A method for oxidizing high-concentration trivalent arsenic using copper-nickel synergistic catalysis
The copper-nickel synergistic catalytic method is used to oxidize trivalent arsenic in an autoclave, which solves the problems of slow oxidation rate of As(III) and high price of oxidants in the existing technology, and achieves efficient and economical trivalent arsenic treatment, which is suitable for the metallurgical industry. .
Patent Information
- Application Number
- CN202310524373.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-10
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-05-10
AI Technical Summary
When treating high-concentration arsenic waste liquid, the existing technology oxidizes As(III) to As(V) slowly, and commonly used oxidants are expensive or dangerous, making it difficult to effectively treat high-concentration trivalent arsenic materials in the metallurgical industry. .
Using the copper-nickel synergistic catalysis method, materials containing trivalent arsenic are mixed with copper-nickel sulfide, acidity adjusting liquid is added, and oxidation gas is introduced into an autoclave for heating and pressurization to promote the oxidation of trivalent arsenic and generate pentavalent arsenic. valent arsenic and waste acid.
The method is simple and easy to operate, the reagents used are easy to obtain, the reaction does not produce by-products, and the waste acid can be recycled. It is suitable for treating high-concentration trivalent arsenic and has great economic value.
Smart Images

Figure CN116495776B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of hazardous waste treatment, and in particular to a method for using copper-nickel synergistic catalytic oxidation of high-concentration trivalent arsenic. Background Art
[0002] Arsenic is a toxic element that is widely associated with non-ferrous metal minerals. Its single substance and compounds are highly toxic and carcinogenic. Over the past decades, my country's non-ferrous metal industry has flourished. While non-ferrous metal minerals have been widely mined, the problem of arsenic pollution has become increasingly prominent.
[0003] After passing through the nonferrous smelting system, most of the arsenic enters the pyrometallurgical slag, smoke, wet metallurgical wastewater, waste slag and electrolytic anode mud. The commonly used wet arsenic fixation methods, such as lime neutralization, sulfide precipitation, iron-arsenic co-precipitation, scorodite method, etc., are mainly aimed at high arsenic concentration wastewater and are widely used in purifying wet metallurgical wastewater. Generally, for some high-arsenic materials that cannot be stably stored, the arsenic in them can first be made to enter the liquid phase in the form of ions through a wet leaching process to obtain a high-concentration arsenic-containing leaching solution, and then solidified through the above methods, or the arsenic can be made into an arsenic trioxide product. The methods used for wet arsenic fixation or the production of arsenic trioxide are all developed based on As(V) as the main phase. These methods fix arsenic in the form of a pentavalent compound or produce arsenic trioxide by reducing As(V). Because, compared with As(III), As(V) is less toxic and less mobile, and the arsenic precipitating minerals of As(V) are generally more stable. In general, the acidic wastewater produced by acid production, smelting and copper electrolytic refining processes, as well as the solution produced by treating smelting smoke, contain a large amount of As(III). Therefore, before fixing arsenic, the As(III) in them must be oxidized to As(V) in advance.
[0004] In order to increase the oxidation rate of As(III), the oxidation of arsenic in the process of high-arsenic material treatment generally relies on a variety of high-priced and active strong oxidants, such as hydrogen peroxide, permanganate, etc. Oxygen can also be used as an oxidant for arsenic, and it is cheap and easy to prepare, but the reaction is very slow without a catalyst. Common catalysts include manganese dioxide, potassium permanganate, ultraviolet light, etc. The concentration of arsenic-containing wastewater in the metallurgical industry is generally several grams per liter or even tens of grams per liter. At present, the production process that does not use air as an oxidant for oxidation is used. Air is a cheap oxidant, easy to prepare and low in danger. Summary of the invention
[0005] The present invention discloses a method for using copper and nickel to catalyze the oxidation of high-concentration trivalent arsenic, so as to solve any of the above and other potential problems in the prior art.
[0006] In order to solve the above problems, the technical solution of the present invention is: a method for catalytically oxidizing high-concentration trivalent arsenic using copper and nickel, the method specifically comprising the following steps:
[0007] S1) mixing a material containing trivalent arsenic with copper-nickel sulfide, and then adding an acidity regulating liquid to adjust the acidity of the mixed material to obtain a mixed solution;
[0008] S2) placing the mixed solution obtained in S1) in an autoclave, stirring it at a certain speed, introducing an oxidizing gas, heating and pressurizing it, and performing an oxidation reaction under a certain pressure to obtain pentavalent arsenic and waste acid.
[0009] Furthermore, the concentration of trivalent arsenic in the mixed solution in S1) is 5 to 30 g / l;
[0010] Further, the copper ion concentration in the mixed solution is 30 to 50 g / l;
[0011] Further, the concentration of nickel ions in the mixed solution is 3 to 20 g / l;
[0012] Furthermore, the acidity is 50 to 250 g / l.
[0013] Furthermore, the material containing trivalent arsenic in S1) is arsenic sulfide filter cake or arsenous acid.
[0014] Furthermore, the arsenic sulfide filter cake is an arsenic filter cake obtained after sulfidation treatment of waste acid from non-ferrous smelting purification.
[0015] Furthermore, the copper-nickel sulfide is the copper-nickel sulfide in the arsenic sulfide filter cake after the copper smelting flue gas purification treatment or a mixture of copper sulfate and nickel sulfate.
[0016] Furthermore, the acidity regulating liquid in S1) is sulfuric acid.
[0017] Further, the stirring rate in S2) is 100-1000 rpm; the heating temperature is 80-150°C; the amount of the oxidizing gas introduced is 100-1000 Nm 3 / h, pressure is 0.8-1.5Mpa; duration is 1-6h.
[0018] Furthermore, the oxidizing gas is air.
[0019] Furthermore, the oxidation rate of the trivalent arsenic is not less than 40%.
[0020] Furthermore, the waste acid is used as the acidity regulating liquid in S1).
[0021] The present invention can promote the oxidation of trivalent arsenic by adding copper sulfate, nickel sulfate or copper-nickel sulfide in arsenic sulfide filter cake after copper smelting flue gas purification treatment to a high-concentration trivalent arsenic solution or arsenic sulfide filter cake slurry, introducing air into the autoclave to make the reaction system have a high-pressure environment, and heating the autoclave at the same time. Compared with the prior art, the present invention has the following beneficial effects:
[0022] (1) The process is simple, easy to operate, and the equipment required for the reaction has been widely used in industry.
[0023] (2) The reagents copper sulfate and nickel sulfate used are selected from copper-nickel sulfides in the by-products of non-ferrous smelting or the arsenic sulfide filter cake after the purification of copper smelting flue gas. They are easy to obtain in copper smelting enterprises and are inexpensive even if purchased.
[0024] (3) During the implementation process, no other by-products are generated, and there is no loss of copper and nickel. The waste acid generated can be reused, especially in conjunction with the wet process for preparing arsenic trioxide. Copper, nickel and sulfuric acid are added once and can be recycled later without repeated addition.
[0025] (4) This method is suitable for treating high-concentration trivalent arsenic and is suitable for strongly acidic trivalent arsenic solutions. This provides great convenience to the metallurgical industry and is of great significance. Compared with other methods, this method has significant economic value. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 The present invention discloses a schematic flow chart of a method for oxidizing high-concentration trivalent arsenic using copper-nickel coordinated catalysis. DETAILED DESCRIPTION
[0027] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and understandable, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific implementation disclosed below.
[0028] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0029] like Figure 1 As shown, the present invention provides a method for oxidizing high-concentration trivalent arsenic using copper-nickel synergistic catalysis, the method specifically comprising the following steps:
[0030] S1) mixing a material containing trivalent arsenic with copper-nickel sulfide, and then adding an acidity regulating liquid to adjust the acidity of the mixed material to obtain a mixed solution;
[0031] S2) placing the mixed solution obtained in S1) in an autoclave, stirring it at a certain speed, introducing an oxidizing gas, heating and pressurizing it, and performing an oxidation reaction under a certain pressure to obtain pentavalent arsenic and waste acid.
[0032] The concentration of trivalent arsenic in the mixed solution in S1) is 5 to 30 g / l;
[0033] The copper ion concentration in the mixed solution is 30 to 50 g / l;
[0034] The concentration of nickel ions in the mixed solution is 3 to 20 g / l;
[0035] The acidity is 50-250 g / l.
[0036] The material containing trivalent arsenic in S1) is arsenic sulfide filter cake or arsenous acid.
[0037] The arsenic sulfide filter cake is an arsenic filter cake obtained after sulfidation treatment of waste acid from non-ferrous smelting purification.
[0038] The copper-nickel sulfide is the copper-nickel sulfide in the arsenic sulfide filter cake after the copper smelting flue gas is purified, or a mixture of copper sulfate and nickel sulfate.
[0039] The acidity regulating liquid in S1) is sulfuric acid.
[0040] The stirring rate in S2) is 100-1000 rpm; the heating temperature is 80-150°C; the amount of oxidizing gas introduced is 100-1000 Nm 3 / h, pressure is 0.8-1.5Mpa; duration is 1-6h.
[0041] The oxidizing gas is air.
[0042] The oxidation rate of trivalent arsenic is not less than 40%.
[0043] The waste acid is used as the acidity regulating liquid in S1).
[0044] Example 1
[0045] The waste acid was prepared to contain 35.8g / l copper, 5.9g / l nickel, and 179.8g / l acidity (in terms of sulfuric acid), and was mixed with arsenic sulfide filter cake (arsenic 40% on dry basis) at a liquid-solid ratio of 8:1, and then moved into an autoclave, while passing air and increasing pressure and temperature, the temperature in the autoclave was raised to 115°C, the pressure to 1.0MPa, and the solution was stirred at a stirring rate of 900rpm at a uniform speed. After the temperature and pressure were raised, the reaction was maintained for 180min, during which sampling was performed every 30min, and the samples obtained at 30min, 60min, 90min, 120min, 150min and 180min were tested and analyzed. The trivalent arsenic oxidation rates obtained were 16.7%, 42.8%, 52.9%, 67.8%, 83.3%, and 91.7%, respectively.
[0046] Example 2
[0047] According to the conditions of Example 1, the liquid-solid ratio was adjusted to 12:1. After the temperature and pressure were raised, the reaction was maintained for 180 minutes, during which samples were taken every 30 minutes, and the samples obtained at 30 minutes, 60 minutes, 90 minutes, 120 minutes, 150 minutes and 180 minutes were tested and analyzed. The trivalent arsenic oxidation rates were 34.2%, 57.6%, 82.7%, 90.8%, 91.6% and 92.3%, respectively.
[0048] Example 3
[0049] According to the conditions of Example 1, the reaction temperature was controlled at 135°C. After the temperature and pressure were raised, the reaction was maintained for 180 minutes, during which samples were taken every 30 minutes, and the samples obtained at 30 minutes, 60 minutes, 90 minutes, 120 minutes, 150 minutes and 180 minutes were tested and analyzed. The trivalent arsenic oxidation rates were 20.1%, 53.9%, 68.3%, 85.6%, 89.3% and 92.1%, respectively.
[0050] Example 4
[0051] The waste acid was prepared to contain 43.9g / l copper, 10.8g / l nickel, and 200.7g / l acidity (in terms of sulfuric acid), and was mixed with arsenic sulfide filter cake (arsenic 40% on dry basis) at a liquid-solid ratio of 8:1, and then moved into an autoclave, while passing air and increasing pressure and temperature, the temperature in the autoclave was raised to 115°C, the pressure to 1.0MPa, and the solution was stirred at a stirring rate of 900rpm at a uniform speed. After the temperature and pressure were raised, the reaction was maintained for 180min, during which sampling was performed every 30min, and the samples obtained at 30min, 60min, 90min, 120min, 150min and 180min were tested and analyzed. The trivalent arsenic oxidation rates obtained were 18.9%, 50.1%, 68.7%, 79.6%, 86.8%, and 93.7%, respectively.
[0052] Example 5
[0053] The waste acid was prepared to contain 46.8g / l of copper, 3.2g / l of nickel, and 110.9g / l of acidity (in terms of sulfuric acid). It was mixed with arsenic sulfide filter cake (arsenic 40% on dry basis) at a liquid-solid ratio of 8:1, and then moved into an autoclave, while passing air and increasing the pressure and temperature. The temperature in the autoclave was raised to 125°C, the pressure to 1.2MPa, and the solution was stirred at a stirring rate of 900rpm. After the temperature and pressure were raised, the reaction was maintained for 180min, during which samples were taken every 30min, and the samples obtained at 30min, 60min, 90min, 120min, 150min and 180min were tested and analyzed. The trivalent arsenic oxidation rates obtained were 19.8%, 56.9%, 83.6%, 89.3%, 91.8% and 92.9%, respectively.
[0054] The description of the above embodiments is only used to help understand the method of the present application and its core idea; at the same time, for a person skilled in the art, according to the idea of the present application, there will be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.
[0055] For example, certain words are used in the specification and claims to refer to specific components. Those skilled in the art should understand that hardware manufacturers may use different nouns to refer to the same component. This specification and claims do not use differences in names as a way to distinguish components, but use differences in the functions of components as the criteria for distinction. As mentioned throughout the specification and claims, "including" and "comprising" are open-ended terms, so they should be interpreted as "including / including but not limited to". "Approximately" means that within an acceptable error range, those skilled in the art can solve the technical problems within a preset error range and basically achieve the technical effects. The subsequent description of the specification is a preferred embodiment of the present application, but the description is for the purpose of illustrating the general principles of the present application, and is not used to limit the scope of the present application. The scope of protection of the present application shall be subject to that defined in the attached claims.
[0056] It should also be noted that the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a product or system including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such a product or system. In the absence of more restrictions, the elements defined by the sentence "comprises a ..." do not exclude the existence of other identical elements in the product or system including the elements.
[0057] It should be understood that the term "and / or" used in this article is only a description of the association relationship of associated objects, indicating that there can be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.
[0058] The above description shows and describes several preferred embodiments of the present application, but as mentioned above, it should be understood that the present application is not limited to the form disclosed herein, and should not be regarded as excluding other embodiments, but can be used in various other combinations, modifications and environments, and can be modified within the scope of the application concept described herein through the above teachings or the technology or knowledge of the relevant field. The changes and modifications made by those skilled in the art do not deviate from the spirit and scope of the present application, and should be within the scope of protection of the claims attached to the present application.
Claims
1. A method for oxidizing high concentration trivalent arsenic using copper-nickel synergistic catalysis, It is characterized in that The method specifically comprises the following steps: S1) mixing a material containing trivalent arsenic with copper-nickel sulfide, and then adding an acidity regulating liquid to adjust the acidity of the mixed material to obtain a mixed solution; The concentration of trivalent arsenic in the mixed solution in S1) is 5 to 30 g / l; The copper ion concentration in the mixed solution is 30-50 g / l; the nickel ion concentration in the mixed solution is 3-20 g / l; the acidity is 50-250 g / l in terms of sulfuric acid; The copper-nickel sulfide is the copper-nickel sulfide in the arsenic sulfide filter cake after the copper smelting flue gas purification treatment, or the copper-nickel sulfide is a mixture of copper sulfate and nickel sulfate; The acidity regulating liquid is sulfuric acid; S2) placing the mixed solution obtained in S1) in an autoclave, stirring it at a certain speed, introducing an oxidizing gas, heating and pressurizing it, and performing an oxidation reaction under a certain pressure to obtain pentavalent arsenic and waste acid; The stirring rate in S2) is 100-1000 rpm; the heating temperature is 80-150°C; the amount of oxidizing gas introduced is 100-1000 Nm 3 / h, pressure is 0.8~1.5Mpa; duration is 1~6h.
2. The method according to claim 1, It is characterized in that The material containing trivalent arsenic in S1) is arsenic sulfide filter cake or arsenous acid.
3. The method according to claim 1, It is characterized in that The arsenic sulfide filter cake is an arsenic filter cake obtained after sulfidation treatment of waste acid from non-ferrous smelting purification.
4. The method according to claim 1, It is characterized in that The oxidizing gas is air.
5. The method according to claim 1, It is characterized in that The oxidation rate of trivalent arsenic is not less than 40%.
6. The method according to claim 1, It is characterized in that The waste acid is used as the acidity regulating liquid in S1).