Polycrystalline silicon rod, method for manufacturing polycrystalline silicon rod, and heat treatment method for polycrystalline silicon
By heating the silicon core wire in the presence of chlorosilane compounds and hydrogen and heat treatment in hydrogen, argon and helium gas, the surface temperature and gas flow of the polycrystalline silicon rod are controlled, and the high impurity concentration and deformation near the surface of the polycrystalline silicon rod are solved. The problem of high rate improves overall purity and reduces collapse rate.
Patent Information
- Application Number
- CN202180078110.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-11-27
- Filing Date
- 2021-09-01
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-09-01
AI Technical Summary
During the high-temperature heat treatment process of existing polycrystalline silicon rods, the concentration of impurities near the surface is higher, resulting in a decrease in purity and a higher internal deformation rate and collapse rate.
By heating the silicon core wire in the presence of chlorosilane compounds and hydrogen, and heat treatment in the presence of hydrogen, argon and helium gas, the surface temperature of the polycrystalline silicon is controlled between T1+30℃ and T1+100℃. And it is less than 1030°C, and the gas flow rate is adjusted in the heat treatment process to reach F1/S ≥ 20Nm3/hr/m2 to reduce the impurity concentration and deformation rate.
The overall purity of the polycrystalline silicon rod is improved and the internal deformation rate and collapse rate are reduced, thereby enhancing the manufacturing yield rate.
Smart Images

Figure CN116490461B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a polycrystalline silicon rod, a method for manufacturing the polycrystalline silicon rod and a method for heat treating polycrystalline silicon. Background Art
[0002] As a method for producing polycrystalline silicon, the Siemens method (Siemens method: bell jar method) is known. In the Siemens method, a raw material gas containing a chlorosilane compound and hydrogen is supplied to the reactor while a core wire for silicon precipitation (hereinafter referred to as a "silicon core wire") is electrically heated inside a reactor, thereby precipitating polycrystalline silicon on the surface of the silicon core wire. Patent document 1 discloses a technology for reducing deformation of polycrystalline silicon by heat treatment after precipitation of polycrystalline silicon using the Siemens method.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent No. 3357675 Summary of the invention
[0006] Problems to be solved by the invention
[0007] However, according to the technology disclosed in Patent Document 1, it is necessary to heat the polycrystalline silicon rod until the surface temperature reaches a high temperature of 1030 degrees or more. Therefore, there is a risk that the concentration of impurities in the polycrystalline silicon rod, especially in the portion near the surface, will increase. In other words, the purity of the portion near the surface of the polycrystalline silicon rod will decrease. In addition, "purity" refers to the degree to which the content of impurities in any portion of the polycrystalline silicon rod is low.
[0008] One aspect of the present invention has been made in view of the above-mentioned problems, and an object of the present invention is to improve the purity of the entire polycrystalline silicon rod by improving the purity of a portion near the surface of the polycrystalline silicon rod.
[0009] Means for solving problems
[0010] In order to solve the above-mentioned problems, one aspect of the present invention relates to a polycrystalline silicon rod, wherein an outer total concentration obtained by summing up the concentrations of iron, chromium and nickel in a portion radially from a surface parallel to a central axis to a depth of 4 mm is less than 100 pptw, and if the total concentration obtained by summing up the concentrations of iron, chromium and nickel in a portion radially away from the surface by more than 4 mm is set as an inner total concentration, then the ratio of the outer total concentration to the inner total concentration is greater than 1.0 and less than 2.5.
[0011] In order to solve the above-mentioned problems, one aspect of the present invention relates to a method for manufacturing a polycrystalline silicon rod, which includes: a precipitation process, in which polycrystalline silicon is precipitated on the surface of a silicon core wire by heating the silicon core wire in the presence of a chlorosilane compound and hydrogen; and a heat treatment process, in which the polycrystalline silicon precipitated in the precipitation process is heat-treated in the presence of at least one gas selected from hydrogen, argon and helium. If the surface temperature of the polycrystalline silicon at the moment when the current value of the current flowing through the silicon core wire begins to decrease when the silicon core wire is heated in the precipitation process is set to T1, then the surface temperature T2 of the polycrystalline silicon in the heat treatment process includes a period of more than T1+30°C and less than T1+100°C, and is less than 1030°C.
[0012] In order to solve the above-mentioned problems, one aspect of the present invention relates to a method for heat treating polycrystalline silicon, which includes a heat treatment step, in which the polycrystalline silicon is heat treated inside a straight body portion of a reactor in the presence of at least one gas selected from hydrogen, argon and helium. In the heat treatment step, if the flow rate of the gas (first annealing gas) flowing into the reactor is set to F1, and the cross-sectional area of the straight body portion is set to S, then the step includes a value of F1 / S reaching 20Nm 3 / hr / m 2 The above period.
[0013] Effects of the Invention
[0014] According to one aspect of the present invention, the purity of the entire polycrystalline silicon rod can be improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 This is a diagram schematically showing a polycrystalline silicon rod according to one embodiment of the present invention.
[0016] Figure 2 This is a diagram showing a sample according to one embodiment of the present invention.
[0017] Figure 3 Yes means Figure 1 FIG. 1 is a flow chart of an example of a method for manufacturing a polycrystalline silicon rod.
[0018] Figure 4 Yes means Figure 3 A graph showing an example of the flow rate of hydrogen in each step of the manufacturing method shown.
[0019] Figure 5 It means manufacturing Figure 1 A schematic diagram of a reactor used for producing polycrystalline silicon rods is shown. DETAILED DESCRIPTION
[0020] Next, an embodiment of the present invention will be described. In addition, in this specification, for numerical values X and Y (where X < Y) other than the component numbers, "X to Y" means "X or more and Y or less".
[0021] [Polysilicon rod]
[0022] Use Figure 1 The polysilicon rod 1 according to an embodiment of the present invention will be described. As Figure 1 shown, the polysilicon rod 1 is formed by a silicon core wire 10 and polysilicon 20 deposited around the silicon core wire 10. In addition, the outer shape of the polysilicon rod 1 is cylindrical. Such a polysilicon rod 1 can be manufactured, for example, by the Siemens method.
[0023] In Figure 1 the example shown, the polysilicon rod 1 obtained by cutting the polysilicon 20 deposited around the silicon core wire 10 into a specified length is shown. The diameter of the polysilicon rod 1 is not particularly limited, and the polysilicon rod 1 can be, for example, a large diameter of 100 mm or more.
[0024] When the diameter is 100 mm or more, in a general polysilicon rod, the impurity content in the outer part is likely to be more than that in the inner part. However, in the polysilicon rod 1, the impurity content in the outer part can be effectively reduced, and finally the purity of the whole polysilicon rod 1 can be improved. Moreover, when the diameter is 100 mm or more, in a general polysilicon rod, the internal deformation rate tends to increase and the collapse rate tends to increase. However, in the polysilicon rod 1, the internal deformation rate and even the collapse rate can be reduced compared with the prior art. In addition, the upper limit of the diameter of the polysilicon rod 1 is not particularly limited, but is preferably 200 mm or less, more preferably 150 mm or less. In addition, the length of the polysilicon rod 1 is not particularly limited, but is preferably about 150 cm to 250 cm.
[0025] In the polysilicon rod 1, the total outer concentration C1 obtained by summing the concentrations of iron, chromium, and nickel in the portion from the surface 21 parallel to the central axis AX to a depth of 4 mm in the radial direction (hereinafter referred to as "the portion near the surface 21") is 100 pptw or less. As Figure 1 shown, the central axis AX of the polysilicon rod 1 coincides with the central axis of the silicon core wire 10. In this specification, the direction orthogonal or substantially orthogonal to the central axis of the polysilicon rod 1 is defined as the "radial direction". Iron, chromium, and nickel are all impurities contained in the polysilicon rod 1. Hereinafter, iron, chromium, and nickel are sometimes collectively referred to as "impurities". In addition, from the viewpoint of further improving the purity of the portion near the surface 21, the total outer concentration C1 is preferably 80 pptw or less, more preferably 60 pptw or less.
[0026] In addition, in the polycrystalline silicon rod 1, the ratio of the outer total concentration C1 to the inner total concentration C2, i.e., C1 / C2, is 1.0 to 2.5. The inner total concentration C2 is a value obtained by summing the concentrations of iron, chromium, and nickel in a portion of the polycrystalline silicon rod 1 that is more than 4 mm away from the surface 21 in the radial direction (hereinafter referred to as the "portion on the central axis AX side"). The present inventors have found that the outer total concentration C1 tends to be higher than the inner total concentration C2, and the above numerical range is the understanding obtained by the present inventors after in-depth research on this basis.
[0027] In the polycrystalline silicon rod 1, by setting C1 / C2 to 1.0 to 2.5, the purity of the entire polycrystalline silicon rod 1 can be improved. In addition, from the viewpoint of further improving the purity of the entire polycrystalline silicon rod 1, C1 / C2 is preferably 2.0 or less, and more preferably 1.5 or less. For the same reason, the total concentration C2 inside the polycrystalline silicon rod 1 is preferably 60 pptw or less, and more preferably 40 pptw or less.
[0028] The internal deformation rate of the polycrystalline silicon rod 1 in the radial direction is less than 1.0×10 -4 cm -1 . Therefore, the collapse rate of the polycrystalline silicon rod 1 can be reduced compared with the past. The internal deformation rate is limited by a known definition and can be calculated by a known method. For example, the internal deformation rate can be calculated by the method disclosed in paragraph 20 of item 6 to paragraph 10 of item 7 of patent document 1. In addition, the definition disclosed in paragraphs 11 to 30 of item 7 of patent document 1 is the definition of the internal deformation rate. In addition, when the polycrystalline silicon rod 1 is used as a raw material for pulling a single crystal by recharging, etc., in order to achieve that the rod is not prone to cracking even if it is directly supplied to the reactor 100 described below, the internal deformation rate of the polycrystalline silicon rod 1 is preferably 9.0×10 -5 cm -1 the following.
[0029] <Calculation Method of the Outside Total Concentration and Inside Total Concentration of Polycrystalline Silicon Rod>
[0030] Next, use Figure 1 and Figure 2 , the calculation method of the outer total concentration and the inner total concentration of the polycrystalline silicon rod 1 is described. The outer total concentration C1 and the inner total concentration C2 of the polycrystalline silicon rod 1 can be calculated, for example, by the following method.
[0031] First, take out the polycrystalline silicon rod 1 Figure 1Specifically, the core rod 30 is taken out from the polycrystalline silicon rod 1 at a predetermined position in the height direction based on either the first end face 211 or the second end face 212, substantially perpendicularly to the central axis AX. As the "predetermined position in the height direction", for example, the center position in the height direction of the polycrystalline silicon rod 1 can be cited.
[0032] The core rod 30 has a cylindrical shape and includes a portion 11 of the silicon core wire 10. The removal method can be a known method, for example, the removal method described in ASTM F1723-96 "Standard Practice for Evaluation Silicon Rods by Float-Zone Crystal Growth and Spectroscopy; Standard Practice for Evaluation of Polycrystalline Silicon Rods by Float-Zone Crystal Growth and Spectroscopy".
[0033] In addition, in the present embodiment, the portion according to the method described in ASTM F1723-96 is only the portion of taking out the core rod 30 from the polycrystalline silicon rod 1. Specifically, first, a hole is drilled in the polycrystalline silicon rod 1 obtained by precipitating polycrystalline silicon 20 on the silicon core wire 10, thereby taking out a cylinder (core rod 30) having a diameter of 20 mm.
[0034] Both end faces 31 of the core rod 30 are part of the surface 21 of the polycrystalline silicon rod 1 and are formed into curved surfaces corresponding to the shape of the surface 21. The diameter of the core rod 30 is not particularly limited and can be set arbitrarily. In this embodiment, the diameter of the core rod 30 is about 20 mm.
[0035] Then, if Figure 2 As shown in the figure, a roughly disk-shaped rod piece with a maximum thickness of about 4 mm is cut out from the end face 31 side of the mandrel 30 substantially perpendicularly to the central axis (not shown) of the mandrel 30. The surface of the rod piece opposite to the cut surface is the end face 31 of the mandrel 30. In addition, the maximum thickness of the rod piece is the shortest distance from the most protruding top edge of the end face 31 to the cut surface. Hereinafter, the rod piece including the end face 31 is referred to as the "skin rod piece 32".
[0036] Furthermore, three disc-shaped rod pieces with a thickness of about 4 mm are cut from the cut surface side of the core rod 30 after the outer skin rod piece 32 is cut by the same method as described above. Hereinafter, these three rod pieces are referred to as "first rod piece 33, second rod piece 34, and third rod piece 35" in the order of cutting from the earliest to the latest. In addition, the outer skin rod piece 32 and the first rod piece 33, the second rod piece 34, and the third rod piece 35 are collectively referred to as "measurement rod pieces 32 to 35". In addition, the number of measurement rod pieces is not particularly limited except that the outer skin rod piece 32 is included.
[0037] A diamond cutter is an example of a tool used when manufacturing the measuring rod pieces 32 to 35 by cutting the core rod 30. The blade of the diamond cutter has a thickness of, for example, 0.7 to 1.2 mm and requires a cutting margin of about 1.5 mm.
[0038] The outer skin rod piece 32 corresponds to the portion of the polycrystalline silicon rod 1 from the surface 21 along the radial direction of the polycrystalline silicon rod 1 (the central axis direction of the core rod 30) to a depth of 4 mm. In addition, the first rod piece 33, the second rod piece 34, and the third rod piece 35 correspond to the portion of the polycrystalline silicon rod 1 that is more than 4 mm away from the surface 21 along the radial direction of the polycrystalline silicon rod 1. In addition, the maximum thickness of the outer skin rod piece 32 and the thickness of each of the first rod piece 33, the second rod piece 34, and the third rod piece 35 may not be about 4 mm. Their thickness may be 3 mm to 10 mm, preferably 4 mm to 6 mm.
[0039] In the present embodiment, the total concentration of the concentrations of the impurities contained in the outer skin rod piece 32 is equivalent to the total concentration C1 of the outer side of the polycrystalline silicon rod 1. Here, the basis for defining the outer skin rod piece 32 as a portion extending from the surface 21 along the radial direction of the polycrystalline silicon rod 1 to a depth of about 4 mm (hereinafter referred to as "a portion extending to a depth of about 4 mm") will be described in detail below.
[0040] The outer skin bar piece 32 is curved so that the surface of the outer skin side portion thereof protrudes outward. Therefore, the outer skin bar piece 32 is cut to a depth of about 4 mm based on the most outwardly protruding portion of the outer skin side portion (the radial center portion of the outer skin bar piece 32). Therefore, the thickness (maximum thickness) of the radial center portion of the outer skin bar piece 32 is about 4 mm.
[0041] The outer skin rod piece 32 is produced by cutting it in a direction parallel to the central axis of the polycrystalline silicon rod 1. Therefore, the thickness of the outer skin rod piece 32 becomes thinner as it moves from the radial center of the outer skin rod piece 32 toward the peripheral direction of the outer skin rod piece 32 (the circumferential direction of the polycrystalline silicon rod 1). For example, when the diameter of the polycrystalline silicon rod 1 is 100 mm (the radius is 50 mm), if the core rod 30 with a diameter of 20 mm is taken out, the thickness of the end of the outer skin rod piece 32 becomes about 3 mm. In addition, since the outer skin of the polycrystalline silicon rod 1 is not smooth, the surface roughness (Ra) needs to be considered. Normally, the surface roughness (Ra) of the outer skin of the polycrystalline silicon rod 1 is about 1 mm. In other words, there is a thickness unevenness of about 1 mm on the outer skin rod piece 32.
[0042] Considering the shape of the polycrystalline silicon rod 1 as described above and the cutting using the blade of the diamond cutter, by selecting the outer skin rod piece 32 as the portion up to a depth of about 4 mm, the outer total concentration C1 can be stably and accurately determined. For example, when the outer skin rod piece 32 is selected as the portion up to a depth of about 2 mm or less, considering that the surface of the outer skin side portion of the polycrystalline silicon rod 1 is convex and the surface roughness (Ra) of the surface, the diamond cutter is easily broken and damaged during cutting. Therefore, the outer skin rod piece 32 cannot be stably produced. On the other hand, for example, when the outer skin rod piece 32 is selected as the portion up to a depth of about 6 mm or more, it will become a form in which the actual impurity amount of the contaminated outer skin side portion is diluted, which is not suitable for quality evaluation. Therefore, in the present embodiment, the outer skin rod piece 32 is selected as the portion up to a depth of about 4 mm.
[0043] After the measuring rod pieces 32 to 35 are prepared as described above, the impurity concentration is measured for each of the measuring rod pieces 32 to 35. In the following description, the method of measuring the concentration of impurities contained in the outer skin rod piece 32 is described as an example. The concentration of the first rod piece 33, the second rod piece 34, and the third rod piece 35 is also measured by the same method.
[0044] First, the entire surface of the outer skin rod piece 32 is etched away by about 100 μm using a nitric-fluoric acid solution, thereby suppressing processing contamination when removing the core rod 30 and cutting the outer skin rod piece 32. Next, the outer skin rod piece 32 is washed with water and dried, and the mass of the outer skin rod piece 32 is measured. Then, the outer skin rod piece 32 is completely dissolved in a predetermined amount of nitric-fluoric acid solution (for example, 200 ml of nitric acid and 200 ml of hydrofluoric acid), and the mass of each of iron, chromium and nickel contained in the solution is measured using a known inductively coupled plasma mass spectrometer (ICP-MS). The analysis using ICP-MS is performed in accordance with, for example, JIS General Rules (JIS K 01332007JIS; General Rules for High Frequency Plasma Mass Analysis).
[0045] Next, the obtained measurement results are used to calculate the concentration of impurities contained in the outer skin rod piece 32. Specifically, the concentration of each of iron, chromium and nickel is calculated by dividing the mass of each of iron, chromium and nickel by the mass of the outer skin rod piece 32. Then, the concentration of impurities in the outer skin rod piece 32 is calculated by adding up these concentrations.
[0046] In other words, the impurity concentration thus calculated is the total concentration obtained by summing up the concentrations of iron, chromium, and nickel contained in the outer rod piece 32. That is, the impurity concentration of the outer rod piece 32 is the outer total concentration C1. Based on this idea, in this embodiment, the inner total concentration C2 is set to a value obtained by averaging the concentrations of impurities in the first rod piece 33, the second rod piece 34, and the third rod piece 35. In addition, when the concentrations of impurities in the first rod piece 33, the second rod piece 34, and the third rod piece 35 are substantially the same value, the concentration of impurities in any one of the first rod piece 33, the second rod piece 34, or the third rod piece 35 can be set to the inner total concentration C2.
[0047] [Manufacturing method of polycrystalline silicon rod]
[0048] Next, use Figure 3 to Figure 5 , a method for manufacturing a polycrystalline silicon rod 1 according to an embodiment of the present invention is described. Figure 3 and Figure 4 As shown, the method for manufacturing the polycrystalline silicon rod 1 includes: a precipitation step S1 , a heat treatment step S2 , and a cooling step S3 .
[0049] In addition, Figure 4 On the horizontal axis of the graph shown, the point t1 at which the precipitation step S1 ends is used as a reference, in other words, the point t1 at which the heat treatment step S2 starts is used as a reference, and the operation points before and after (points t2 to t9) are plotted. The unit of the horizontal axis is the elapsed time t〔min.〕(minutes) from the start time of the precipitation step S1. In the manufacture of the first to third samples and the manufacture of the comparative sample, the supply amount of the raw material gas, the first hydrogen gas and the second hydrogen gas, and the current value are controlled as follows Figure 4 As shown in the graph, the surface temperature of the polysilicon 20 in each process is adjusted to Figure 4 The details of the first to third samples, the comparative sample, the raw material gas, the first hydrogen gas, and the second hydrogen gas will be described below.
[0050] In addition, in this embodiment, the precipitation step S1 and the heat treatment step S2 are performed continuously. Therefore, the time when the supply amount of the raw material gas starts to decrease, i.e. Figure 4 Point t1 in the graph of is the time when the precipitation step S1 is completed and the time when the heat treatment step S2 is started. Figure 4 Point t9 in the graph is the time when the heat treatment step S2 ends and the time when the cooling step S3 starts.
[0051] <Precipitation process>
[0052] First, in the precipitation step S1, polycrystalline silicon 20 is precipitated by a known method (Siemens method). In the Siemens method, generally, Figure 5 The reactor 100 is shown in FIG. The reactor 100 is composed of a straight body 101 and a hemispherical surface formed on the upper side of the straight body 101. Next, the silicon core wire 10 is heated in the presence of a chlorosilane compound and hydrogen inside the straight body 101, so that polycrystalline silicon 20 is precipitated on the surface of the silicon core wire 10. Hereinafter, the gas containing the chlorosilane compound and hydrogen is referred to as "raw material gas". Specifically, the cross-sectional area of the straight body 101 is as follows: Figure 5 As shown in FIG. 1 , when the straight body portion 101 is cut by a virtual plane perpendicular to the central axis AX in the height direction of the polycrystalline silicon rod 1, the inner wall surface (refer to FIG. 1 ) of the straight body portion 101 is Figure 5 The area S of the region enclosed by the dotted line in the figure.
[0053] More specifically, after the silicon core wire 10 is arranged in an inverted U shape inside the straight body 101, the raw material gas is filled into the reactor 100. Specifically, the silicon core wire 10 is opened. Figure 5 The valve 51 shown in the figure supplies the raw material gas to the inside of the reactor 100, thereby filling the reactor 100 with the raw material gas. In the present embodiment, the flow rate of the raw material gas flowing into the reactor 100 is maintained at a predetermined amount before the precipitation step S1 is completed. In other words, the supply amount F of the raw material gas is maintained at a predetermined amount. Next, in this state, a current is passed through the silicon core wire 10 to heat the silicon core wire 10, thereby precipitating polycrystalline silicon 20 on the surface of the silicon core wire 10. The raw material gas supplied to the inside of the reactor 100 and the first hydrogen gas and the second hydrogen gas ( Figure 5 "Supply gas" in ), after being used for the intended purpose, such as Figure 5 As shown, it is discharged from the reactor 100 to the outside.
[0054] also, Figure 5 The structure of the reactor 100 shown is only an example, and the structure of the reactor 100 is not particularly limited. In addition, the reaction conditions in the precipitation step S1 are not particularly limited. As the reactor 100, various well-known reactors can be used, and in the precipitation step S1, the polycrystalline silicon 20 can be precipitated under various well-known reaction conditions.
[0055] When the polycrystalline silicon 20 is deposited on the surface of the silicon core wire 10 in an amount sufficient to obtain the polycrystalline silicon rod 1 of the desired size, the deposition step S1 is completed. The deposition step S1 is completed when the supply amount F of the raw material gas starts to decrease compared to the normal deposition condition (point t1). Figure 4As shown in FIG. 1 , the time from the start of precipitation of the polycrystalline silicon 20 to the moment (point t1) when the precipitation step S1 ends is not particularly limited. The above time can be set to the time until the polycrystalline silicon rod 1 of the desired size is obtained according to the supply amount F of the raw material gas, the temperature when the polycrystalline silicon 20 is precipitated, etc. It is usually 100 hr to 200 hr. With respect to the first to third samples described below and the comparative samples described below, the sizes of the polycrystalline silicon rods are adjusted to be the same.
[0056] <About Preferred Countermeasures in the Precipitation Step / Preparation Before the Heat Treatment Step>
[0057] (About the surface temperature and current value of polysilicon in the precipitation process)
[0058] The end of the deposition step S1 is set to the time when the supply amount F of the raw material gas is reduced (point t1). Here, if the supply amount F of the raw material gas is reduced while the current value of the current flowing through the silicon core wire 10 is kept constant, there is a risk that the surface temperature of the polycrystalline silicon 20 deposited on the silicon core wire 10 will become too high as the supply amount F of the raw material gas is reduced. Therefore, in order to avoid this phenomenon, it is preferred to reduce the current value of the current flowing through the silicon core wire 10 from the time before the end of the deposition step S1 (point t1), that is, from point t2. In other words, it is preferred that the surface temperature of the polycrystalline silicon 20 is gradually reduced by gradually reducing the current value after the polycrystalline silicon 20 is deposited under certain conditions.
[0059] In this embodiment, the surface temperature of the polycrystalline silicon 20 before the current value is reduced is set to T1, which is simply referred to as the surface temperature T1 in the following description. The surface temperature T1 is equivalent to the surface temperature of the polycrystalline silicon 20 when the polycrystalline silicon 20 is normally precipitated. The so-called normal precipitation of polycrystalline silicon 20 refers to the precipitation of polycrystalline silicon 20 when the supply amount F of the raw material gas is a certain amount and the current value is also a certain value.
[0060] Moreover, in the present embodiment, in the subsequent heat treatment step S2, it is important to perform annealing (heat treatment) at a temperature that is 30°C to 100°C higher than the surface temperature T1 and is lower than 1030°C. In addition, the surface temperature T1 is not particularly limited as long as it is a temperature lower than 1000°C and at which the polycrystalline silicon 20 can be precipitated. However, in consideration of the productivity of the polycrystalline silicon 20, the surface temperature T1 is preferably 800°C or higher and lower than 1000°C, and more preferably 900°C or higher and lower than 1000°C.
[0061] Moreover, in the present embodiment, although the current value of the current flowing through the silicon core wire 10 starts to decrease from point t2, the surface temperature of the polycrystalline silicon 20 also starts to decrease from point t2. There is no particular limitation on the surface temperature of the polycrystalline silicon 20 at the time (point t1) when the supply amount F of the raw material gas is reduced. However, from the viewpoint of improving the productivity of the polycrystalline silicon 20 and avoiding excessive heating of the polycrystalline silicon 20, the surface temperature of the polycrystalline silicon 20 at point t1 is preferably a temperature of about 0°C (the same as T1 temperature) to 100°C lower than the surface temperature T1, and more preferably a temperature of about 10°C to 80°C lower than the surface temperature T1.
[0062] Furthermore, there is no particular restriction on point t2. Considering the productivity and quality of the polysilicon 20, point t2 is preferably about 10 to 120 minutes earlier than point t1, and more preferably about 20 to 100 minutes earlier than point t1. In addition, in the first to third samples described below and the comparative samples described below, point t2 is set to a time 60 minutes earlier than point t1. Moreover, the reason for setting point t2 is to suppress the surface temperature of the polysilicon 20 from being too high. If there is no risk of the surface temperature of the polysilicon 20 being too high, there is no need to set point t2.
[0063] (Preliminary supply of annealing gas in the precipitation process)
[0064] In addition, in the precipitation step S1, the first hydrogen gas as the first annealing gas may be supplied to the reactor 100 from point t3 before the end of the precipitation of the polycrystalline silicon 20 (point t1). In the following, although the case where the first annealing gas is hydrogen gas is described as an example, the first annealing gas may be at least one gas selected from hydrogen, argon and helium.
[0065] The first hydrogen gas is used as a part of the hydrogen supplied for the annealing process in the heat treatment step S2, and is supplied separately from the hydrogen gas constituting the raw material gas. Figure 5 The valve 52 shown supplies the first hydrogen gas together with the raw material gas into the reactor 100. Point t3 is set to the same time as point t1 or a time earlier than point t1. However, in order to easily obtain the supply timing of each hydrogen gas and effectively supply the first hydrogen gas, it is preferred to set point t3 to a time earlier than point t1. In addition, regarding point t3, it can be appropriately set in consideration of various devices used to manufacture the polycrystalline silicon rod 1, the desired size of the polycrystalline silicon rod 1, and the precipitation efficiency. Usually, point t3 is set to a time about 5 minutes to 1 hour earlier than point t1.
[0066] Regarding the supply of the first hydrogen gas, although Figure 4In the graph, the supply amount is gradually increased so that the arrival supply amount of the first hydrogen gas becomes f1, but the supply amount can also be changed from 0 (zero) to the arrival supply amount F1 at one time. In this case, point t4 does not exist, in other words, point t4 is replaced by point t3. In addition, in the manufacture of the first to third samples described below and the manufacture of the comparative sample described below, point t3 is set to a time 30 minutes earlier than point t1, and it takes 20 minutes to gradually increase the supply amount of the first hydrogen gas until point t4. In addition, the supply amount of the first hydrogen gas after point t4 is maintained at the arrival supply amount f1. However, for the first to third samples and the comparative sample, the values of their respective arrival supply amounts f1 are different.
[0067] In the precipitation step S1, the second hydrogen gas may be supplied to the reactor 100 from point t5 before the end of the precipitation of the polycrystalline silicon 20 (point t1). Although hydrogen gas is used as an example below, the second hydrogen gas may be at least one of hydrogen, argon and helium.
[0068] The second hydrogen gas is used as a part of the hydrogen supplied for the annealing process in the heat treatment process S2. The second hydrogen gas is preferably used as the second annealing gas in the cooling process S3 and is supplied separately from the hydrogen gas constituting the raw material gas. Figure 5 The valve 53 shown supplies the second hydrogen gas into the reactor 100 together with the raw material gas.
[0069] Point t5 is set to Figure 4 The point t5 is set to be the same as point t1 in or earlier than point t1. However, in order to easily obtain the supply timing of each hydrogen gas and reliably supply the second hydrogen gas, it is preferred to set point t5 to a time earlier than point t1. In addition, regarding point t5, it can be appropriately set in consideration of various devices used to manufacture the polycrystalline silicon rod 1, the desired size of the polycrystalline silicon rod 1, and the precipitation efficiency. Usually, point t5 is set to a time about 1 minute to 30 minutes earlier than point t1.
[0070] The supply amount of the second hydrogen gas is preferably smaller than the supply amount of the first hydrogen gas. Furthermore, in order to further improve the operability related to the supply of the second hydrogen gas, the supply amount of the second hydrogen gas supplied in the precipitation step S1 is preferably set to be the same as the supply amount of the second annealing gas supplied in the cooling step S3. Figure 4 As shown, the reaching supply amount f2 of the second hydrogen gas supplied in the precipitation step S1 is the same as the flow rate F2 of the second annealing gas supplied in the cooling step S3 .
[0071] In this case, in the heat treatment step S2, the total amount of the first hydrogen gas supply amount f1 and the second hydrogen gas supply amount f2 is equal to the flow rate F1 of the first annealing gas. Then, in the cooling step S3 that is performed continuously after the heat treatment step S2, by stopping only the supply of the first hydrogen gas, the supply amount of the second annealing gas in the cooling step S3 becomes the desired amount F2 (= f2).
[0072] Regarding the supply of the second hydrogen gas, Figure 4 In the graph, the supply amount is changed from 0 (zero) to the supply amount f2 at one time. For example, although the supply amount of the second hydrogen gas can be gradually increased until it reaches the supply amount f2, since the supply amount of the second hydrogen gas is smaller than the supply amount of the first hydrogen gas as a whole, it is preferred to reach the supply amount f2 at one time from the perspective of operating efficiency and the like. In addition, in the manufacture of the first to third samples described below and the manufacture of the comparative samples described below, point t5 is set to a time 5 minutes earlier than point t1. In addition, the arrival supply amount f2 of the second hydrogen gas is made the same as the flow rate F2 of the second annealing gas.
[0073] <Heat treatment process>
[0074] Then, if Figure 3 and Figure 4 As shown, after the precipitation step S1 is completed, the heat treatment step S2 is performed. In the heat treatment step S2, the polycrystalline silicon 20 precipitated in the precipitation step S1 is annealed in the presence of an annealing gas (first annealing gas) supplied separately from the raw material gas to the inside of the straight body 101 of the reactor 100. The annealing treatment is a heat treatment to remove the residual stress generated in the polycrystalline silicon 20 by heating the polycrystalline silicon 20 precipitated in the precipitation step S1.
[0075] In this embodiment, the composition and flow rate of the first annealing gas can be changed over time. However, as described above, the first annealing gas used in the heat treatment step S2 does not include hydrogen contained in the raw material gas. In other words, the combination of annealing gases supplied to the reactor 100 separately from the raw material gas is used as the first annealing gas.
[0076] The heat treatment step S2 is a heat treatment step for heat treating the polycrystalline silicon 20 precipitated in the precipitation step S1 in the presence of the first annealing gas. In the heat treatment step S2, the surface temperature T2 of the polycrystalline silicon (hereinafter referred to as "surface temperature T2") is adjusted so that it includes a period of surface temperature T1+30°C or more and surface temperature T1+100°C or less, and is less than 1030°C. In addition, in the following description, although the case of using hydrogen as the first annealing gas is described as an example, if at least one gas selected from hydrogen, argon and helium is used as the first annealing gas, the same result can be obtained.
[0077] In the heat treatment step S2, in order to adjust the surface temperature T2, the supply amount of the first annealing gas, the current value of the current flowing through the silicon core wire 10, etc. are adjusted. Since the surface temperature T2 is above the surface temperature T1+30°C, the internal deformation rate of the polycrystalline silicon 20 precipitated in the precipitation step S1 can be reduced compared with the past. Moreover, the collapse rate of the polycrystalline silicon rod 1 can be reduced compared with the past, and the yield when manufacturing the polycrystalline silicon rod 1 can be improved. Furthermore, since the surface temperature T2 includes a period below the surface temperature T1+100°C and is less than 1030°C, the phenomenon of impurities mixing into the surface of the polycrystalline silicon 20 in the heat treatment step S2 can be reduced. As a result, the purity of the polycrystalline silicon 20 after the heat treatment step S2 can be improved, and ultimately the purity of the polycrystalline silicon rod 1 as a whole can be improved.
[0078] In the manufacture of the first to third samples described below and the manufacture of the comparative sample described below, the surface temperature of the polycrystalline silicon 20 is adjusted so as to rise from the time point t1 and reach the surface temperature T2 at the time point t6 (see Figure 4 ). As long as the surface temperature of the polysilicon 20 reaches T2, the surface temperature T2 must include a period of surface temperature above T1+30°C and below T1+100°C, and is less than 1030°C. However, in reality, before the surface temperature of the polysilicon 20 reaches T2, the surface temperature of the polysilicon 20 includes a period of surface temperature above T1+30°C and below T1+100°C, and is less than 1030°C.
[0079] In addition, the time from point t1 to point t6 is not particularly limited. In other words, the time until the surface temperature of the polycrystalline silicon 20 reaches T2 in the heat treatment step S2 is not particularly limited. However, in order to obtain a higher purity and high-quality polycrystalline silicon rod 1, the above time is preferably as short as possible. Specifically, the above time is preferably 1 min to 30 min, and more preferably 1 min to 10 min. In the manufacture of the first to third samples described below and the manufacture of the comparative sample described below, the above time is set to 5 min.
[0080] In the present embodiment, the subsequent cooling process S3 starts from the moment (point t9) when the power supply to the silicon core wire 10 is stopped. In this case, there is no particular restriction on the time (time from point t6 to point t9) for the surface temperature T2 to reach a period including a surface temperature of more than 30°C and less than 1030°C including a surface temperature of T1+100°C. However, in order to obtain a polycrystalline silicon rod 1 with a higher collapse rate and purity than before, it is preferred to set the above time to 10 min to 180 min. Alternatively, it is more preferred to set it to 20 min to 150 min, and even more preferred to set it to 60 min to 120 min. In the manufacture of the first to third samples described below and the manufacture of the comparative samples described below, the above time is set to 90 min.
[0081] like Figure 4 As shown in FIG. 1 , the supply of the raw material gas is stopped at point t7 in the heat treatment step S2. When the supply of the raw material gas is stopped, for example, only the supply of the chlorosilane compound may be stopped, and the hydrogen gas constituting the raw material gas may be used as a part of the first annealing gas. However, since a high degree of supply control is required, and there is a risk of deterioration in the quality of the polycrystalline silicon rod 1. Therefore, when the supply of the raw material gas is stopped, it is preferred to reduce both the chlorosilane compound and the hydrogen gas and stop both of them completely.
[0082] In addition, the time from point t1 to point t7 is not particularly limited. However, if the supply of the raw gas is stopped instantaneously, there is a risk of poor appearance and quality of the polycrystalline silicon rod 1. On the other hand, if the above time is too long, the precipitation of the polycrystalline silicon 20 will not be completely completed. Therefore, it is preferred to set the above time to 1min to 60min, and more preferably to 3min to 30min. In the manufacture of the first to third samples described below and the manufacture of the comparative sample described below, the above time is set to 15min.
[0083] <Preferred Treatment Method in Heat Treatment Step; Supply of First Annealing Gas>
[0084] Next, the preferred treatment method in the heat treatment step S2 is described. First, preferably, when the precipitation step S1 is about to end, the supply amount of the first hydrogen is set to the arrival supply amount f1, the supply amount of the second hydrogen is set to the arrival supply amount f2, these hydrogen gases are supplied to the reactor 100, and the heat treatment step S2 is started after the precipitation step S1.
[0085] Furthermore, the heat treatment step S2 preferably satisfies the following conditions. That is, if the flow rate of the first annealing gas is set to F1, and the cross-sectional area of the straight body portion 101 of the reactor 100 is set to S (refer to Figure 5 ), the heat treatment step S2 preferably includes a F1 / S value of 20Nm 3 / hr / m 2 During the time from point t1 to point t8, the flow rate F1 of the first annealing gas is the sum of the arrival supply rate f1 and the arrival supply rate f2. That is, during the time from point t1 to point t8, the flow rate F1 of the first annealing gas is the maximum sum of the supply rate of the first hydrogen gas and the supply rate of the second hydrogen gas.
[0086] As mentioned above, the value of F1 / S is 20Nm 3 / hr / m 2 As described above, during the heat treatment process, impurity components generated by components and the like existing inside the reactor 100 can be quickly discharged to the outside of the reactor 100. Therefore, the purity of the polysilicon 20 after the heat treatment process S2 can be improved. In addition, there is no particular restriction on the upper limit of the value of F1 / S. Therefore, even if the hydrogen contained in the raw material gas temporarily remains inside the reactor 100, no adverse effect will be generated. However, in order to reduce the amount of the first annealing gas used to reduce the cost required to implement the heat treatment process S2, it is preferred to set the upper limit of the value of F1 / S to less than 130 Nm 3 / hr / m 2 .
[0087] In addition, in order to use the first annealing gas efficiently, the supply amount of the first hydrogen gas is actually reduced from a time earlier than point t8 in the heat treatment step S2. However, even in this case, since there is a period in the heat treatment step S2 when the total amount of the supply amount f1 and the supply amount f2 reaches the flow rate F1 of the first annealing gas, the value of F1 / S reaches 20 Nm 3 / hr / m 2 The above period.
[0088] In addition, the F1 / S value reaches 20Nm 3 / hr / m 2 The above period (the time from point t1 to point t8) is not particularly limited. However, if the time is too short, the effect of reducing impurities and the effect of suppressing the collapse rate cannot be fully obtained. Therefore, it is preferred to set the above time to more than 10 minutes, and more preferably to more than 30 minutes. On the other hand, considering the effective use of the first annealing gas, the upper limit of the above time is 120 minutes.
[0089] In this embodiment, if Figure 4As shown, from the time of point t8, the supply amount of the first hydrogen gas starts to decrease from the supply amount f1. Here, since the total amount of hydrogen gas supplied to the inside of the reactor 100 decreases after the time of point t8, there is a risk of increasing the surface temperature T2. Therefore, the current amount of the current flowing through the silicon core wire 10 is adjusted so that the surface temperature T2 includes a period of more than the surface temperature T1+30°C and less than the surface temperature T1+100°C and is less than 1030°C.
[0090] In the manufacture of the first to third samples described below and the manufacture of the comparative sample described below, the time from point t1 to point t8 is set to 60 minutes, and it takes 30 minutes to reduce the supply amount of the first hydrogen gas from the final supply amount f1 to 0 (zero). The time when the supply amount of the first hydrogen gas becomes 0 (zero) is the time when the heat treatment step S2 ends, specifically, the time when the current value of the current flowing through the silicon core wire 10 becomes 0 (zero) at point t9. In other words, point t9 is the time when the cooling step S3 starts.
[0091] As described above, in the heat treatment step S2 , by limiting the flow rate F1 of the first annealing gas to a predetermined numerical range, it is possible to obtain the polycrystalline silicon rod 1 having a C1 / C2 value of 1.0 to 2.0.
[0092] Although the preferred method for supplying the first annealing gas in the heat treatment step S2 is illustrated in this embodiment, the treatment method in the heat treatment step S2 is not limited to this method. For example, only the first hydrogen gas can be used as the first annealing gas. For another example, after the supply of the raw material gas is stopped, only hydrogen gas is supplied by the same means as the supply means of the raw material gas, thereby also being able to use the hydrogen gas as part of the first annealing gas. Furthermore, although a high degree of supply control is required, the first annealing gas can also be supplied from the moment (point t1) when the heat treatment step S2 starts.
[0093] <Cooling process>
[0094] Then, if Figure 3 and Figure 4 As shown, after the heat treatment step S2 is completed, a cooling step S3 is performed. In the cooling step S3, the polycrystalline silicon 20 that has been annealed in the heat treatment step S2 is cooled. In this embodiment, the polycrystalline silicon 20 is naturally cooled. Natural cooling is a heat treatment in which the current is stopped from flowing through the silicon core wire 10 and the polycrystalline silicon 20 is placed as it is inside the straight body 101 of the reactor 100.
[0095] However, in order to remove the gas trapped inside the reactor 100, it is preferred that a second annealing gas is also supplied to the reactor 100 in the cooling step S3. The second annealing gas is a gas supplied to the reactor 100 for purging. As the second annealing gas, it is sufficient to be at least one of hydrogen, argon and helium. Although the example cited in the following description is the case where the second annealing gas is hydrogen, other gases can also obtain the same effect. In addition, it can be considered that the second annealing gas can also play a role in completely discharging the raw material gas to the outside of the reactor 100.
[0096] In this embodiment, if Figure 4 As shown, the cooling process S3 starts from the moment when the current value of the current flowing through the silicon core wire 10 becomes 0 (zero), that is, the moment of point t9. Moreover, in the present embodiment, the cooling process S3 is performed continuously following the heat treatment process S2, and at the moment of point t9 when the above-mentioned current value becomes 0 (zero), the supply amount of the first hydrogen gas also becomes 0 (zero). However, this timing is only an example, and the moment when the above-mentioned current value becomes 0 (zero) and the moment when the supply amount of the first hydrogen gas becomes 0 (zero) may also be different. In addition, in the manufacture of the first to third samples described below and the manufacture of the comparative samples described below, the moment when the above-mentioned current value becomes 0 (zero) and the moment when the supply amount of the first hydrogen gas becomes 0 (zero) are set to be simultaneous.
[0097] The cooling step S3 preferably satisfies the following conditions. That is, if the flow rate of the second annealing gas is set to F2, the cooling step S3 preferably includes a value of F2 / S reaching 0.4 Nm 3 / hr / m 2 As a preferred method for supplying the second annealing gas, for example, the following method can be cited: Figure 4 As shown, only by continuing to supply the second hydrogen gas at the final supply amount f2 after the heat treatment step S2, the flow rate F2 of the second annealing gas reaches a certain value.
[0098] As a particularly preferred method for supplying the second annealing gas, for example, the following method can be cited: in the precipitation step S1 and the heat treatment step S2, the second annealing gas is still supplied at a flow rate F2 equal to the second hydrogen gas that reaches the supply amount f2. Figure 4 As shown, the second hydrogen gas is continuously supplied at the final supply amount f2 from the time point t4 in the precipitation step S1. By adopting this method, the second annealing gas can be reliably and easily supplied to the inside of the reactor 100.
[0099] The upper limit of the flow rate F2 of the second annealing gas is not particularly limited, but is preferably less than 4 Nm 3 / hr / m 2 By adopting this upper limit value, the polycrystalline silicon 20 after the heat treatment step S2 can be prevented from being rapidly cooled by the second annealing gas, and the internal deformation rate of the polycrystalline silicon 20 after the cooling step S3 can be reduced compared with the past. As a result, the collapse rate of the polycrystalline silicon rod 1 can be reduced compared with the past, and the yield rate when manufacturing the polycrystalline silicon rod 1 can be improved.
[0100] Furthermore, in the cooling step S3, the value of F2 / S reaches 0.4 Nm 3 / hr / m 2 The above period is not particularly limited, and is, for example, a period until the surface temperature of the polycrystalline silicon rod 1 reaches approximately room temperature (e.g., below 30° C.). In addition, in the manufacture of the first to third samples described below and the manufacture of the comparative sample described below, the cooling step S3 is terminated when the surface temperature of the polycrystalline silicon rod 1 reaches 30° C.
[0101] <Post-processing process>
[0102] After the natural cooling and purging process as described above, the polysilicon 20 in the straight body portion 101 is cooled to approximately room temperature, and the cooling process S3 is completed. Figure 5 The valve 53 shown is closed to stop the supply of the second hydrogen gas, thereby replacing the hydrogen gas with nitrogen gas in the reactor 100. The polycrystalline silicon 20 cooled to approximately room temperature after the cooling step S3 is completed becomes the polycrystalline silicon rod 1 as a final product.
[0103] <Modification>
[0104] The various processes in the precipitation step S1, the heat treatment step S2, and the cooling step S3 are merely examples, and various changes may be adopted. For example, the values of the points t1 to t9, the flow rate F1 of the first annealing gas, and the flow rate F2 of the second annealing gas may be arbitrarily changed within the range that can improve the purity of the entire polycrystalline silicon rod 1 and reduce the collapse rate.
[0105] In addition, as for the composition and flow rate of the annealing hydrogen gas in the heat treatment step S2, the values of the points t1 to t9 may be changed as long as they are within the range that can improve the purity of the entire polycrystalline silicon rod 1 and reduce the collapse rate. In addition, the flow rate F1 of the first annealing gas and the flow rate F2 of the second annealing gas may also be changed. Furthermore, the cooling step S3 is not a necessary step in the manufacture of the polycrystalline silicon rod 1, and the cooling step S3 may be omitted.
[0106] Furthermore, in the heat treatment step S2 and the cooling step S3, the gas flowing into the reactor 100 may not be the hydrogen gas described in this embodiment. In the heat treatment step S2 and the cooling step S3, at least one gas selected from hydrogen, argon and helium may flow into the reactor 100.
[0107] 〔Overview〕
[0108] One aspect of the present invention relates to a polycrystalline silicon rod, wherein an outer total concentration obtained by summing up the concentrations of iron, chromium and nickel in a portion radially from a surface parallel to a central axis to a depth of 4 mm is 100 pptw or less, and if the total concentration obtained by summing up the concentrations of iron, chromium and nickel in a portion radially away from the surface by more than 4 mm is set as an inner total concentration, then the ratio of the outer total concentration to the inner total concentration is greater than 1.0 and less than 2.5.
[0109] According to the above configuration, the total concentration of the outer side of the polycrystalline silicon rod involved in one aspect of the present invention is less than 100 pptw. Therefore, the concentration of impurities (iron, chromium and nickel) in the portion near the surface of the polycrystalline silicon rod can be reduced compared with the past. In other words, the purity of the portion near the surface of the polycrystalline silicon rod can be improved.
[0110] In addition, according to the polycrystalline silicon rod according to one aspect of the present invention, the ratio of the outer total concentration to the inner total concentration is 1.0 or more and 2.5 or less. Therefore, the purity of the entire polycrystalline silicon rod can be improved.
[0111] According to one aspect of the present invention, the polycrystalline silicon rod, wherein the internal deformation rate in the radial direction is less than 1.0×10 -4 cm -1 . According to the above-mentioned structure, the internal deformation rate in the radial direction of the polycrystalline silicon rod involved in one aspect of the present invention (hereinafter sometimes referred to as "internal deformation rate") is lower than the internal deformation rate of the conventional polycrystalline silicon rod. Therefore, the collapse rate (hereinafter referred to as "collapse rate") when manufacturing the polycrystalline silicon rod can be reduced compared with the past. Therefore, it is possible to simultaneously improve the purity of the polycrystalline silicon rod as a whole and reduce the collapse rate.
[0112] The polycrystalline silicon rod involved in one aspect of the present invention has a diameter of 100 mm or more. Generally, the longer the diameter of the polycrystalline silicon rod, in other words, the thicker the polycrystalline silicon rod, the greater its internal deformation rate and the higher the risk of collapse. Moreover, the thicker the polycrystalline silicon rod, the higher the concentration of impurities in the portion near the surface. In view of this point, according to the above-mentioned structure, even if it is a polycrystalline silicon rod with a diameter of more than 100 mm, generally, the concentration of impurities in the portion near the surface is high, and the collapse rate is also high, at least the concentration of the polycrystalline silicon rod as a whole can be improved. In addition, even if it is a polycrystalline silicon rod with a thick diameter as described above, in which the concentration of impurities and the collapse rate are generally high, a polycrystalline silicon rod with a lower risk of collapse than before can be manufactured.
[0113] One aspect of the present invention relates to a method for manufacturing a polycrystalline silicon rod, which includes: a precipitation step, in which polycrystalline silicon is precipitated on the surface of a silicon core wire by heating the silicon core wire in the presence of a chlorosilane compound and hydrogen; and a heat treatment step, in which the polycrystalline silicon precipitated in the precipitation step is heat-treated in the presence of at least one gas selected from hydrogen, argon and helium. If the surface temperature of the polycrystalline silicon at the moment when the current value of the current flowing through the silicon core wire begins to decrease when the silicon core wire is heated in the precipitation step is set to T1, then the surface temperature T2 of the polycrystalline silicon in the heat treatment step includes a period of not less than T1+30°C and not more than T1+100°C, and is less than 1030°C.
[0114] According to the above configuration, since the surface temperature T2 of the polycrystalline silicon in the heat treatment process is T1+30°C or higher, the internal deformation rate of the polycrystalline silicon precipitated in the precipitation process can be reduced compared with the past, and the collapse rate of the polycrystalline silicon rod can be reduced compared with the past. Therefore, the yield rate when manufacturing the polycrystalline silicon rod can be improved.
[0115] In addition, since the surface temperature T2 of the polycrystalline silicon during the heat treatment process is below T1+100°C and less than 1030°C, the phenomenon of being mixed into the surface of the polycrystalline silicon during the heat treatment process can be reduced. Therefore, the purity of the polycrystalline silicon after the heat treatment process can be improved, and the purity of the polycrystalline silicon rod as a whole can be improved.
[0116] On the other hand, if the surface temperature T2 of the polycrystalline silicon is lower than T1+30°C, the annealing effect of removing the internal deformation of the polycrystalline silicon is insufficient, the collapse rate becomes high, and the yield rate when manufacturing the polycrystalline silicon rod tends to decrease. On the other hand, if the surface temperature T2 of the polycrystalline silicon is higher than T1+100°C and is above 1030°C, the concentration of impurities near the surface of the polycrystalline silicon becomes high, and the impurity concentration of the obtained polycrystalline silicon tends to become high.
[0117] According to one aspect of the present invention, the method for manufacturing a polycrystalline silicon rod may be configured as follows: the precipitation step and the heat treatment step are performed inside the straight body portion of the reactor. In the heat treatment step, if the flow rate of the gas (first annealing gas) flowing into the reactor is set to F1, and the cross-sectional area of the straight body portion is set to S, then the step includes the step of: the value of F1 / S reaches 20 Nm 3 / hr / m 2 The above period.
[0118] According to the above structure, since the value of F1 / S is 20Nm 3 / hr / m 2 As described above, during the heat treatment process, impurity components generated by components etc. present inside the reactor can be rapidly discharged to the outside of the reactor. Therefore, the purity of polycrystalline silicon after the heat treatment process can be improved.
[0119] In addition, when hydrogen is used as the first annealing gas, hydrogen as a constituent element of the raw material gas supplied together with trichlorosilane (chlorosilane compound) is not included in the first annealing gas. In addition, there is no particular upper limit on the flow rate F1 of the first annealing gas, but from the viewpoint of reducing the amount of the first annealing gas used, it is preferred that the value of F1 / S be set to less than 130 Nm 3 / hr / m 2 .
[0120] According to one aspect of the present invention, the method for manufacturing a polycrystalline silicon rod may be configured as follows: after the heat treatment step, a cooling step of cooling the polycrystalline silicon is further included. In the cooling step, if the flow rate of the gas (second annealing gas) flowing into the reactor is set to F2, the step includes a value of F2 / S reaching 0.4 Nm 3 / hr / m 2 The above period.
[0121] According to the above structure, since the value of F2 / S is 0.4Nm 3 / hr / m 2 As described above, in the cooling process, impurity components generated by components etc. present inside the reactor can be quickly discharged to the outside of the reactor. Therefore, the purity of polycrystalline silicon after the cooling process can be improved.
[0122] The upper limit of the flow rate F2 of the second annealing gas is not particularly limited, but the value of F2 / S is preferably set to less than 4 Nm 3 / hr / m 2 By setting the value of F2 / S to less than 4Nm 3 / hr / m 2, it is possible to prevent the polysilicon after the heat treatment process from being rapidly cooled by the second annealing gas, and to reduce the internal deformation rate of the polysilicon after the cooling process compared to the past. As a result, it is possible to reduce the collapse rate of the polysilicon rods compared to the past, and further improve the yield rate when manufacturing the polysilicon rods.
[0123] One aspect of the present invention relates to a method for heat treating polycrystalline silicon, comprising a heat treatment step of heat treating the polycrystalline silicon inside a straight body portion of a reactor in the presence of at least one gas selected from hydrogen, argon and helium, wherein in the heat treatment step, if the flow rate of the gas (first annealing gas) flowing into the reactor is set to F1 and the cross-sectional area of the straight body portion is set to S, the step includes: 3 / hr / m 2 The above period.
[0124] [Notes]
[0125] The present invention is not limited to the above-described embodiments and modifications, and various modifications can be made within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in the above-described embodiments and modifications are also included in the technical scope of the present invention.
[0126] [Example]
[0127] Next, an embodiment of the present invention will be described. In addition, in the following description, the condition that the surface temperature T2 during the annealing process includes a period of surface temperature T1+30°C or more and surface temperature T1+100°C or less and is less than 1030°C is referred to as the "first manufacturing condition". Furthermore, the value of F1 / S reaches 20Nm 3 / hr / m 2 More than and preferably less than 130Nm 3 / hr / m 2 This condition is called the "second manufacturing condition". Furthermore, the value of F2 / S is set to 0.4 Nm 3 / hr / m 2 More than and preferably less than 4Nm 3 / hr / m 2 This condition is called the "third manufacturing condition".
[0128] <Sample production>
[0129] First, the polycrystalline silicon rods 1 according to the first to third embodiments of the present invention are manufactured using the same reactor 100 and other manufacturing equipment as those in the above-mentioned embodiment of the present invention, and by the same manufacturing method as that in the embodiment of the present invention. Hereinafter, the polycrystalline silicon rods 1 according to the first to third embodiments of the present invention are referred to as "first to third samples".
[0130] Specifically, as shown in Table 1 below, the surface temperature T1 at the point t2 in the precipitation process S1 is 970° C. in all the first to third samples. In addition, the surface temperature T2 at the point t6 in the heat treatment process S2 is 1010° C. in all the first to third samples. On the other hand, F1 / S and F2 / S in the heat treatment process S2 are different in all the first to third examples.
[0131] Specifically, the first sample was manufactured in a state where only the first manufacturing condition was satisfied, but the second and third manufacturing conditions were not satisfied. The second sample was manufactured in a state where the first and second manufacturing conditions were satisfied, but the third manufacturing condition was not satisfied. The third sample was manufactured in a state where all the first to third manufacturing conditions were satisfied. In addition, the diameters of the first to third samples and the comparative sample were all 120 mm.
[0132] The polycrystalline silicon rod (not shown) involved in the comparative example of the present invention is also manufactured through the same steps as one embodiment of the present invention. Hereinafter, the polycrystalline silicon rod involved in the comparative example of the present invention is referred to as the "comparative sample". In addition, as shown in Table 1 below, when the comparative sample is manufactured, it is manufactured under the same conditions as the third sample except for the first manufacturing condition. The surface temperature T1 of the polycrystalline silicon 20 at point t2 in the precipitation step S1 is 970°C, the same as the first to third samples.
[0133]
Table 1
[0134]
[0135] <Sample Evaluation>
[0136] Next, the outer total concentration C1, the inner total concentration C2, C1 / C2, and the internal deformation rate were calculated for the first to third samples and the comparative sample by the same method as one embodiment of the present invention. The calculation results are shown in Table 1 above. In addition, in Table 1 above, the comprehensive evaluation of "○" indicates that both C1 / C2 and the internal deformation rate are good results. In addition, the comprehensive evaluation of "×" indicates that at least one of C1 / C2 and the internal deformation rate is a bad result.
[0137] "C1 / C2 is a good result" means that C1 / C2 is within the numerical range of 1.0 to 2.5. Therefore, when C1 / C2 is outside the numerical range of 1.0 to 2.5, it becomes "C1 / C2 is a bad result". In addition, "internal deformation rate is a good result" means that the internal deformation rate is less than 1.0×10 -4 cm -1 Therefore, the internal deformation rate is 1.0×10 -4cm -1 The above situation becomes "internal deformation rate is an unfavorable result".
[0138] First, for the first to third samples, the numerical range of C1 / C2 is good compared with the previous polycrystalline silicon rods (comprehensive evaluation is "○"). On the other hand, for the comparative sample, its outer total concentration C1 is in a numerical range (400pptw~600pptw) that is significantly higher than the outer total concentration C1 of the first to third samples, so it becomes a poor result (comprehensive evaluation is "×"). Next, as for the inner total concentration C2, the first to third samples and the comparative sample are all in the same numerical range. From this, it can be confirmed that the inner total concentration C2 is roughly unaffected by the manufacturing conditions.
[0139] On the other hand, regarding the outside total concentration C1, the results calculated using the first to third samples and the comparative sample are different. In particular, the outside total concentration C1 of the comparative sample is in a numerical range (400pptw to 600pptw) that is significantly higher than the outside total concentration C1 of the first to third samples. The main reason for this result is that only the surface temperature T2 of the comparative sample during annealing is 1100°C, which is higher than the surface temperature T2 of the first to third samples during annealing (1010°C).
[0140] Regarding the first to third samples, although the manufacturing conditions other than the surface temperature T2 during the annealing treatment are different, the difference in the numerical range of the outer total concentration C1 between them is almost non-existent compared with the difference between them and the comparative sample. It can be inferred that the surface temperature T2 during the annealing treatment has a great influence on the outer total concentration C1.
[0141] Explanation of symbols
[0142] 1. Polysilicon rod
[0143] 10. Silicon core wire
[0144] 20. Polysilicon
[0145] 21. Surface
[0146] 100. Reactor
[0147] 101. Straight body part
[0148] C1, total concentration outside
[0149] C2, total concentration inside
[0150] F1, flow rate of the first annealing gas (flow rate of at least one gas selected from hydrogen, argon and helium)
[0151] F2, flow rate of the second annealing gas (flow rate of at least one gas selected from hydrogen, argon and helium)
[0152] f1. Arrival supply amount of the first hydrogen
[0153] f2, the second hydrogen supply amount
[0154] T1, surface temperature (the surface temperature of polysilicon at the moment when the amount of chlorosilane compounds and hydrogen begins to decrease)
[0155] T2, surface temperature (surface temperature of polysilicon during heat treatment process)
[0156] S, cross-sectional area
[0157] AX, center axis
Claims
1. A polycrystalline silicon rod, wherein: The total outer concentration obtained by summing up the concentrations of iron, chromium and nickel in the portion from the surface parallel to the central axis to a depth of 4 mm in the radial direction is 100 pptw or less. If the total concentration of the iron, chromium and nickel in a portion radially more than 4 mm away from the surface is taken as the inner total concentration, the ratio of the outer total concentration to the inner total concentration is greater than or equal to 1.0 and less than or equal to 2.
5.
2. The polycrystalline silicon rod according to claim 1, wherein: The internal deformation rate in the radial direction is less than 1.0×10 -4 cm -1 . 3 . The polycrystalline silicon rod according to claim 1 , wherein the polycrystalline silicon rod has a diameter of 100 mm or more.
4. A method for manufacturing a polycrystalline silicon rod, comprising: a precipitation step of heating the silicon core wire in the presence of a chlorosilane compound and hydrogen to precipitate polycrystalline silicon on the surface of the silicon core wire; as well as a heat treatment step of heat-treating the polycrystalline silicon precipitated in the precipitation step in the presence of at least one gas selected from hydrogen, argon and helium, If the surface temperature of the polycrystalline silicon at the moment when the current value flowing through the silicon core wire begins to decrease when the silicon core wire is heated in the precipitation process is set to T1, then the surface temperature T2 of the polycrystalline silicon in the heat treatment process includes a period above T1+30°C and below T1+100°C, and is less than 1030°C.
5. The method for manufacturing a polycrystalline silicon rod according to claim 4, wherein: The precipitation step and the heat treatment step are performed inside the straight body of the reactor, In the heat treatment step, if the flow rate of the gas, i.e., the first annealing gas, flowing into the reactor is set to F1, and the cross-sectional area of the straight body portion is set to S, then the step includes a value of F1 / S reaching 20 Nm 3 / hr / m 2 The above period.
6. The method for manufacturing a polycrystalline silicon rod according to claim 5, wherein: After the heat treatment process, a cooling process of cooling the polysilicon is also included. In the cooling step, if the flow rate of the gas flowing into the reactor, that is, the second annealing gas, is set to F2, the step includes a step in which the value of F2 / S reaches 0.4 Nm 3 / hr / m 2 The above period.