A preparation device and method of nylon / polyaniline / polypyrrole composite fiber
Through continuous traction of nylon fiber and four U-shaped device processing, the continuous preparation of nylon/polyaniline/polypyrrole composite fiber is achieved, solving the problems of expensive equipment and cumbersome processing in the prior art, and improving production efficiency and structure Regularity, suitable for industrial applications.
Patent Information
- Application Number
- CN202310490644.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-04
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-05-04
AI Technical Summary
In the prior art, the preparation method of nylon/polyaniline/polypyrrole ternary composite materials has problems such as expensive equipment, complicated template removal, complicated emulsion polymerization process, low interface polymerization yield, irregular structure of ultrasonic polymerization, and difficult to achieve. Large-scale, continuous mass production.
The continuous traction of nylon fiber is carried out through four U-shaped devices for decomposition, aniline surface polymerization, pyrrole surface polymerization, cleaning and drying, so as to achieve the continuous preparation of nylon/polyaniline/polypyrrole composite fiber. The reaction system is full water phase. No templates and organic solvents are required, and the monomer and initiator are mixed with gravity to simplify the post-treatment process.
One-step continuous mass production of nylon/polyaniline/polypyrrole composite fiber is realized, which improves production efficiency, structural regularity, reduces cost and operational complexity, is suitable for industrial production, and has high application potential.
Smart Images

Figure CN116497540B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of preparation of composite fiber materials, and particularly relates to a method for preparing nylon / polyaniline / polypyrrole composite fibers. Background Art
[0002] As an important material in the national economic production, the functionalization of nylon materials has very important practical significance. Combining nylon materials with conductive polymers to prepare functional composite materials can give nylon energy storage properties while ensuring its high mechanical properties and flexibility, and is expected to show great application potential in the fields of supercapacitors, conductive devices, chemical sensors, etc. Among the many conductive polymer materials, polyaniline and polypyrrole have the advantages of cheap and easy raw materials, convenient synthesis, high conductivity, good environmental stability, and unique doping mechanism. Compounding them with nylon materials to prepare nylon / polyaniline / polypyrrole ternary composite materials has high application value, but the preparation method of nylon / polyaniline / polypyrrole ternary composite materials has not been reported yet.
[0003] The preparation methods for common conductive polymers such as polyaniline and polypyrrole include physical methods such as electrospinning [CN101973713A, CN101967279A, CN100360725C] and mechanical stretching, as well as electrochemical polymerization and chemical oxidation. The electrochemical polymerization method is to dissolve the monomer in an electrolyte and directly polymerize it on an inert electrode to obtain a conductive polymer, but this process requires expensive instruments and equipment, and is limited by the electrode area, making it difficult to mass produce. The chemical oxidation method is considered to be the most promising preparation method because of its simple operation and suitability for mass production. It mainly includes hard template method, soft template method and template-free method. The hard template method is to add zeolite, porous membrane, porous alumina membrane and other materials as templates in the reaction system, so that the monomers are polymerized in the template channels, thereby realizing the orderly arrangement of the conductive polymer structure; the soft template method is to use surfactants and alcohols as templates to restrict the growth of conductive polymers. Both use templates to induce and restrict the growth of conductive polymers [CN101284908A, CN100586987C], but the template needs to be removed in the later stage, which is cumbersome to operate and may damage the structure of the conductive polymer during the processing. The template-free method does not require the use of a template, and mainly includes emulsion polymerization [CN102060993A, CN102050947A], interfacial polymerization [CN101016660A, CN100497440C, CN101710541A, CN100480443C, CN101037504A] and ultrasonic polymerization [CN1323199C], etc. Although the template-free method does not require the removal of the template, it also has some problems. For example, a large amount of emulsifiers are often used in the emulsion polymerization process, and the post-processing process is cumbersome; the interfacial polymerization method requires the use of a large amount of organic solvents, the synthesis yield is low, and batch production is limited; the product structure obtained by the ultrasonic polymerization method is not regular enough, and it needs to use ultrasonic equipment, and it is difficult to prepare continuously. The present invention proposes a novel nylon / polyaniline / polypyrrole ternary composite fiber preparation device and method, through the continuous traction of nylon fiber, impurity removal, aniline surface polymerization, pyrrole surface polymerization, cleaning, drying and collection are carried out in sequence, and finally the continuous preparation of nylon / polyaniline / polypyrrole ternary composite fiber is realized.
[0004] The invention has low cost and simple operation. The reaction system is a full-water phase, and no template and organic solvent are needed. No complicated post-treatment process is needed. The continuous movement of the nylon fiber can effectively induce the surface oriented growth of polyaniline and polypyrrole, and can effectively improve the structural regularity. The one-step continuous batch production of nylon / polyaniline / polypyrrole composite fibers can be achieved, and the production efficiency is greatly improved. The invention is an effective way to achieve the industrialized production of nylon / polyaniline / polypyrrole composite fibers. Summary of the invention
[0005] In view of the problems existing in the prior art, the present invention provides a preparation device and method for nylon / polyaniline / polypyrrole composite fibers. The nylon fiber is subjected to the action of a traction device, and sequentially passes through four U-shaped devices, and is respectively subjected to impurity removal, aniline surface polymerization, pyrrole surface polymerization, and cleaning, and then dried by a dryer. The final product is collected by a collecting device, and the nylon / polyaniline / polypyrrole composite fiber is obtained continuously. The present invention mixes the reaction solution through a conduit by gravity, without the need for a mixing device, and the continuous traction of the nylon fiber contributes to the further uniform mixing of the reaction solution, and can effectively induce polyaniline and polypyrrole to grow on the surface orientation; the method is low in cost and simple to operate, the reaction system is a full aqueous phase, and there is no need to use a template and an organic solvent, and there is no need for a cumbersome post-processing process, and the one-step continuous batch production of nylon / polyaniline / polypyrrole composite fibers can be effectively realized, which greatly improves production efficiency and is an effective way to realize the industrial production of nylon / polyaniline / polypyrrole composite fibers.
[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0007] A preparation device for nylon / polyaniline / polypyrrole composite fibers comprises four U-shaped devices, namely a pretreatment device, an aniline polymerization device, a pyrrole polymerization device, and a post-treatment device. An aniline monomer input device and an aniline monomer initiator device are arranged above the aniline polymerization device, and a pyrrole monomer input device and a pyrrole monomer initiator device are arranged above the pyrrole polymerization device. The aniline monomer input device and the aniline monomer initiator device are respectively connected to a connecting conduit I through a connecting branch pipe, and the connecting conduit I is connected to the aniline polymerization device. The pyrrole monomer input device and the pyrrole monomer initiator device are respectively connected to a connecting conduit II through a connecting branch pipe, and the connecting conduit II is connected to the pyrrole polymerization device. The invention also comprises a traction device and a collection device, and a dryer is arranged between the post-treatment device and the traction device.
[0008] Preferably, the inner diameter of the U-shaped device is 10-100 mm, the inner diameters of the connecting conduit I and the connecting conduit II are 1-30 mm, the rotation speed of the traction device is 0.01-1 r / s, and valves are provided on the connecting conduit I and the connecting conduit II.
[0009] Preferably, the heights of the aniline monomer input device, the aniline monomer initiator device, the pyrrole monomer input device and the pyrrole monomer initiator device are always kept the same and are all adjustable, with a height relative to the upper edge of the U-shaped device of 0.1 to 2 m, and a diameter of the connecting conduit I and the connecting conduit II of 1 to 30 mm.
[0010] Preferably, the aniline polymerization device and the aniline monomer input device and the aniline monomer initiator device connected to it via the connecting conduit I can be used as a whole and exchanged with the pyrrole polymerization device and the pyrrole monomer input device and the pyrrole monomer initiator device connected to it via the connecting conduit II to prepare nylon / polypyrrole / polyaniline composite fibers.
[0011] The present invention also provides a method for preparing nylon / polyaniline / polypyrrole composite fibers using the device, comprising the following steps:
[0012] (1) dissolving aniline monomer and aniline monomer initiator in a doping acid solution to obtain aniline monomer solution and aniline monomer initiator solution, respectively, and injecting them into an aniline monomer input device and an aniline monomer initiator device, respectively; dissolving pyrrole monomer and pyrrole monomer initiator in a doping acid solution to obtain pyrrole monomer and pyrrole monomer initiator solution, respectively, and injecting them into a pyrrole monomer input device and a pyrrole monomer initiator device, respectively;
[0013] (2) injecting a certain amount of pretreatment solution and posttreatment solution into the pretreatment device and the posttreatment device respectively, passing the nylon fiber into the pretreatment device, the aniline polymerization device, the pyrrole polymerization device and the posttreatment device respectively, and connecting the nylon fiber to the traction device after passing through the dryer; the traction device can not only serve as a driving force for the nylon, but also enable the nylon to be fully mixed and reacted with the aniline monomer solution and the pyrrole monomer solution in sequence, so as to obtain a nylon / polyaniline / polypyrrole ternary composite fiber with a layered structure;
[0014] (3) Open the valves on the connecting conduit I and the connecting conduit II to allow the aniline monomer solution and the aniline monomer initiator solution, the pyrrole monomer solution and the pyrrole monomer initiator solution to flow downward into the aniline polymerization device and the pyrrole polymerization device by gravity. After reaching a certain volume in the aniline polymerization device and the pyrrole polymerization device, turn on the power of the traction device to move the nylon fiber at a certain speed;
[0015] (4) The nylon fiber is subjected to a pretreatment device to remove surface impurities, and aniline monomer is polymerized on its surface in an aniline polymerization device to generate nylon / polyaniline; in a pyrrole polymerization device, the surface is coated with polypyrrole to generate nylon / polyaniline / polypyrrole, and then the product is cleaned in a post-treatment device, and finally dried and collected to obtain nylon / polyaniline / polypyrrole composite fibers.
[0016] Preferably, the pretreatment solution comprises a single solution or a mixed solution of water, ethanol, acetone, chloroform, methanol, dilute ammonia, and dilute formamide; and the post-treatment solution is a single solution or a mixed solution of water and ethanol.
[0017] Preferably, the doping acid in the doping acid solution can be a single or mixed doping acid selected from the group consisting of inorganic acids such as hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid, and perchloric acid; or a single or mixed doping acid selected from the group consisting of organic acids such as sulfosalicylic acid, saturated fatty acids, azobenzenesulfonic acid, naphthalenesulfonic acid, camphorsulfonic acid, and dodecylbenzenesulfonic acid; or a mixed acid of an organic acid and an inorganic acid, and the molar concentration of the doping acid is 0.1 to 8 mol / L.
[0018] Preferably, the aniline monomer initiator and the pyrrole monomer initiator are single or compound initiators selected from ferric chloride, hydrogen peroxide, ammonium persulfate, formyl peroxide, azobisisobutyronitrile, and potassium dichromate, and the molar concentration of the aniline monomer initiator solution and the pyrrole monomer initiator solution is 0.01-10 mol / L.
[0019] Preferably, the aniline monomer and pyrrole monomer include monomers and their derivatives, and the molar concentration of the aniline monomer solution and the pyrrole monomer solution is 0.03~7 mol / L; the thickness of the polyaniline and polypyrrole layer can be adjusted by the molar ratio of the monomers, and the molar ratio of the aniline monomer to the pyrrole monomer is 1:(0.1~15).
[0020] Preferably, the doped acid solution may contain a cosolvent, which is a single or compound cosolvent selected from methanol, ethanol, isopropanol, acetone, dimethylacetamide, dimethylformamide, dimethyl sulfoxide, and N-methylpyrrolidone, and the molar concentration of the cosolvent is 0.001 to 0.5 mol / L. Preferably, the traction device can be used as a driving force for nylon, and can also make nylon fully mixed and reacted with aniline monomer solution and pyrrole monomer solution in sequence to obtain a nylon / polyaniline / polypyrrole ternary composite fiber with a layered structure.
[0021] The synthesis mechanism of the present invention: The present invention uses nylon fiber as a matrix, and through the traction effect, it is sequentially passed through four U-shaped devices to perform surface treatment, aniline polymerization, pyrrole polymerization and cleaning treatment of nylon. After the surface treatment, the nylon fiber enters a mixed solution of aniline and its initiator. The aniline monomer is adsorbed on the surface of the nylon fiber under the action of the intermolecular interaction force. After the initiator induces an in-situ redox reaction, polyaniline is generated on the surface of the nylon fiber to obtain a nylon / polyaniline binary composite fiber, and continues to flow into a mixed solution of pyrrole and its oxidant, so that polypyrrole is further generated on the surface of the binary composite fiber, and finally a nylon / polyaniline / polypyrrole ternary composite fiber is obtained. The ternary composite fiber continues to flow through the post-treatment solution to remove low molecular substances and unreacted monomers on the surface of the composite fiber, and then the product is finally obtained after drying and collection treatment. In this method, the traction effect of the nylon fiber can effectively promote the orderly layer-by-layer molecular self-assembly process of polyaniline and polypyrrole, and while ensuring continuous preparation, the structural regularity can also be greatly improved.
[0022] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0023] (1) The present invention integrates nylon, polyaniline and polypyrrole in one step for the first time, and proposes a method for continuous composite of nylon, polyaniline and polypyrrole; the present invention can effectively regulate the residence time of nylon fiber in each reaction device by controlling the traction device, and can effectively control the thickness of polyaniline and polypyrrole layers; the monomer and initiator are mixed and injected into each U-shaped reaction device through the conduit by gravity, while ensuring the continuous replenishment of the reaction liquid in the U-shaped reaction device, it also avoids the use of additional mixing equipment, and the height of the conduit is adjustable, so that the flow rate of the solution in the conduit is controllable; the traction flow of the nylon fiber not only further orients the nylon fiber, but also makes the reaction liquid more uniform, ensuring the consistency and uniformity of the monomer surface polymerization reaction, and the product is more homogeneous and less prone to agglomeration. In addition, the traction flow of the nylon fiber can also greatly increase the contact probability between the monomer and the initiator, greatly improving the preparation efficiency, and at the same time can effectively induce polyaniline and polypyrrole to self-assemble in an orderly manner on the fiber surface, making the product structure more regular and orderly, which can greatly improve the energy storage performance of the material.
[0024] (2) The present invention is low-cost, continuously controllable, simple to operate, highly repeatable, and has high synthesis efficiency. The reaction system is an all-aqueous phase, and no template or organic solvent is required. No cumbersome post-processing process is required. The one-step continuous batch production of nylon / polyaniline / polypyrrole composite fibers can be effectively achieved, which greatly improves production efficiency and has high potential for industrial application. The aniline polymerization process and the pyrrole polymerization process in the present invention are interchangeable, which facilitates the synthesis of nylon / polypyrrole / polyaniline composite fibers. At the same time, the present invention has high universality for the continuous preparation of fiber-based composite materials. The present invention spatially "one-dimensionalizes" the composite process of nylon, polyaniline, and polypyrrole, which facilitates real-time monitoring of the composite process and is helpful for related mechanism research.
[0025] (3) The nylon / polyaniline / polypyrrole composite fiber prepared by the present invention has a regular and orderly structure and excellent performance, and can be applied to many fields such as supercapacitor electrode materials, conductive materials, anti-corrosion materials, sensor materials, antistatic materials, electromagnetic shielding materials, and adsorption materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 Schematic diagram of the device for preparing nylon / polyaniline / polypyrrole composite fibers.
[0027] Figure 2 This is a scanning electron microscope image of the nylon / polyaniline / polypyrrole composite fiber synthesized in Example 1 of the present invention.
[0028] Figure 3This is the electrochemical cyclic voltammetry curve of the nylon / polyaniline / polypyrrole composite fiber synthesized in Example 2 of the present invention in 1 mol / L sulfuric acid electrolyte.
[0029] Figure 4 This is a scanning electron microscope image of the nylon / polyaniline / polypyrrole composite fiber synthesized in Example 3 of the present invention.
[0030] Figure 5 This is the constant current charge and discharge curve of the nylon / polyaniline / polypyrrole composite fiber synthesized in Example 4 of the present invention in 1 mol / L sulfuric acid electrolyte.
[0031] Figure 6 This is the AC impedance curve of the nylon / polyaniline / polypyrrole composite fiber synthesized in Example 5 of the present invention in 1 mol / L sulfuric acid electrolyte. DETAILED DESCRIPTION
[0032] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0033] Example 1
[0034] like Figure 1 As shown, the preparation device of nylon / polyaniline / polypyrrole composite fiber of this embodiment includes four U-shaped devices, namely a pretreatment device 1, an aniline polymerization device 2, a pyrrole polymerization device 3, and a post-treatment device 4. An aniline monomer input device 5 and an aniline monomer initiator device 6 are arranged above the aniline polymerization device 2, and a pyrrole monomer input device 7 and a pyrrole monomer initiator device 8 are arranged above the pyrrole polymerization device 3. The aniline monomer input device 5 and the aniline monomer initiator device 6 are connected to the connecting conduit I (11) through connecting branch pipes. The connecting conduit Ⅰ (11) is connected to the aniline polymerization device 2, the pyrrole monomer input device 7 and the pyrrole monomer initiator device 8 are respectively connected to the connecting conduit II (12) through connecting branch pipes, and the connecting conduit II (12) is connected to the pyrrole polymerization device 3. Specifically, the connecting conduit I (11) is inserted into the starting end of the aniline polymerization device 2 (one end of the U-shaped device through which the nylon fiber first passes) and is connected to the aniline polymerization device 2, and the connecting conduit II (12) is inserted into the starting end of the phenylpyrrole polymerization device 3 (one end of the U-shaped device through which the nylon fiber first passes) and is connected to the pyrrole polymerization device 3.
[0035] The preparation device of nylon / polyaniline / polypyrrole composite fiber of this embodiment further comprises a traction device 9 and a collecting device 10, and a dryer 13 is provided between the post-processing device 4 and the traction device 9. Valves are provided on the connecting conduit I (11) and the connecting conduit II (12).
[0036] In this embodiment, the inner diameter of the U-shaped device is 10 mm, the rotation speed of the traction device is 0.01 r / s, the height of the monomer and its initiator device relative to the upper edge of the U-shaped device is 0.1 m, the inner diameter of the connecting conduits (connecting conduit I (11) and connecting conduit II (12)) is 3 mm, the traction device 9 continuously provides traction, and the collecting device 10 collects the final product.
[0037] The method for preparing nylon / polyaniline / polypyrrole composite fibers using the above device in this embodiment is as follows:
[0038] (1) Accurately weigh a certain amount of aniline and ammonium persulfate, dissolve them in 1 mol / L hydrochloric acid solution, prepare 0.003 mol / L aniline solution and 0.01 mol / L ammonium persulfate solution, and inject them into aniline monomer input device 5 and aniline monomer initiator device 6 respectively; accurately weigh a certain amount of pyrrole and ammonium persulfate, dissolve them in 1 mol / L hydrochloric acid solution, prepare 0.003 mol / L pyrrole solution and 0.01 mol / L ammonium persulfate solution, and inject them into pyrrole monomer input device 7 and pyrrole monomer initiator device 8 respectively. The molar ratio of aniline to pyrrole is 1:1. A certain amount of ethanol is added to the two monomer solutions as a co-solvent, and the molar concentration of methanol is 0.001 mol / L.
[0039] (2) Ethanol and water are injected into the pretreatment device 1 and the post-treatment device 4 respectively, and the nylon fiber is respectively passed into the pretreatment device 1, the aniline polymerization device 2, the pyrrole polymerization device 3 and the post-treatment device 4, and then connected to the traction device after passing through the dryer. The valves on the connecting conduit I (11) and the connecting conduit II (12) located at the beginning of the aniline polymerization device 2 and the pyrrole polymerization device 3 are opened to allow the aniline monomer solution and its initiator solution, the pyrrole monomer solution and its initiator solution to flow downward into the beginning of the aniline polymerization device 2 and the pyrrole polymerization device 3 by gravity. After the mixed solution reaches a certain volume in the aniline polymerization device 2 and the pyrrole polymerization device 3, the power supply of the traction device 9 is turned on to allow the nylon fiber to move stably under the condition that the rotation speed of the traction device is 0.005 r / s. Subsequently, the product is washed in the post-treatment device 4, and finally dried in the dryer 13 and collected in the collector 10 to obtain the nylon / polyaniline / polypyrrole composite fiber. Polyaniline / polypyrrole (e.g., Figure 2 The electrical conductivity was 0.52 S / cm.
[0040] Example 2
[0041] The inner diameter of the U-shaped device in the continuous preparation device of nylon / polyaniline / polypyrrole composite fibers in this embodiment is 30 mm, the rotation speed of the traction device is 0.05 r / s, the height of the monomer and its initiator device relative to the upper edge of the U-shaped device is 0.5 m, the inner diameter of the connecting conduit is 10 mm, and other implementation methods are the same as those in Example 1.
[0042] The method for preparing nylon / polyaniline / polypyrrole composite fibers using the above device in this embodiment is as follows:
[0043] (1) Accurately weigh a certain amount of aniline and ferric chloride, dissolve them in 8 mol / L phosphoric acid solution, prepare 1 mol / L aniline solution and 4 mol / L ferric chloride solution, and inject them into aniline monomer input device 5 and aniline monomer initiator device 6 respectively; accurately weigh a certain amount of pyrrole and ferric chloride, dissolve them in 8 mol / L phosphoric acid solution, prepare 2 mol / L pyrrole solution and 8 mol / L ferric chloride solution, and inject them into pyrrole monomer input device 7 and pyrrole monomer initiator device 8 respectively. The molar ratio of aniline to pyrrole is 1:2. A certain amount of methanol is added to the two monomer solutions as a co-solvent, and the molar concentration of methanol is 0.005 mol / L.
[0044] (2) Ethanol and water are injected into the pretreatment device 1 and the post-treatment device 4 respectively, and the nylon fiber is respectively passed into the pretreatment device 1, the aniline polymerization device 2, the pyrrole polymerization device 3 and the post-treatment device 4, and then connected to the traction device after passing through the dryer. The valves on the connecting conduit I (11) and the connecting conduit II (12) located at the beginning of the aniline polymerization device 2 and the pyrrole polymerization device 3 are opened, so that the aniline monomer solution and its initiator solution, the pyrrole monomer solution and its initiator solution flow downward into the beginning of the aniline polymerization device 2 and the pyrrole polymerization device 3 by gravity. After the mixed solution reaches a certain volume in the aniline polymerization device 2 and the pyrrole polymerization device 3, the power supply of the traction device is turned on, so that the nylon fiber moves stably under the condition that the rotation speed of the traction device is 0.01 r / s, and then the product is washed in the post-treatment device 4, and finally dried in the dryer 13 and collected in the collector 10 to obtain nylon / polyaniline / polypyrrole composite fiber. Figure 3 The electrochemical cyclic voltammetry curve of the nylon / polyaniline / polypyrrole composite fiber in 1 mol / L sulfuric acid electrolyte at a scan rate of 5 mV / s is given, and its specific capacitance is 359.2 F / g.
[0045] Example 3
[0046] The inner diameter of the U-shaped device in the continuous preparation device of nylon / polyaniline / polypyrrole composite fibers in this embodiment is 100 mm, the rotation speed of the traction device is 1 r / s, the height of the monomer and its initiator device relative to the upper edge of the U-shaped device is 1.5 m, the inner diameter of the connecting conduit is 30 mm, and other implementation methods are the same as Example 1.
[0047] The method for preparing nylon / polyaniline / polypyrrole composite fibers using the above device in this embodiment is as follows:
[0048] (1) Accurately weigh a certain amount of aniline and hydrogen peroxide, dissolve them in 2 mol / L sulfuric acid solution, prepare 7 mol / L aniline solution and 7 mol / L hydrogen peroxide solution, and inject them into aniline monomer input device 5 and aniline monomer initiator device 6 respectively; accurately weigh a certain amount of pyrrole and hydrogen peroxide, dissolve them in 2 mol / L sulfuric acid solution, prepare 3.5 mol / L pyrrole solution and 3.5 mol / L hydrogen peroxide solution, and inject them into pyrrole monomer input device 7 and pyrrole monomer initiator device 8 respectively. The molar ratio of aniline to pyrrole is 1:0.5. A certain amount of ethanol is added to the two monomer solutions as a co-solvent, and the molar concentration of ethanol is 0.01 mol / L.
[0049] (2) Methanol is injected into the pretreatment device 1, water and ethanol are injected into the post-treatment device 4, and the nylon fiber is respectively introduced into the pretreatment device 1, the aniline polymerization device 2, the pyrrole polymerization device 3 and the post-treatment device 4, and connected to the traction device after passing through the dryer. The valves on the connecting conduit I (11) and the connecting conduit II (12) located at the beginning of the aniline polymerization device 2 and the pyrrole polymerization device 3 are opened to allow the aniline monomer solution and its initiator solution, the pyrrole monomer solution and its initiator solution to flow downward into the beginning of the aniline polymerization device 2 and the pyrrole polymerization device 3 by gravity. After the mixed solution reaches a certain volume in the aniline polymerization device 2 and the pyrrole polymerization device 3, the power supply of the traction device is turned on to allow the nylon fiber to move stably under the condition that the rotation speed of the traction device is 1r / s, and then the product is washed in the post-treatment device 4, and finally dried in the dryer 13 and collected in the collector 10 to obtain the nylon / polyaniline / polypyrrole composite fiber. Polyaniline / polypyrrole (e.g., Figure 4 The electrical conductivity was 0.75 S / cm.
[0050] Example 4
[0051] The inner diameter of the U-shaped device in the continuous preparation device of nylon / polyaniline / polypyrrole composite fibers in this embodiment is 20 mm, the rotation speed of the traction device is 0.05 r / s, the height of the monomer and its initiator device relative to the upper edge of the U-shaped device is 0.5 m, the inner diameter of the connecting conduit is 15 mm, and other implementation methods are the same as those in Example 1.
[0052] The method for preparing nylon / polyaniline / polypyrrole composite fibers using the above device in this embodiment is as follows:
[0053] (1) Accurately weigh a certain amount of aniline and azobisisobutyronitrile, dissolve them in a mixed solution of 0.1 mol / L hydrochloric acid and sulfosalicylic acid to prepare 0.1 mol / L aniline solution and 0.1 mol / L azobisisobutyronitrile solution, and inject them into the aniline monomer input device 5 and the aniline monomer initiator device 6 respectively; accurately weigh a certain amount of pyrrole and azobisisobutyronitrile, dissolve them in a mixed solution of 0.1 mol / L hydrochloric acid and sulfosalicylic acid to prepare 1.5 mol / L pyrrole solution and 1.5 mol / L azobisisobutyronitrile solution, and inject them into the pyrrole monomer input device 7 and the pyrrole monomer initiator device 8 respectively. The molar ratio of aniline to pyrrole is 1:15. A certain amount of isopropanol is added to the two monomer solutions as a co-solvent, and the molar concentration of isopropanol is 0.5 mol / L.
[0054] (2) Acetone and water are injected into the pretreatment device 1, and water and ethanol are injected into the post-treatment device 4. The nylon fiber is respectively introduced into the pretreatment device 1, the aniline polymerization device 2, the pyrrole polymerization device 3 and the post-treatment device 4, and then connected to the traction device after passing through the dryer. The valves on the connecting conduit I (11) and the connecting conduit II (12) located at the beginning of the aniline polymerization device 2 and the pyrrole polymerization device 3 are opened to allow the aniline monomer solution and its initiator solution, and the pyrrole monomer solution and its initiator solution to flow downward into the beginning of the aniline polymerization device 2 and the pyrrole polymerization device 3 by gravity. After the mixed solution reaches a certain volume in the aniline polymerization device 2 and the pyrrole polymerization device 3, the power supply of the traction device is turned on to allow the nylon fiber to move stably under the condition that the rotation speed of the traction device is 0.05 r / s. Subsequently, the product is washed in the post-treatment device 4, and finally dried in the dryer 13 and collected in the collector 10 to obtain the nylon / polyaniline / polypyrrole composite fiber. Figure 5 The constant current charge-discharge curves of the nylon / polyaniline / polypyrrole composite fiber in 1 mol / L sulfuric acid electrolyte at a current density of 2 A / g are given, and its specific capacitance is 287.6 F / g.
[0055] Example 5
[0056] The inner diameter of the U-shaped device in the continuous preparation device of nylon / polyaniline / polypyrrole composite fibers in this embodiment is 50 mm, the rotation speed of the traction device is 0.02 r / s, the height of the monomer and its initiator device relative to the upper edge of the U-shaped device is 1 m, the inner diameter of the connecting conduit is 10 mm, and other implementation methods are the same as Example 1.
[0057] The method for preparing nylon / polyaniline / polypyrrole composite fibers using the above device in this embodiment is as follows:
[0058] (1) Accurately weigh a certain amount of aniline and potassium dichromate, dissolve them in 0.4 mol / L sulfuric acid solution, prepare 1 mol / L aniline solution and 1 mol / L potassium dichromate solution, and inject them into aniline monomer input device 5 and aniline monomer initiator device 6 respectively; accurately weigh a certain amount of pyrrole, potassium dichromate and ferric chloride, dissolve them in 1 mol / L sulfuric acid solution, prepare 0.1 mol / L pyrrole solution and 0.1 mol / L potassium dichromate and ferric chloride mixed solution, and inject them into pyrrole monomer input device 7 and pyrrole monomer initiator device 8 respectively. The molar ratio of aniline to pyrrole is 1:0.1. A certain amount of acetone and ethanol are added to the two monomer solutions as co-solvents, and the molar concentrations of acetone and ethanol are 0.2 mol / L.
[0059] (2) Water and dilute ammonia water are injected into the pretreatment device 1, and water and ethanol are injected into the post-treatment device 4. The nylon fiber is respectively passed through the pretreatment device 1, the aniline polymerization device 2, the pyrrole polymerization device 3 and the post-treatment device 4, and then connected to the traction device after passing through the dryer. The valves on the connecting conduit I (11) and the connecting conduit II (12) located at the beginning of the aniline polymerization device 2 and the pyrrole polymerization device 3 are opened to allow the aniline monomer solution and its initiator solution, and the pyrrole monomer solution and its initiator solution to flow downward into the beginning of the aniline polymerization device 2 and the pyrrole polymerization device 3 by gravity. After the mixed solution reaches a certain volume in the aniline polymerization device 2 and the pyrrole polymerization device 3, the power supply of the traction device is turned on to allow the nylon fiber to move stably under the condition that the rotation speed of the traction device is 0.01 r / s. Subsequently, the product is washed in the post-treatment device 4, and finally dried in the dryer 13 and collected in the collector 10 to obtain nylon / polyaniline / polypyrrole composite fiber. Figure 6 The AC impedance curve of the nylon / polyaniline / polypyrrole composite fiber in 1 mol / L sulfuric acid electrolyte is given, and the electrical conductivity obtained by characterizing its electrical properties is 0.54 S / cm.
Claims
1. A preparation device for nylon / polyaniline / polypyrrole composite fiber, characterized in that: The invention comprises four U-shaped devices, namely a pretreatment device (1), an aniline polymerization device (2), a pyrrole polymerization device (3), and a post-treatment device (4). An aniline monomer input device (5) and an aniline monomer initiator device (6) are arranged above the aniline polymerization device (2). A pyrrole monomer input device (7) and a pyrrole monomer initiator device (8) are arranged above the pyrrole polymerization device (3). The aniline monomer input device (5) and the aniline monomer initiator device (6) are respectively connected to a connecting conduit I (11) through a connecting branch pipe. The connecting conduit I (11) is connected to the aniline polymerization device (2). The pyrrole monomer input device (7) and the pyrrole monomer initiator device (8) are respectively connected to a connecting conduit II (12) through a connecting branch pipe. The connecting conduit II (12) is connected to the pyrrole polymerization device (3). The invention also comprises a traction device (9) and a collection device (10). A drying device (13) is arranged between the post-treatment device (4) and the traction device (9). The heights of the aniline monomer input device (5), the aniline monomer initiator device (6), the pyrrole monomer input device (7) and the pyrrole monomer initiator device (8) are always kept the same and are all adjustable, with the height relative to the upper edge of the U-shaped device being 0.1 to 2 m.
2. The device for preparing nylon / polyaniline / polypyrrole composite fibers according to claim 1, characterized in that: The inner diameter of the U-shaped device is 10-100 mm, the inner diameters of the connecting conduit I and the connecting conduit II are 1-30 mm, the rotation speed of the traction device (9) is 0.01-1 r / s, and valves are provided on the connecting conduit I and the connecting conduit II.
3. The preparation device of nylon / polyaniline / polypyrrole composite fiber according to claim 1, characterized in that: The aniline polymerization device (2) and the aniline monomer input device (5) and the aniline monomer initiator device (6) connected to it via the connecting conduit I are used as a whole, and are exchanged with the pyrrole polymerization device (3) and the pyrrole monomer input device (7) and the pyrrole monomer initiator device (8) connected to it via the connecting conduit II, to prepare nylon / polypyrrole / polyaniline composite fibers.
4. A method for preparing nylon / polyaniline / polypyrrole composite fibers using the device according to any one of claims 1 to 3, characterized in that The following steps are involved: (1) dissolving aniline monomer and aniline monomer initiator in a doping acid solution to obtain aniline monomer solution and aniline monomer initiator solution, respectively, and injecting them into an aniline monomer input device (5) and an aniline monomer initiator device (6), respectively; dissolving pyrrole monomer and pyrrole monomer initiator in a doping acid solution to obtain pyrrole monomer and pyrrole monomer initiator solution, respectively, and injecting them into a pyrrole monomer input device (7) and a pyrrole monomer initiator device (8); (2) injecting a certain amount of pretreatment solution and posttreatment solution into the pretreatment device (1) and the posttreatment device (4) respectively, passing the nylon fiber into the pretreatment device (1), the aniline polymerization device (2), the pyrrole polymerization device (3) and the posttreatment device (4) respectively, and connecting the nylon fiber to the traction device after passing through the dryer (13); (3) opening valves on the connecting conduit I and the connecting conduit II, allowing the aniline monomer solution and the aniline monomer initiator solution, the pyrrole monomer solution and the pyrrole monomer initiator solution to flow downward into the aniline polymerization device (2) and the pyrrole polymerization device (3) by gravity, and after reaching a certain volume in the aniline polymerization device (2) and the pyrrole polymerization device (3), turning on the power supply of the traction device to move the nylon fiber at a certain speed; (4) The nylon fiber is subjected to a pretreatment device (1) to remove surface impurities, and aniline monomer is polymerized on the surface of the nylon fiber in an aniline polymerization device (2) to generate nylon / polyaniline; The surface of the polypyrrole is coated in the pyrrole polymerization device (3) to generate nylon / polyaniline / polypyrrole, and the product is then washed in the post-processing device (4), and finally dried and collected to obtain nylon / polyaniline / polypyrrole composite fibers.
5. The method for preparing nylon / polyaniline / polypyrrole composite fiber according to claim 4, characterized in that: The pretreatment solution includes a single solution or a mixed solution of water, ethanol, acetone, chloroform, methanol, dilute ammonia water, and dilute formamide; the post-treatment solution is a single solution or a mixed solution of water and ethanol.
6. The method for preparing nylon / polyaniline / polypyrrole composite fiber according to claim 4, characterized in that: The doping acid in the doping acid solution is a single or mixed doping acid selected from the group consisting of inorganic acids such as hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid, and perchloric acid; or the doping acid in the doping acid solution is a single or mixed doping acid selected from the group consisting of organic acids such as sulfosalicylic acid, saturated fatty acids, azobenzenesulfonic acid, naphthalenesulfonic acid, camphorsulfonic acid, and dodecylbenzenesulfonic acid; or the doping acid in the doping acid solution is a mixed acid of an organic acid and an inorganic acid, and the molar concentration of the doping acid is 0.1 to 8 mol / L.
7. The method for preparing nylon / polyaniline / polypyrrole composite fiber according to claim 4, characterized in that: The aniline monomer initiator and the pyrrole monomer initiator are single or compound initiators in ferric chloride, hydrogen peroxide, ammonium persulfate, formyl peroxide, azobisisobutyronitrile and potassium dichromate, and the molar concentration of the aniline monomer initiator solution and the pyrrole monomer initiator solution is 0.01-10 mol / L.
8. The method for preparing nylon / polyaniline / polypyrrole composite fiber according to claim 4, characterized in that: The aniline monomer and the pyrrole monomer include monomers and derivatives thereof. The molar concentration of the aniline monomer solution and the pyrrole monomer solution is 0.03-7 mol / L; the molar ratio of the aniline monomer to the pyrrole monomer is 1:(0.1-15).
9. The method for preparing nylon / polyaniline / polypyrrole composite fiber according to claim 4, characterized in that: The doped acid solution contains a co-solvent, which is a single or compound co-solvent selected from methanol, ethanol, isopropanol, acetone, dimethylacetamide, dimethylformamide, dimethyl sulfoxide and N-methylpyrrolidone, and the molar concentration of the co-solvent is 0.001-0.5 mol / L.