resolution image, the present invention selects an ultra-thin carbon film (about 5-10nm thick) as the support film on the surface of the support skeleton to reduce the background effect.
[0014] In some embodiments provided by the present invention, the drying temperature is 20° C. to 80° C. More preferably, the drying temperature is 50° C.
[0015] In some embodiments provided by the present invention, coating a 5-35 nm thick carbon film on the surface of the grid sample includes: placing the pointed conical end of a carbon rod in contact with the flat end of another carbon rod and placing them directly above the grid sample to form a carbon film coating device; placing the carbon film coating device in a vacuum chamber and evacuating the chamber; applying current to the ends of the two carbon rods that are not in contact so that the pointed conical ends of the carbon rods are vaporized and deposited on the surface of the grid sample. The carbon film obtained by this method is flat and uniform, not easy to be damaged during the process, the thickness of the carbon film is controllable, and it can be processed in large quantities. The thin carbon films of dozens to tens of nanometers made by other methods are not easy to transfer, and the method of directly covering the carbon film is difficult to operate and has low efficiency.
[0016] In some embodiments provided by the present invention, the diameters of the two carbon rods are both 5 mm to 20 mm. More preferably, the diameter of the carbon rod is 5 mm.
[0017] In some embodiments provided by the present invention, the vacuum pressure is 1×10 -6 Pa ~ 1×10 -4 Pa. Further preferably, the vacuum pressure is 1×10 -5 Pa.
[0018] In some embodiments provided by the present invention, the distance between the pointed cone end and the grid sample is 5 cm to 20 cm. More preferably, the distance between the pointed cone end and the grid sample is 10 cm.
[0019] In some embodiments provided by the present invention, the current is 30A to 80A. More preferably, the current is 50A.
[0020] In some embodiments provided by the present invention, the time for applying the current each time is 1s to 10s. Further preferably, the time for applying the current each time is 3s.
[0021] In a second aspect, the present invention provides a transmission electron microscope magnetic sample pretreatment system, comprising:
[0022] A sample placement area, which is used to place samples to be coated;
[0023] A first carbon rod having at least one planar end;
[0024] A second carbon rod having at least one conical end; the conical end of the second carbon rod is in contact with the planar end of the first carbon rod, and the conical end is located directly above the sample placement area; the other ends of the first carbon rod and the second carbon rod are connected to a power source; and
[0025] The vacuum chamber is used to provide a vacuum environment when current flows between the first carbon rod and the second carbon rod.
[0026] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0027] The pretreatment method for transmission electron microscope magnetic samples provided by the present invention is aimed at transmission electron microscope magnetic samples with an average size of 10-100nm. Such samples are more easily adsorbed on the pole shoe. Based on the conventional transmission electron microscope sample pretreatment method, the present invention adds a step of carbon film coating, which can firmly fix the transmission electron microscope magnetic samples with an average size of 10-100nm on the carrier net, effectively preventing magnetic particles from falling into the transmission electron microscope pole shoe and damaging the instrument. In addition, the pretreatment method can adjust the thickness of the carbon film by adjusting the number of coating times according to the size and resolution requirements of the sample to obtain clear high-resolution transmission electron microscope photos. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0029] Figure 1 This is a high-resolution transmission electron microscopy photograph of a transmission electron microscopy magnetic sample obtained by pretreatment in Example 1 of the present invention; wherein, Figure 1 A and B show the magnification of 1.5×10 5 , 1.2×10 6 High-resolution transmission electron microscopy image of the sample.
[0030] Figure 2 This is a high-resolution transmission electron microscopy photograph of a transmission electron microscopy magnetic sample obtained by pretreatment in Example 2 of the present invention; wherein, Figure 2 A and B show the magnification of 1.2×10 5 , 1.2×10 6 High-resolution transmission electron microscopy image of the sample.
[0031] Figure 3 Schematic diagram of the carbon film coating device. DETAILED DESCRIPTION
[0032] There are many factors that affect the size of magnetism, such as the properties of the material itself and the particle size. The present invention only discusses the particle size because the properties of the material itself are difficult to quantify. The applicant has made samples of different particle sizes. If the particle size of the transmission electron microscope magnetic sample is ≤5nm, it will generally not be sucked away and can be directly prepared with a grid; if the particle size is too large, for example, greater than 100nm, the field generally uses a double-network clamping method for magnetic samples, because at this time the background effect caused by the thickness of the double network can be ignored relative to the thickness of the particle itself.
[0033] The TEM magnetic sample pretreatment method provided by the present invention is aimed at TEM magnetic samples with an average size of 10-100 nm. Such samples are more easily adsorbed onto the pole piece. The present invention solves the problem that the existing magnetic sample fixing technology cannot obtain high-definition and high-resolution images of nano-scale magnetic particles.
[0034] The pretreatment method of the transmission electron microscope magnetic sample provided by the present invention comprises the following steps: dispersing the transmission electron microscope magnetic sample in a volatile solvent to prepare a suspension; dispersing the suspension on a carrier mesh, drying, and obtaining a carrier mesh sample; the support skeleton of the carrier mesh is covered with an ultra-thin support film without holes; and a 5-35nm thick carbon film is plated on the surface of the carrier mesh sample to obtain a sample that can be directly observed under a transmission electron microscope. The method can fully fix the transmission electron microscope magnetic sample with an average size of 10-100nm, ensuring that it is not adsorbed on the pole shoe, and the carbon film is relatively thin, which has little interference on the sample, and a clear high-resolution transmission electron microscope photo can be obtained when observed under a transmission electron microscope.
[0035] Preferably, the thickness of the carbon film plated on the surface of the grid sample in the present invention is 20% to 50% of the average size of the transmission electron microscope magnetic sample.
[0036] The method for pretreating a magnetic sample for a transmission electron microscope provided in an embodiment of the present invention specifically comprises the following steps:
[0037] (1) Disperse the dried TEM magnetic sample in ethanol to make a suspension, drop a small amount of the suspension on the grid, and dry it to obtain a grid sample;
[0038] (2) Take two carbon rods, grind one end of one of the carbon rods into a pointed cone, i.e., the pointed cone end, and grind one end of the other carbon rod into a flat surface, i.e., the flat surface end; fix the pointed cone end and the flat surface end on a bracket, place them directly above the grid sample, place them together in a vacuum chamber, and evacuate them;
[0039] (3) Apply current to the other end of the two carbon rods that are not in contact and maintain it for a certain period of time, so that the conical end of the carbon rod is vaporized and a layer of carbon film is evenly coated on the surface of the grid sample;
[0040] (4) Reduce the current, cool the carbon rod, release the vacuum, and obtain a carbon film on the grid sample. At this time, the grid sample can be observed under a transmission electron microscope. The thickness of the carbon film can be adjusted by adjusting the number of steps (3) as needed. The thickness of the carbon film in step (3) is about 5~7nm. Repeating 1~5 times can obtain a carbon film with a thickness of 5~35nm.
[0041] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0042] Unless otherwise specified, the Pt-Co bimetallic nanocrystalline magnetic powder used in the present invention is prepared according to the preparation method of platinum alloy nanocore-shell cube disclosed in publication number CN105234427A: platinum acetylacetonate and cobalt acetylacetonate are added to an oleylamine-oleic acid mixed solution, carbon monoxide is introduced to react at 220-235°C, and after the reaction is completed, the product is separated, washed, and dried to obtain Pt-Co bimetallic nanocrystalline magnetic powder. In this preparation method, the molar ratio of platinum acetylacetonate and cobalt acetylacetonate and the reaction time are adjusted to obtain Pt-Co bimetallic nanocrystalline magnetic powders of different particle sizes.
[0043] Unless otherwise specified, the copper grid (200 mesh) with an ultra-thin carbon film on its surface used in the present invention was purchased from Beijing Zhongjing Keyi Technology Co., Ltd.
[0044] Example 1
[0045] The transmission electron microscopy magnetic sample in this embodiment is a Pt-Co bimetallic nanocrystalline magnetic powder with a particle size of 30-40 nm. The transmission electron microscopy magnetic sample pretreatment method provided in this embodiment includes the following steps:
[0046] (1) The transmission electron microscopy magnetic sample was dispersed in ethanol to prepare a 1 mg / mL suspension. A small amount of the suspension was dropped onto a copper grid covered with an ultra-thin carbon film and dried at 50°C to obtain a grid sample.
[0047] (2) Take two carbon rods with a diameter of 5 mm and a length of 100 mm, grind one end of one of the carbon rods into a pointed cone shape, and grind one end of the other carbon rod into a flat surface. Place the pointed cone end and the flat surface end opposite to each other and slightly in contact, fix them on a bracket, and place them 10 mm above the grid sample in step (1). The composition is as follows: Figure 3 The carbon film coating device is placed in a vacuum chamber and evacuated to 1×10 -5 Pa.
[0048] (3) Slowly apply 50A current to both ends of the two carbon rods to vaporize the conical ends of the carbon rods and maintain this current for 3 seconds.
[0049] (4) Repeat step (3) twice, cool the carbon rod, release the vacuum, and obtain a carbon film about 10~15nm thick on the grid sample.
[0050] The sample coated in step (4) was pre-absorbed with a strong neodymium magnet at a distance of 5 mm for 10 minutes to observe whether it was absorbed. It was found that no magnetic sample under the transmission electron microscope was absorbed. The sample was directly observed under the transmission electron microscope. The observation effect was as follows Figure 1 , Figure 1 The lattice fringes of the sample are clearly visible.
[0051] Example 2
[0052] The transmission electron microscopy magnetic sample in this embodiment is a 50-60 nm Pt-Co bimetallic nanocrystalline magnetic powder. The transmission electron microscopy magnetic sample pretreatment method provided in this embodiment includes the following steps:
[0053] (1) The transmission electron microscopy magnetic sample was dispersed in ethanol to prepare a 1 mg / mL suspension. A small amount of the suspension was dropped onto a copper grid covered with an ultra-thin carbon film and dried at 50°C to obtain a grid sample.
[0054] (2) Take two carbon rods with a diameter of 5 mm and a length of 100 mm, grind one end of one of the carbon rods into a pointed cone shape, and grind one end of the other carbon rod into a flat surface. Place the pointed cone end and the flat surface end opposite to each other and slightly in contact, fix them on a bracket, and place them 10 mm above the grid sample in step (1). The composition is as follows: Figure 3 The carbon film coating device is placed in a vacuum chamber and evacuated to 1×10 -5 Pa.
[0055] (3) Slowly apply 50A current to both ends of the two carbon rods to vaporize the conical ends of the carbon rods and maintain this current for 3 seconds.
[0056] (4) Repeat step (3) three times, cool the carbon rod, release the vacuum, and obtain a carbon film about 15~20nm thick on the grid sample.
[0057] The sample coated in step (4) was pre-absorbed with a strong neodymium magnet at a distance of 5 mm for 10 minutes to observe whether it was absorbed. It was found that no magnetic sample under the transmission electron microscope was absorbed. The sample was directly observed under the transmission electron microscope. The observation effect was as follows Figure 2 , Figure 2 The lattice fringes of the sample are clearly visible.
[0058] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for pretreating magnetic samples for transmission electron microscopy, characterized in that: The average size of the transmission electron microscope magnetic sample is 30-60 nm, and the transmission electron microscope magnetic sample is Pt-Co bimetallic nanocrystalline magnetic powder; the pretreatment method comprises the following steps: The transmission electron microscope magnetic sample is dispersed in a volatile solvent to prepare a suspension; the suspension is dispersed on a grid and dried to obtain a grid sample; the support frame of the grid is covered with an ultra-thin support film without holes; the thickness of the ultra-thin support film is 5 to 10 nm; A carbon film with a thickness of 5 to 35 nm is coated on the surface of the grid sample, so that a sample that can be directly observed under a transmission electron microscope is obtained; The method of coating a carbon film with a thickness of 5 to 35 nm on the surface of the grid sample comprises: placing a conical end of a carbon rod in contact with a flat end of another carbon rod and placing them directly above the grid sample to form a carbon film coating device; The carbon film coating device is placed in a vacuum chamber and evacuated; Apply current to the non-contacting ends of the two carbon rods to vaporize the conical ends of the carbon rods and deposit them on the surface of the grid sample. Wherein: the diameters of the two carbon rods are both 5 mm to 20 mm; the vacuum pressure is 1×10 -6 Pa~1×10 -4 Pa; the current is 30A to 80A; the distance between the pointed cone end and the grid sample is 5cm to 20cm; the time for each current application is 1s to 10s.
2. The method for pretreating magnetic samples for transmission electron microscopy according to claim 1, characterized in that: The volatile solvent is one or more of anhydrous ethanol, water, cyclohexane, acetone and chloroform.
3. The method for pretreating magnetic samples for transmission electron microscopy according to claim 1, characterized in that: The supporting skeleton is one or more of copper, molybdenum and nickel.