A kind of hydrophobic polyester fiber and preparation method thereof
By coating a hydrophobic coating of specific compositions on the surface of the polyester fiber to form a hydrophobic layer, the problem of poor waterproof performance of existing polyester fiber fabrics is solved, and higher hydrophobicity and waterproof performance are achieved.
Patent Information
- Application Number
- CN202310571078.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-20
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-05-20
AI Technical Summary
The existing polyester fiber fabrics have average hydrophobic effects and poor durability in terms of waterproofing performance, making it difficult to meet the needs of high-performance waterproofing.
By coating a hydrophobic coating composed of silicone epoxy resin, organic fluororesin, filler, etc. on the surface of the polyester fiber, a hydrophobic layer is formed to enhance the hydrophobic properties of the fiber.
It significantly improves the hydrophobicity and waterproof properties of polyester fibers, enhances the adhesion and stability of the fiber surface, and improves the durability of the waterproof fabric.
Smart Images

Figure BDA0004238632030000061 
Figure BDA0004238632030000071 
Figure BDA0004238632030000072
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of polyester fibers, and more specifically, to a hydrophobic polyester fiber and a preparation method thereof. Background Art
[0002] At present, the quality, quantity and benefits of China's clothing and textile exports are rising year by year. At the same time, clothing consumption patterns are showing a diversified trend, which not only meets the growing needs of consumers, but also promotes the textile industry chain to develop in the direction of technological innovation, green environmental protection and sustainable development, which will inevitably make my country's textile and clothing industry's global market competitiveness continue to improve.
[0003] Currently, most clothing and textiles are made of chemical fiber fabrics, among which polyester fiber is the main one. The biggest feature of polyester fiber is its good elasticity and chemical stability. It will not react with weak acids, weak bases, and oxidants at normal temperatures, so it is widely used.
[0004] In order to expand the scope of use of polyester fabrics, polyester fabrics are usually modified to improve the water and oil repellency of polyester fabrics, and the fabrics are directly waterproofed. This treatment method has a general hydrophobic effect and poor durability. Therefore, there is an urgent need for a polyester fiber with strong hydrophobic properties to weave waterproof fabrics. Summary of the invention
[0005] In order to prepare polyester fibers with strong hydrophobicity, the present application provides a hydrophobic polyester fiber and a preparation method thereof.
[0006] In a first aspect, the present application provides a hydrophobic polyester fiber, which adopts the following technical solution:
[0007] A hydrophobic polyester fiber, characterized in that it consists of polyester fiber and a hydrophobic layer, wherein the hydrophobic layer is formed by coating the polyester fiber surface with a hydrophobic coating and drying it, wherein the hydrophobic coating is mainly made of the following raw materials in parts by weight: 1-2 parts of an organic silicon epoxy resin, 1-2 parts of an organic fluorine resin, 10-20 parts of a filler, 15-25 parts of a solvent, 10-20 parts of an acrylic emulsion, 0.1-0.5 parts of a curing agent, 1-2 parts of a dispersant, and 1-2 parts of an adhesive, wherein the filler is at least three of talcum powder, modified stainless steel honeycomb panel powder, mesh polypropylene fiber, and four-needle zinc oxide whiskers, and a preparation method for the modified stainless steel honeycomb panel powder comprises the following steps: crushing, stirring, and grinding the stainless steel honeycomb panel powder, and immersing the powder in methyl hydrogen silicone oil to obtain the obtained product.
[0008] By adopting the above technical scheme, the organic fluorine resin will cross-link itself into a three-dimensional mesh membrane structure with a relatively smooth surface. The low surface tension of the carbon fluorine in the organic fluorine resin helps to further enhance the hydrophobicity of the hydrophobic layer. The organic silicon epoxy resin and the acrylic emulsion cooperate with each other to jointly enhance the connection stability between the components in the hydrophobic layer. The modified stainless steel honeycomb plate powder in the filler is filled in the mesh of the mesh polypropylene fiber so as to fix the mesh polypropylene fiber on the surface of the polyester fiber. At the same time, the surface of the modified stainless steel honeycomb plate powder contains a waterproof film of silicone oil, which is convenient for further increasing the waterproofness of the polyester fiber. Talc powder and four-needle zinc oxide whiskers are filled in the gaps between adjacent stainless steel honeycomb plate powders to improve the compactness of the hydrophobic layer. Talc powder has an anti-sedimentation effect, which helps to enhance the suspension of other components of the filler in the hydrophobic coating, and facilitates the uniform distribution of the filler in the hydrophobic coating, so as to further improve the stability and hydrophobicity of the hydrophobic layer, thereby improving the hydrophobicity of the hydrophobic polyester fiber.
[0009] Preferably, the filler is composed of talcum powder, modified stainless steel honeycomb panel powder, mesh polypropylene fiber, and four-needle zinc oxide whisker in a mass ratio of (5-6):(2-3):(1-2):(2-3).
[0010] By adopting the above technical scheme, the filler is compounded from four components, namely, talcum powder, modified stainless steel honeycomb panel powder, mesh polypropylene fiber, and four-needle zinc oxide whisker. The ratio of the four components is adjusted to achieve the best ratio. Part of the mesh polypropylene fiber is mixed and interwoven to form the skeleton of the hydrophobic layer, and part of the modified stainless steel honeycomb panel powder is filled in the network structure formed on the surface of the mesh polypropylene fiber. On the one hand, the pore volume in the network structure is reduced and the density of the network structure is improved. On the other hand, the stability of the network structure is enhanced. Part of the talcum powder and part of the four-needle zinc oxide whisker are filled in the gaps in the network structure, the gaps between the network polypropylene fiber and the modified stainless steel honeycomb panel powder, and the gaps between adjacent modified stainless steel honeycomb panel powders, further improving the stability and density of the network structure. At the same time, the whisker part of the four-needle zinc oxide whisker may face the side away from the polyester fiber to further enhance the hydrophobicity of the polyester fiber.
[0011] Preferably, the modified stainless steel honeycomb panel powder is pretreated, and the pretreatment method comprises the following steps: immersing the modified stainless steel honeycomb panel powder in styrene acrylic emulsion, then adding modified nano titanium dioxide, stirring evenly, and drying to obtain the modified nano titanium dioxide. The preparation method of modified nano titanium dioxide comprises the following steps: dissolving titanium dioxide in anhydrous ethanol, mixing with zinc stearate after ultrasonication, and ultrasonication to obtain the modified nano titanium dioxide.
[0012] By adopting the above technical solution, zinc stearate is a substance with low surface energy, and part of the zinc stearate may adhere to the outer surface or honeycomb of the modified stainless steel honeycomb panel powder under the action of styrene acrylic emulsion, so as to further improve the hydrophobicity of the modified stainless steel honeycomb panel powder. Nano titanium dioxide has a small particle size, and part of the titanium dioxide may form a dense and uniform coating on the surface of the modified stainless steel honeycomb panel powder, which helps to improve the hydrophobicity of the coating. At the same time, part of the hydrophobic long-chain alkyl of zinc stearate may be grafted onto the surface of nano titanium dioxide, and the stearate further enhances the hydrophobicity of nano titanium dioxide, thereby enhancing the hydrophobicity of the modified stainless steel honeycomb panel powder.
[0013] Preferably, the mesh polypropylene fiber is a modified mesh polypropylene fiber. The preparation method of the modified mesh polypropylene fiber comprises the following steps: immersing the mesh polypropylene fiber in a styrene-acrylic emulsion, then adding needle-shaped wollastonite, mixing and stirring, and obtaining the modified mesh polypropylene fiber.
[0014] By adopting the above technical scheme, the styrene-acrylic emulsion adheres to the surface of the mesh polypropylene fiber, so as to form a bonding layer on the surface of the mesh polypropylene fiber, so as to facilitate the adhesion of the needle-shaped wollastonite to the mesh polypropylene fiber, so that the surface of the mesh polypropylene fiber becomes rough and uneven, and the needle-shaped wollastonite may form a needle-shaped layer on the surface of the mesh polypropylene fiber, which may cause water molecules to form a rolling effect on the surface of the mesh polypropylene fiber, thereby increasing the contact angle of the mesh polypropylene fiber, increasing the hydrophobicity of the surface of the mesh polypropylene fiber, and thereby increasing the hydrophobicity of the hydrophobic polyester fiber.
[0015] Preferably, the mesh polypropylene fibers are roughened before impregnation.
[0016] By adopting the above technical solution, after the mesh polypropylene fiber is roughened, the surface contact area is increased, which is conducive to the adhesion of more needle-shaped wollastonite, and may increase the density of the needle-shaped layer, which is conducive to further increasing the hydrophobicity of the modified mesh polypropylene fiber, thereby improving the waterproofness of the hydrophobic polyester fiber.
[0017] Preferably, the central body diameter of the four-needle zinc oxide whisker is 0.7-1.4 μm, and the root diameter is 0.1-3 μm.
[0018] By adopting the above technical scheme, the addition of four-needle zinc oxide whiskers helps to enhance the strength of the hydrophobic layer on the one hand, and may be interwoven with the mesh zinc oxide fibers in the hydrophobic layer to further enhance the stability of the network structure; on the other hand, the four needle tips of the four-needle zinc oxide whiskers exhibit a special tip nano effect, which causes water molecules to form a rolling effect on the surface of the four-needle zinc oxide whiskers, so as to improve the impermeability of the hydrophobic layer and further improve the hydrophobicity of the hydrophobic layer.
[0019] Preferably, the dispersant is oxidized polyethylene wax.
[0020] By adopting the above technical scheme, the oxidized polyethylene wax has good thermal stability and low high-temperature volatility. The oxidized polyethylene wax has both excellent external lubricity and strong internal lubricity, and has good compatibility with other components in the raw materials, and can effectively improve the dispersibility of each raw material component in the system.
[0021] Preferably, the silicone resin is a modified silicone epoxy resin, and the preparation method of the modified silicone epoxy resin comprises the following steps: S1 pretreatment of the silicone epoxy resin: dissolving the silicone epoxy resin, adding an organotin catalyst and 4-fluorophenyl isocyanate, and mixing them evenly to obtain a pretreated silicone epoxy resin; S2 preparation of modified calcium carbonate: immersing calcium carbonate in a styrene-acrylic emulsion, and drying to obtain modified calcium carbonate; S3 preparation of the modified silicone epoxy resin: mixing the pretreated silicone epoxy resin obtained in step S1 and the modified calcium carbonate obtained in step S2 to obtain.
[0022] By adopting the above technical scheme, the pretreated silicone epoxy resin obtained by the reaction of 4-fluorophenyl isocyanate and silicone epoxy resin contains phenyl. The electron-rich cloud in the phenyl reacts with the polyester fiber and cooperates with the adhesive to help enhance the adhesion of the hydrophobic layer on the surface of the polyester fiber. The pretreated silicone epoxy resin contains fluorosilicone groups, which further reduces the surface energy of the pretreated silicone epoxy resin. Part of the modified calcium carbonate may fill the pores between the resins, thereby improving the density of the resin.
[0023] Preferably, the talcum powder is modified talcum powder, and the preparation method of the modified talcum powder comprises the following steps: adding talcum powder to silica sol and stirring evenly, then adding cerium oxide powder, and then spraying granulation to obtain the modified talcum powder.
[0024] By adopting the above technical scheme, talcum powder, cerium oxide powder and silica sol are sprayed and granulated. During the process, the water in the silica sol evaporates, and the colloidal particles tightly and firmly bond the talcum powder and cerium oxide powder together. The prepared modified talcum powder has good adhesion and permeability and can be dispersed in the hydrophobic layer. The cerium oxide powder has intrinsic hydrophobicity due to its surface orientation and oxygen vacancy level, so as to further improve the hydrophobicity of the talcum powder, thereby improving the hydrophobicity of the hydrophobic layer and the contact angle of the hydrophobic polyester fiber.
[0025] In a second aspect, the present application provides a method for preparing a hydrophobic polyester fiber, using the following technical solution:
[0026] A method for preparing a hydrophobic polyester fiber comprises the following steps:
[0027] (1) Preparation of hydrophobic coating: mixing organic silicon epoxy resin, organic fluorine resin, adhesive, filler, solvent, acrylic emulsion, curing agent and dispersant to obtain hydrophobic coating;
[0028] (2) Preparation of polyester fiber: The hydrophobic coating prepared in step (1) is coated on the outer layer of the polyester fiber and dried to form a hydrophobic layer.
[0029] By adopting the above technical scheme, the hydrophobic polyester fiber of the present application adopts the method of coating the hydrophobic coating on the surface of the polyester fiber, and wrapping a hydrophobic layer on the surface of the polyester fiber. The process is simple and the obtained hydrophobic polyester fiber has better hydrophobic performance.
[0030] In summary, this application has the following beneficial effects:
[0031] 1. The hydrophobic polyester fiber of the present application is composed of polyester fiber and a hydrophobic layer on the surface. The hydrophobic layer is formed by coating a hydrophobic coating on the surface of the polyester fiber. The silicone epoxy resin and the organic fluorine resin in the hydrophobic coating complement each other. The organic fluorine resin itself is cross-linked into a network membrane structure and distributed on the surface of the hydrophobic layer. The carbon fluorine on the surface of the organic fluorine resin has a low surface tension, which is convenient for improving the hydrophobicity of the hydrophobic layer and the adhesion between the hydrophobic layer and the polyester fiber.
[0032] 2. The hydrophobic coating in the hydrophobic polyester fiber of the present application has a filler added therein, and the four components in the filler cooperate together to enhance the strength and density of the hydrophobic layer, thereby improving the hydrophobicity of the hydrophobic layer, which helps to enhance the hydrophobicity of the hydrophobic polyester fiber. DETAILED DESCRIPTION
[0033] The present application is further described in detail below with reference to the embodiments.
[0034] Preparation example of hydrophobic coating
[0035] Preparation Example 1: A hydrophobic coating, comprising the following raw materials by weight: 1 kg of silicone epoxy resin, 1 kg of organic fluorine resin, 1 kg of adhesive, 10 kg of filler, 15 kg of solvent, 10 kg of acrylic emulsion, 0.1 kg of curing agent, and 1 kg of dispersant, wherein the silicone epoxy resin is commercially available, the organic fluorine resin is commercially available, the adhesive is vinyltrimethoxysilane, and the filler is composed of talcum powder, modified stainless steel honeycomb panel powder, and mesh polypropylene fiber in a mass ratio of 1:1:2. The preparation method of the modified stainless steel honeycomb panel powder comprises the following steps: crushing, stirring and grinding the stainless steel honeycomb panel powder, and immersing it in methyl hydrogen silicone oil to obtain; the shape of the talcum powder is composed of fibrous, flaky, and needle-like in a mass ratio of 2:1:2; the solvent is composed of butanol and carbonate in a mass ratio of 1:1, the acrylic emulsion is composed of pure acrylic emulsion and acetic acid acrylic emulsion in a mass ratio of 1:1, the curing agent is dibenzoyl peroxide, and the dispersant is oxidized polyethylene wax.
[0036] Preparation Example 2: A hydrophobic coating, which differs from Preparation Example 1 in that it includes the following raw materials by weight: 2 kg of silicone epoxy resin, 2 kg of organic fluorine resin, 2 kg of adhesive, 20 kg of filler, 25 kg of solvent, 20 kg of acrylic emulsion, 0.5 kg of curing agent, and 1 kg of dispersant.
[0037] Preparation Example 3: A hydrophobic coating, which differs from Preparation Example 2 in that the filler is composed of talcum powder, modified stainless steel honeycomb plate powder, mesh polypropylene fiber, and four-needle zinc oxide whisker in a mass ratio of 5:2:1:2. The central body diameter of the four-needle zinc oxide whisker is 0.7-1.4 μm, and the root diameter is 0.1-3 μm.
[0038] Preparation Example 4: A hydrophobic coating, which differs from Preparation Example 2 in that the filler is composed of talcum powder, modified stainless steel honeycomb plate powder, mesh polypropylene fiber, and four-needle zinc oxide whisker in a mass ratio of 6:3:2:3. The central body diameter of the four-needle zinc oxide whisker is 0.7-1.4 μm, and the root diameter is 0.1-3 μm.
[0039] Preparation Example 5: A hydrophobic coating, which differs from Preparation Example 2 in that the filler is composed of talcum powder, modified stainless steel honeycomb plate powder, mesh polypropylene fiber, and four-needle zinc oxide whisker in a mass ratio of 1:1:1:1. The central body diameter of the four-needle zinc oxide whisker is 0.7-1.4 μm, and the root diameter is 0.1-3 μm.
[0040] Preparation Example 6: A hydrophobic coating, which differs from Preparation Example 4 in that: the modified stainless steel honeycomb panel powder is pretreated, and the pretreatment method comprises the following steps: immersing the modified stainless steel honeycomb panel powder in a styrene-acrylic emulsion, then adding modified nano titanium dioxide, stirring evenly, and drying to obtain a modified nano titanium dioxide preparation method, comprising the following steps: dissolving titanium dioxide in anhydrous ethanol, mixing with zinc stearate after ultrasonication, and ultrasonication to obtain a modified nano titanium dioxide. Among them, the particle size of nano titanium dioxide is 25nm; the time of two ultrasonications is 1h; the mass ratio of titanium dioxide to zinc stearate is 0.2:1. The mass ratio of titanium dioxide to anhydrous ethanol is 2:10. The solid content of the styrene-acrylic emulsion is 48%.
[0041] Preparation Example 7: A hydrophobic coating, which is different from Preparation Example 6 in that the mesh polypropylene fiber is a modified mesh polypropylene fiber, and the preparation method of the modified mesh polypropylene fiber comprises the following steps: the mesh polypropylene fiber is subjected to a roughening treatment, and then immersed in a styrene-acrylic emulsion, and then needle-shaped wollastonite is added, mixed and stirred, and dried to obtain. The mass ratio of the mesh polypropylene fiber to the needle-shaped wollastonite is 1:8, and the solid content of the styrene-acrylic emulsion is 48%. The roughening treatment method comprises the following steps: placing the mesh polypropylene fiber in an acidic solution for corrosion treatment, the corrosion time is 13s, the acidic solution is a sulfuric acid solution, and the molar concentration of the substance in the sulfuric acid solution is 1mol / L.
[0042] Preparation Example 8: A hydrophobic coating, which differs from Preparation Example 7 in that the silicone resin is a modified silicone epoxy resin, and the preparation method of the modified silicone epoxy resin comprises the following steps: S1 pretreatment of the silicone epoxy resin: dissolving the silicone epoxy resin in xylene, adding an organotin catalyst and 4-fluorophenyl isocyanate, and mixing them evenly to obtain a pretreated silicone epoxy resin; S2 preparation of modified calcium carbonate: immersing calcium carbonate in a styrene-acrylic emulsion, drying, and obtaining modified calcium carbonate; S3 preparation of modified silicone epoxy resin: mixing the pretreated silicone epoxy resin obtained in step S1 and the modified calcium carbonate obtained in step S2. Among them, the mass ratio of the pretreated silicone epoxy resin and the modified calcium carbonate in step S3 is 3:1; the solid content of the styrene acrylic emulsion in step S2 is 48%, the drying temperature is 30°C, the organotin catalyst in step S1 is dibutyltin dilaurate, and the mass ratio of the silicone epoxy resin, the organotin catalyst, and 4-fluorophenyl isocyanate is 100:0.5:4.
[0043] Preparation Example 9: A hydrophobic coating, which is different from Preparation Example 8 in that the talc powder is modified talc powder, and the preparation method of the modified talc powder comprises the following steps: adding talc powder to silica sol and stirring evenly, then adding cerium oxide powder, and then spraying granulation to obtain a hydrophobic coating. The mass ratio of talc powder to cerium oxide powder is 1:5, and the particle size ratio of talc powder to cerium oxide powder is 5:1.
[0044] Example
[0045] Example 1: A hydrophobic polyester fiber, comprising a polyester fiber and a hydrophobic layer, wherein the polyester fiber is a common polyester fiber, and the hydrophobic layer is formed by coating a hydrophobic coating on the surface of the polyester fiber and drying the coating, wherein the preparation example of the hydrophobic coating is shown in Table 1, and the hydrophobic coating is prepared by Preparation Example 1. The coating amount of the hydrophobic coating is 30 g / m 2 .
[0046] The preparation method of the hydrophobic polyester fiber comprises the following steps:
[0047] (1) Preparation of hydrophobic coating: mixing organic silicon epoxy resin, organic fluorine resin, adhesive, filler, solvent, acrylic emulsion, curing agent and dispersant to obtain hydrophobic coating;
[0048] (2) Preparation of polyester fiber: The hydrophobic coating prepared in step (1) is coated on the outer layer of the polyester fiber and dried to form a hydrophobic layer. The coating is performed using a high-speed online coating device.
[0049] Table 1 Examples 1-9 Preparation of hydrophobic coating for hydrophobic polyester fibers
[0050]
[0051]
[0052] Example 2-9: A hydrophobic polyester fiber. The preparation example of the hydrophobic coating is shown in Table 1. The difference from Example 1 is that the preparation example of the hydrophobic coating is different.
[0053] Comparative Example
[0054] Comparative Example 1: A hydrophobic polyester fiber, which is different from Example 1 in that: there is no hydrophobic layer on the surface of the polyester fiber.
[0055] Comparative Example 2: A hydrophobic polyester fiber, which is different from Example 1 in that the filler is talcum powder.
[0056] Comparative Example 3: A hydrophobic polyester fiber, which differs from Example 1 in that an equal amount of talcum powder is used to replace the reticulated polypropylene fiber.
[0057] Comparative Example 4: A hydrophobic polyester fiber, which differs from Example 1 in that an equal amount of talcum powder is used to replace the modified stainless steel honeycomb panel powder.
[0058] Detection Methods
[0059] Hydrophobicity test: The hydrophobic polyester fibers prepared in Examples 1-9 and Comparative Examples 1-4 were fixed flat on a glass slide, and the water contact angles were measured using a static drop method at ambient temperature using a contact angle goniometer in a sessile drop mode. The test results are shown in Table 2.
[0060] Table 2 Performance test of hydrophobic polyester fibers of Examples 1-9 and Comparative Examples 1-4
[0061]
[0062]
[0063] Combining Example 1 and Comparative Example 1, and combining the data in Table 2, it can be seen that the contact angle of the hydrophobic polyester fiber prepared in Example 1 is much larger than the contact angle of the hydrophobic polyester fiber prepared in Comparative Example 1, indicating that the polyester fiber prepared in the present application has better hydrophobicity. The inventors of the present application believe that the hydrophobic layer on the surface of the polyester fiber facilitates enhancing the hydrophobicity of the polyester fiber.
[0064] In combination with Example 1, Comparative Examples 2-4, and the data in Table 2, it can be seen that the contact angle of the polyester fiber prepared in Example 1 is greater than the contact angle of the polyester fiber prepared in Comparative Examples 2-4. The difference between Example 1 and Comparative Examples 2-4 is that the filler in Example 1 is composed of three components: talcum powder, modified stainless steel honeycomb panel powder, and mesh polypropylene fiber. The inventors of the present application believe that the three components in the filler cooperate with each other and cooperate with other components in the hydrophobic coating to improve the strength and density of the hydrophobic layer, and at the same time, improve the hydrophobicity of the hydrophobic layer, thereby improving the hydrophobicity of the hydrophobic polyester fiber.
[0065] In combination with Examples 1-2 and the data in Table 2, it can be seen that the contact angle of the hydrophobic polyester fiber prepared in Examples 1-2 is relatively large. The inventors of the present application believe that: the components of the homemade hydrophobic coating of the present application are coordinated together, and the hydrophobic layer formed on the surface of the polyester fiber has a large contact angle and better hydrophobicity.
[0066] In combination with Examples 2-5 and the data in Table 2, it can be seen that the contact angle of the hydrophobic polyester fiber prepared in Examples 3-4 is greater than the contact angle of the hydrophobic polyester fiber prepared in Examples 2 and 5. The difference between Examples 3-4 and Examples 2 and 5 is that the proportion of each filler component in Examples 3-4 is within a limited range. The inventors of the present application believe that the proportion of each filler component has a great influence on the hydrophobicity of the hydrophobic layer in the hydrophobic polyester fiber and cannot be randomly selected.
[0067] In combination with Example 4 and Example 6, and in combination with the data in Table 2, it can be seen that the contact angle of the polyester fiber prepared in Example 6 is greater than the contact angle of the polyester fiber prepared in Example 4. The difference between Example 6 and Example 4 is that the modified stainless steel honeycomb panel powder in Example 6 is pretreated. The inventors of the present application believe that zinc stearate and nano-titanium dioxide grafted with hard acid are adhered to the surface of the modified stainless steel honeycomb panel powder after pretreatment, which helps to enhance the hydrophobicity of the surface of the modified stainless steel honeycomb panel powder, thereby enhancing the hydrophobicity of the hydrophobic layer and improving the contact angle of the hydrophobic polyester fiber.
[0068] In combination with Examples 6-7 and the data in Table 2, it can be seen that the contact angle of the polyester fiber prepared in Example 7 is greater than the contact angle of the polyester fiber prepared in Example 6. The difference between Example 7 and Example 6 is that the mesh polypropylene fiber in Example 7 is modified and has needle-shaped wollastonite adhered to the surface. The inventors of the present application believe that the needle-shaped wollastonite adhered to the surface of the mesh polypropylene fiber forms a needle tip aggregation layer on the surface of the mesh polypropylene fiber, which is convenient for further enhancing the hydrophobicity of the surface of the mesh polypropylene fiber, thereby enhancing the contact angle of the hydrophobic polyester fiber surface.
[0069] In combination with Examples 7-8 and the data in Table 2, it can be seen that the contact angle of the polyester fiber prepared in Example 8 is greater than the contact angle of the polyester fiber prepared in Example 7. The difference between Example 8 and Example 7 is that the silicone epoxy resin in Example 8 is modified. The inventors of the present application believe that the modified silicone epoxy resin contains phenyl and fluorosilicone groups, which is convenient for enhancing the adhesion between the hydrophobic layer and the polyester fiber, and at the same time, improving the hydrophobicity of the hydrophobic polyester fiber.
[0070] In combination with Examples 8-9 and the data in Table 2, it can be seen that the contact angle of the polyester fiber prepared in Example 9 is greater than the contact angle of the polyester fiber prepared in Example 8. The difference between Example 9 and Example 8 is that the talc powder in Example 9 has been modified. The inventors of the present application believe that: the surface of the modified talc powder is adhered with cerium oxide powder, which helps to further enhance the hydrophobicity of the polyester fiber.
[0071] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A hydrophobic polyester fiber, characterized in that: The invention comprises polyester fiber and a hydrophobic layer, wherein the hydrophobic layer is formed by coating a hydrophobic coating on the surface of the polyester fiber and drying the coating, wherein the hydrophobic coating is mainly made of the following raw materials in parts by weight: 1-2 parts of an organic silicon epoxy resin, 1-2 parts of an organic fluorine resin, 10-20 parts of a filler, 15-25 parts of a solvent, 10-20 parts of an acrylic emulsion, 0.1-0.5 parts of a curing agent, 1-2 parts of a dispersant, and 1-2 parts of an adhesive, wherein the filler comprises talcum powder, modified stainless steel honeycomb plate powder, mesh polypropylene fiber, and four-needle zinc oxide whisker in a mass ratio of (5-6):(2-3):(1-2):(2-3). The preparation method of the modified stainless steel honeycomb plate powder comprises the following steps: crushing, stirring, and grinding the stainless steel honeycomb plate powder, and immersing the powder in methyl hydrogen-containing silicone oil to obtain the modified stainless steel honeycomb plate powder.
2. A hydrophobic polyester fiber according to claim 1, characterized in that: The modified stainless steel honeycomb plate powder is pretreated, and the pretreatment method comprises the following steps: immersing the modified stainless steel honeycomb plate powder in styrene acrylic emulsion, then adding modified nano titanium dioxide, stirring evenly, and drying to obtain the modified nano titanium dioxide. The preparation method of the modified nano titanium dioxide comprises the following steps: dissolving titanium dioxide in anhydrous ethanol, mixing with zinc stearate after ultrasonic treatment, and ultrasonic treatment to obtain the modified nano titanium dioxide.
3. The hydrophobic polyester fiber according to claim 1, characterized in that: The mesh polypropylene fiber is a modified mesh polypropylene fiber. The preparation method of the modified mesh polypropylene fiber comprises the following steps: immersing the mesh polypropylene fiber in styrene-acrylic emulsion, then adding needle-shaped wollastonite, mixing and stirring to obtain the modified mesh polypropylene fiber.
4. A hydrophobic polyester fiber according to claim 3, characterized in that: The mesh polypropylene fibers are roughened before impregnation.
5. The hydrophobic polyester fiber according to claim 1, characterized in that: The central body diameter of the four-needle zinc oxide whisker is 0.7-1.4 μm, and the root diameter is 0.1-3 μm.
6. The hydrophobic polyester fiber according to claim 1, characterized in that: The dispersant is oxidized polyethylene wax.
7. The hydrophobic polyester fiber according to claim 1, characterized in that: The organosilicon epoxy resin is a modified organosilicon epoxy resin. The preparation method of the modified organosilicon epoxy resin comprises the following steps: S1 pre-treating the organosilicon epoxy resin: dissolving the organosilicon epoxy resin, adding an organotin catalyst and 4-fluorophenyl isocyanate, and mixing them evenly to obtain the pre-treated organosilicon epoxy resin; S2 preparing modified calcium carbonate: immersing calcium carbonate in a styrene-acrylic emulsion, and drying to obtain modified calcium carbonate; S3 preparing the modified organosilicon epoxy resin: mixing the pre-treated organosilicon epoxy resin obtained in step S1 and the modified calcium carbonate obtained in step S2 to obtain.
8. The hydrophobic polyester fiber according to claim 1, characterized in that: The talcum powder is modified talcum powder. The preparation method of the modified talcum powder comprises the following steps: adding talcum powder to silica sol and stirring evenly, then adding cerium oxide powder, and then spraying and granulating to obtain the modified talcum powder.
9. A method for preparing the hydrophobic polyester fiber according to any one of claims 1 to 8, characterized in that: The steps include: (1) Preparation of hydrophobic coating: uniformly mixing silicone epoxy resin, organic fluorine resin, adhesive, filler, solvent, acrylic emulsion, curing agent and dispersant to obtain a hydrophobic coating; (2) Preparation of polyester fiber: The hydrophobic coating prepared in step (1) is coated on the outer layer of the polyester fiber and dried to form a hydrophobic layer.
Citation Information
Patent Citations
Strong-hydrophobicity clothes and preparation method
CN114622420A
Efficient hydrophobic polyester master batch as well as preparation method and application thereof
CN117603559A
Hydrophobic polyester fiber and preparation method thereof
CN118029002A
Hydrophobic slurry, liquid diode, preparation methods therefor and applications thereof
WO2022252275A1