A modified KIT-6 composite adsorbent and its preparation method and application

Through the preparation of modified KIT-6 composite adsorbent, the reaction and impregnation technology of KIT-6 molecular sieve and ionic liquid are used to solve the problem of reducing absorption efficiency caused by the increase in viscosity of ionic liquid, and high selectivity, high adsorption capacity and good CO2 adsorption effect of regeneration performance.

CN116510694BActive Publication Date: 2024-12-06GUILIN UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310728742.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-19
Publication Date
2024-12-06
Estimated Expiration
2043-06-19

AI Technical Summary

Technical Problem

In the prior art, the viscosity of ionic liquid as CO2 absorber increases or decreases, resulting in a decrease in absorption efficiency. Thermodynamic factors affect the absorption difficulty, making it difficult to prepare a solid adsorbent with high selectivity, high adsorption capacity, low cost and environmentally friendly.

Method used

By using the preparation method of modified KIT-6 composite adsorbent, KIT-6 molecular sieve reacts with N-[3-(trimethoxysilyl)propyl]ethylenediamine and tetraethylenepentaamine salt ionic liquid. A silanized modified carrier was formed and impregnated by anhydrous ethanol solution to obtain a modified KIT-6 composite adsorbent with excellent adsorption properties.

Benefits of technology

The optimal adsorption value was achieved in the range of 25-45% loading at 60°C and normal pressure. 2N-K6P30% and 2N-K6L40% showed high adsorption amounts, and remained well after multiple adsorption and desorption cycles. The regeneration properties of the two types of physical adsorption and chemical adsorption describe the synergistic effects of physical adsorption and chemical adsorption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116510694B_ABST
    Figure CN116510694B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of removing carbon dioxide. The present invention provides a modified KIT-6 composite adsorbent and a preparation method and application thereof. The preparation method comprises the following steps: reacting KIT-6 molecular sieve, toluene and N-[3-(trimethoxysilyl)propyl]ethylenediamine to obtain a silanized modified carrier; impregnating the silanized modified carrier with an anhydrous ethanol solution of an ionic liquid to obtain a modified KIT-6 composite adsorbent; the ionic liquid is a tetraethylenepentamine salt ionic liquid. At 60°C and normal pressure, 2N-K6P30% exhibits an adsorption value of 1.497mmol·g ‑1 , the adsorption amount of 2N‑K6L40% is 2.509mmol·g ‑1 , 2N‑K6L40% has an adsorption capacity of up to 3.670mmol·g at 90℃ ‑1 After 5 adsorption-desorption cycles, the sample still has good regeneration performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of removing carbon dioxide, and in particular to a modified KIT-6 composite adsorbent and a preparation method and application thereof. Background Art

[0002] Post-combustion CO2 capture technology removes CO2 and other impurity gases from burning fossil fuels based on physical or chemical adsorption / absorption mechanisms. According to the principle of the capture process, it can be divided into adsorption, absorption, membrane separation and cryogenic distillation. Compared with other post-combustion CO2 capture methods, adsorption has the advantages of low cost and high CO2 capacity. The preparation of solid adsorbents with high selectivity, high adsorption capacity, good mechanical strength, easy regeneration, low cost and environmental friendliness is the focus of research.

[0003] Currently, ionic liquids (ILs) have received increasing attention as new amphoteric solvents, and are considered to be good solvents for capturing CO2 due to their unique properties, including low vapor pressure, high thermal stability, and adjustable characteristics. The increase in viscosity of amine-functionalized ILs after absorbing CO2 is due to the strong hydrogen bonding network, which may be an obstacle to the application of ILs as CO2 absorbents. Not only functionalized ILs, but also the viscosity of ordinary ILs will increase or decrease after mixing with CO2. In addition, thermodynamic factors affect the further absorption of CO2, that is, the absorbed CO2 makes it difficult to further absorb CO2.

[0004] Amine-modified solid adsorbents are mainly composed of a support with highly developed porosity and an active ingredient with affinity for CO2. Two main techniques are used to prepare amine-modified solid adsorbents. One technique is physical impregnation, where liquid amine molecules are impregnated into a porous support by van der Waals forces. The other technique is chemical grafting, where alkanolamine molecules are grafted onto the inner surface of a porous support by reacting with silanol groups. The grafting method generally has the advantages of fast adsorption and high amine efficiency, while the impregnation method is more convenient, easier to operate, consumes less energy, and can load more active CO2-affinity sites. KIT-6 mesoporous molecular sieve is a three-dimensional structure with simple synthesis conditions, excellent mass transfer performance, large pore volume, thick pore wall and adjustable pore size.

[0005] Therefore, it is of great significance to study and obtain a modified KIT-6 composite adsorbent with high selectivity, high adsorption capacity, easy regeneration, low cost and environmental friendliness. Summary of the invention

[0006] The purpose of the present invention is to provide a modified KIT-6 composite adsorbent and a preparation method and application thereof in order to overcome the deficiencies of the prior art.

[0007] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0008] The present invention provides a method for preparing a modified KIT-6 composite adsorbent, comprising the following steps:

[0009] 1) reacting KIT-6 molecular sieve, toluene and N-[3-(trimethoxysilyl)propyl]ethylenediamine to obtain a silanized modified carrier;

[0010] 2) impregnating the silanized modified carrier with an anhydrous ethanol solution of the ionic liquid to obtain a modified KIT-6 composite adsorbent;

[0011] The ionic liquid is a tetraethylenepentamine salt ionic liquid.

[0012] Preferably, in step 1), the mass volume ratio of the KIT-6 molecular sieve and toluene is 1 g: 90-110 mL, and the mass volume ratio of the KIT-6 molecular sieve and N-[3-(trimethoxysilyl)propyl]ethylenediamine is 1 g: 1.2-1.8 mL.

[0013] Preferably, the reaction temperature in step 1) is 80-90° C., and the reaction time is 14-18 h.

[0014] Preferably, the mass of the ionic liquid in step 2) is 25-45% of the total mass of the ionic liquid and the silanized modified carrier.

[0015] Preferably, the ionic liquid is a tetraethylenepentamine nitrate ionic liquid or a tetraethylenepentamine lysine salt ionic liquid.

[0016] Preferably, when the ionic liquid is tetraethylenepentamine nitrate ionic liquid, the mass of the ionic liquid is 25-35% of the total mass of the ionic liquid and the silanized modified carrier; when the ionic liquid is tetraethylenepentamine lysine salt ionic liquid, the mass of the ionic liquid is 35-45% of the total mass of the ionic liquid and the silanized modified carrier.

[0017] Preferably, the immersion time in step 2) is 5 to 7 hours.

[0018] The present invention also provides a modified KIT-6 composite adsorbent prepared by the preparation method.

[0019] The present invention also provides the use of the modified KIT-6 composite adsorbent in adsorbing carbon dioxide.

[0020] The beneficial effects of the present invention include:

[0021] In the present invention, N-[3-(trimethoxysilyl)propyl]ethylenediamine (denoted as 2N) was used as a grafting agent, and the dry grafting method was used, and [TEPA][NO3] and [TEPA][Lys] were used as impregnating agents to modify the KIT-6 molecular sieve. In the range of loading amount of 25-45%, at 60°C and normal pressure, 2N-K6P30% showed an optimal adsorption value of 1.497mmol·g -1 The optimal loading amount of the series of samples loaded with [TEPA][Lys] was 40%, and the adsorption amount of 2N-K6L 40% was 2.509 mmol·g -1 The adsorption capacity of 2N-K6L40% at 90℃ is as high as 3.67mmol·g -1 The Avrami model was used to fit the adsorption data of the best adsorbent at different temperatures, which can better describe the adsorption process of the composite adsorbent, which is the combined effect of physical adsorption and chemical adsorption. After 5 adsorption and desorption cycles, the composite adsorbent sample still has good regeneration performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 The TGA weight loss curves of the composite adsorbents of Examples 1 to 2 and Comparative Examples 1 to 2 and their corresponding DTG curves, wherein A is the TGA weight loss curve and B is the DTG curve;

[0023] Figure 2 The infrared spectra of KIT-6, 2N-KIT-6-1.5, 2N-K6P30% of Example 1 and 2N-K6L-40% of Example 2;

[0024] Figure 3 The low-temperature nitrogen adsorption-desorption isotherms of the composite adsorbents of Example 2 and Comparative Example 2 at 77K;

[0025] Figure 4 The nitrogen adsorption-desorption isotherms of 2N-KIT-6-1.5 of Example 1 and the composite adsorbents of Examples 1 and 2 at 77K;

[0026] Figure 5 is the amine efficiency of the composite adsorbent of Examples 1-2 and Comparative Examples 1-2;

[0027] Figure 6 The CO2 adsorption curves of the composite adsorbents of Examples 1 to 2 and Comparative Examples 1 to 2 at 60°C, wherein A is Example 1 and Comparative Example 1, and B is Example 2 and Comparative Example 2;

[0028] Figure 7 The composite adsorbents of Example 1 and Example 2 are adsorption curves of CO2 at different adsorption temperatures, wherein A is Example 1 and B is Example 2;

[0029] Figure 8 This is a graph showing the CO2 cycle adsorption, desorption and regeneration test of the composite adsorbent of Example 1 and Example 2;

[0030] Fig. 9 The Avrami equation fitting curves of the composite adsorbents of Example 1 and Example 2 for adsorbing CO2 at different temperatures, wherein A is Example 1 and B is Example 2. DETAILED DESCRIPTION

[0031] The present invention provides a method for preparing a modified KIT-6 composite adsorbent, comprising the following steps:

[0032] 1) reacting KIT-6 molecular sieve, toluene and N-[3-(trimethoxysilyl)propyl]ethylenediamine to obtain a silanized modified carrier;

[0033] 2) impregnating the silanized modified carrier with an anhydrous ethanol solution of the ionic liquid to obtain a modified KIT-6 composite adsorbent;

[0034] The ionic liquid is a tetraethylenepentamine salt ionic liquid.

[0035] In the present invention, the mass volume ratio of the KIT-6 molecular sieve (ordered mesoporous silica having a cage-like three-dimensional interconnected pore structure) and toluene in step 1) is preferably 1 g: 90-110 mL, further preferably 1 g: 95-105 mL, and more preferably 1 g: 100 mL; the mass volume ratio of the KIT-6 molecular sieve and N-[3-(trimethoxysilyl)propyl]ethylenediamine (2N) is preferably 1 g: 1.2-1.8 mL, further preferably 1 g: 1.4-1.6 mL, and more preferably 1 g: 1.5 mL.

[0036] In the present invention, the reaction temperature in step 1) is preferably 80-90°C, more preferably 82-88°C, more preferably 84-85°C; the reaction time is preferably 14-18h, more preferably 15-17h, more preferably 16h.

[0037] In the present invention, the KIT-6 molecular sieve is preferably dried before the reaction, and the drying temperature is preferably 95 to 105° C., and more preferably 100° C.; the reaction is preferably carried out under condensation reflux conditions.

[0038] The product after the reaction is completed is preferably vacuum filtered, washed and dried to obtain a silanized modified carrier (2N-KIT-6-X, X represents the volume of 1g of KIT-6 molecular sieve dry-grafted silane coupling agent 2N); the washing reagent is preferably anhydrous ethanol, and the number of washings is preferably 3 to 4 times; the drying temperature is preferably 95 to 105°C, more preferably 100°C, and the drying time is preferably 22 to 26h, more preferably 24h.

[0039] The mass of the ionic liquid in step 2) of the present invention is preferably 25-45% of the total mass of the ionic liquid and the silanized modified carrier.

[0040] In the present invention, the ionic liquid is preferably a tetraethylenepentamine nitrate ionic liquid or a tetraethylenepentamine lysine salt ionic liquid.

[0041] In the anhydrous ethanol solution of the ionic liquid of the present invention, the mass volume ratio of the ionic liquid to the anhydrous ethanol is preferably 0.2-0.4 g:10-20 mL, more preferably 0.25-0.35 g:12-18 mL, and more preferably 0.3 g:15-16 mL.

[0042] In the present invention, when the ionic liquid is a tetraethylenepentamine nitrate ionic liquid, the mass of the ionic liquid is preferably 25-35% of the total mass of the ionic liquid and the silanized modified carrier, further preferably 27-32%, and more preferably 29-30%; when the ionic liquid is a tetraethylenepentamine lysine salt ionic liquid, the mass of the ionic liquid is preferably 35-45% of the total mass of the ionic liquid and the silanized modified carrier, further preferably 38-42%, and more preferably 40%.

[0043] In the present invention, the immersion time in step 2) is preferably 5 to 7 hours, more preferably 5.5 to 6.5 hours, and more preferably 6 hours.

[0044] In step 2) of the present invention, after the impregnation is completed, the product is dried and cooled in sequence to obtain a modified KIT-6 composite material (2N-K6P-X or 2N-K6L-X), where P in 2N-K6P-X is [TEPA][NO3], L in 2N-K6L-X is [TEPA][Lys], and X is the mass fraction of the mass of the ionic liquid to the total mass of the ionic liquid and the silanized modified carrier 2N-KIT-6-X.

[0045] The present invention also provides a modified KIT-6 composite adsorbent prepared by the preparation method.

[0046] The present invention also provides the use of the modified KIT-6 composite adsorbent in adsorbing carbon dioxide.

[0047] In the present invention, the adsorption temperature is preferably 60 to 95°C, more preferably 75 to 90°C.

[0048] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0049] In the embodiments and comparative examples, tetraethylenepentamine (TEPA, purity is 99.5%), the mass fraction of the aqueous solution of nitric acid is 40%, the purity of N2 is 5N, and lysine (Lys, purity is 97%);

[0050] Polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer (P123, purity is AR, manufacturer is Sigma), hydrochloric acid (purity is AR, manufacturer is Xilong), n-butanol (BuOH, purity is 99.5%, manufacturer is Xilong), tetraethyl orthosilicate (TEOS, purity is AR, manufacturer is Xilong).

[0051] Example 1

[0052] The preparation method of tetraethylenepentamine nitrate ionic liquid is as follows: at room temperature, a round-bottom flask is purged with nitrogen to exhaust air, and then a 0.5 mol nitric acid aqueous solution is added dropwise to a TEPA aqueous solution (60 wt%) in an ice water environment at 5°C using a constant pressure funnel at a rate of 1 drop / s, and the molar ratio of TEPA to lysine is 1:1, and the reaction is continued at a rate of 450r / min in a three-necked flask at 25°C and N2 atmosphere for 8 hours to obtain an ionic liquid. The ionic liquid is then freeze-dried at -45°C for 5 days to remove the remaining water in the mixture until it is dry, and finally the ionic liquid is placed in a vacuum drying oven at 60°C (vacuum degree is -0.081MPa) for 24 hours to obtain a tetraethylenepentamine nitrate ionic liquid [TEPA][NO3].

[0053] The preparation method of tetraethylenepentamine lysine salt ionic liquid is as follows: a round-bottom flask is purged with nitrogen at room temperature to discharge the air in the flask, a TEPA aqueous solution (60 wt%) is placed in the round-bottom flask, lysine is added to the flask according to a molar ratio of TEPA to lysine of 1:1, and the ionic liquid is obtained by constant temperature reflux stirring (at a rate of 400 r / min) at 25°C under a nitrogen atmosphere for 8 hours. The ionic liquid is then freeze-dried at -45°C for 5 days to remove the remaining water in the mixture until it is dry, and finally the ionic liquid is placed in a vacuum drying oven at 60°C (vacuum degree of -0.081 MPa) for 24 hours to obtain tetraethylenepentamine lysine salt ionic liquid [TEPA][Lys].

[0054] The preparation method of KIT-6 molecular sieve is as follows: 4g P123 is dissolved in 142.39mL ultrapure water, and 6.32mL of hydrochloric acid with a mass fraction of 37% is added at the same time. The mixture is stirred in a water bath at 350r / min and 35°C until it becomes transparent white flocculent, and completely dissolved P123 is obtained. 4.90mL of n-butanol is added dropwise to the mixture at a rate of 2 drops / s and stirring is continued for 1h. The temperature is raised to 40°C, and 9.13mL of ethyl orthosilicate is added at a uniform rate at 450r / min to prepare a gel, and the mixture is stirred continuously for 24h. The liquid and the white precipitate in the three-necked flask are transferred into a high-pressure reactor together, and hydrothermally crystallized at 100°C for 24h. After the high-pressure reactor was cooled to room temperature, the precipitate was vacuum filtered (vacuum degree of 99.5 KPa, power of 180 W, time of 10 min) to remove excess water, and the filtered white solid was dried in an oven at 100 ° C for 24 h; the dried white powder was heated to 550 ° C in a muffle furnace at a heating rate of 1 ° C / min and calcined for 6 h to remove the template P123, thereby obtaining a white powdery ordered mesoporous silica KIT-6 molecular sieve.

[0055] The preparation method of 2N-KIT-6-1.5 is as follows: KIT-6 molecular sieve is placed in an oven at 100°C to dry, 1g of the dried KIT-6 molecular sieve sample is placed in a flat-bottomed flask, 100mL of toluene is added, and the mixture is stirred at a rate of 400r / min with a magnetic oil bath stirrer until homogeneous. The temperature is raised to 85°C, 1.5mL of N-[3-(trimethoxysilyl)propyl]ethylenediamine (2N) is slowly added dropwise at 85°C, a condenser is installed, and condensation reflux is continued for 16h. After the reaction is completed, the solid-liquid mixture is taken out, and the supernatant is removed by vacuum filtration (vacuum degree is 99.5KPa, power is 180W) to obtain a viscous white solid, the white solid is washed 4 times with anhydrous ethanol, and finally the viscous white solid is placed in an oven at 100°C to dry for 24h to obtain a silanized modified carrier, which is recorded as 2N-KIT-6-1.5.

[0056] The preparation method of 2N-K6P-30% is as follows: 0.3g [TEPA] [NO3] is dissolved in 15mL anhydrous ethanol, the mixed solution is placed in an ultrasonic cleaner and ultrasonicated at a power of 300W for 10 minutes to fully dissolve the ionic liquid, and then 0.7g 2N-KIT-6-1.5 powder is added after stirring at room temperature for 30 minutes in a magnetic stirrer. The mixed solution is continuously stirred for 6 hours, and placed in a forced air drying oven at 60°C for drying and evaporation for 18 hours to remove anhydrous ethanol, and finally placed in a vacuum drying oven at 60°C for 24 hours. After natural cooling, a modified KIT-6 composite adsorbent is obtained, which is recorded as 2N-K6P30%.

[0057] Example 2

[0058] The 0.3 g [TEPA] [NO3] in Example 1 was changed to 0.4 g [TEPA] [Lys], 0.7 g

[0059] The 2N-KIT-6-1.5 powder was changed to 0.6 g of 2N-KIT-6-1.5 powder, and the other conditions were the same as in Example 1 to obtain 2N-K6L40%.

[0060] Comparative Example 1

[0061] The [TEPA][NO3] in Example 1 was changed to 0.2g, 0.4g, and 0.5g, respectively, and the 2N-KIT-6-1.5 powder was correspondingly changed to 0.8g, 0.6g, and 0.5g, to obtain 2N-K6P20%, 2N-K6P40%, and 2N-K6P50%, respectively.

[0062] Comparative Example 2

[0063] The [TEPA][Lys] in Example 2 was changed to 0.2g, 0.3g, and 0.5g, respectively, and the 2N-KIT-6-1.5 powder was changed to 0.8g, 0.7g, and 0.5g accordingly, to obtain 2N-K6L20%, 2N-K6L30%, and 2N-K6L50%, respectively.

[0064] Performance test of the composite adsorbents of Examples 1 to 2 and Comparative Examples 1 to 2

[0065] Thermal stability test: The thermal stability of the material was tested using a microcomputer differential thermal balance with a sensitivity of 0.1 μg produced by Beijing Hengjiu Instrument Factory. Thermogravimetric analysis was performed using a TGA instrument in a N2 atmosphere. Before the experiment, the sample was dried in an oven at 80°C for 8 hours, with a N2 inlet flow rate of 100 mL min -1 , keep the temperature at 25℃ for 1h to eliminate interference, and then -1 The temperature was raised to 600°C, and the change in sample mass with temperature was calculated to determine the thermal stability of the material.

[0066] The TGA weight loss curves of the composite adsorbents of Examples 1 to 2 and Comparative Examples 1 to 2 and their corresponding DTG curves are as follows: Figure 1 As shown, A is the TGA weight loss curve and B is the DTG curve. Due to the release of CO2 and the evaporation of water, all samples experience the first stage of weight loss in the range of room temperature to 100°C. Amine volatilization and decomposition are the main reasons for the second stage of weight loss of the samples. For the 2N-K6P-X series samples, a large weight loss occurs in the range of 200-350°C, and the maximum weight loss rate occurs near 280°C; while for the 2N-K6L-X series samples, the second weight loss stage is mainly in the range of 120-250°C, and the maximum weight loss rate occurs near 180°C. Figure 1It can be seen that with the increase of ionic liquid loading, the corresponding composite adsorbent weight loss rate also increases. The weight loss rates of adsorbents 2N-K6P20%, 2N-K6P30%, 2N-K6P40% and 2N-K6P50% are 22.9%, 29.8%, 42.4% and 54.8%, respectively, while the weight loss rates of adsorbents 2N-K6L20%, 2N-K6L30%, 2N-K6L40% and 2N-K6L50% are 41.0%, 45.0%, 59.1% and 62.1%, respectively. The actual loading of 2N-K6P-X series adsorbents is close to the theoretical loading, but the 2N-K6L-X series samples have a larger weight loss rate, which is due to the decomposition of the grafted silane modifier 2N. All samples showed no obvious weight loss after 550 °C, and the composite adsorbents impregnated with [TEPA][NO3] and [TEPA][Lys] showed thermal stability within 280 °C and 180 °C, respectively, indicating that the regeneration and desorption temperature of 110 °C is suitable for the cyclic adsorption and desorption process.

[0067] FTIR test: KIT-6, 2N-KIT-6-1.5, 2N-K6P30% of Example 1 and 2N-K6L40% of Example 2 were analyzed by Fourier transform infrared spectroscopy (model 470FTIR, manufacturer: Thermo Fisher Scientific Inc., USA). Figure 2 As shown. The experiment adopted KBr (purity is SP, manufacturer is Xilong) tableting method. Before testing, the sample was dried in an oven at 100°C for 12 hours. The whole sample preparation process was carried out under the irradiation of infrared light. First, the spectral grade KBr was ground into white powder in an agate mortar, and then the sample to be tested (the mass ratio of sample to KBr is 1:120) was added and fully mixed and ground, and a very thin transparent sheet was pressed out with a tablet press. Before measuring, the background value was first scanned, and then the prepared thin slice was placed in a Fourier infrared spectrometer for scanning measurement. The spectral scanning range was 4000~400cm -1 .

[0068] Depend on Figure 2 It can be seen that the wave number is 3435cm -1 、1632cm -1 、1080cm -1 、808cm -1 and 460cm -1 The infrared absorption peaks near 3435cm -1 The absorption peak at 1632cm is the OH bond vibration peak, which is caused by the adsorbed water on the adsorbent surface and the antisymmetric stretching vibration of OH generated during the immersion process; -1 It is caused by the complete vibration of the OH bonds on the surface of the adsorbent material after adsorption of water and modification; 1080cm -1 、808cm-1 and 460cm -1 They are the antisymmetric stretching vibration, symmetric stretching vibration and bending vibration of Si-O-Si groups in the material. After grafting 2N, the infrared spectrum of 2N-KIT-6-1.5 shows that 1476 cm -1 The CH bending vibration appears at 1632cm -1 The absorption peak at the KIT-6 is weakened, which is attributed to the acetal reaction between the Si-OH on KIT-6 and the methoxy group in 2N to form a siloxy group. The reaction formula is: Si-OH+RNH2→Si-O - N + H3R Si-OH+R2NH→Si-O - N + H2R2.

[0069] Using 2N-KIT-6-1.5 as the carrier, the ionic liquids [TEPA][NO3] and [TEPA][Lys] were impregnated at 2976 cm -1 、2860cm -1 and 1572cm -1 There is an absorption peak at 2976cm -1 and 2860cm -1 The symmetric and asymmetric vibrations of the CH bond are 1572 cm -1 The NH bond bending vibration of the primary amine is shown in Figure 1. According to the infrared spectrum, [TEPA][NO3] and [TEPA][Lys] were successfully impregnated onto the carrier 2N-KIT-6-1.5.

[0070] Low-temperature nitrogen adsorption-desorption test: The JW-BK200C fully automatic specific surface area analyzer (Jingwei Gaobo, Beijing) was used to carry out N2 adsorption and desorption measurement at a liquid nitrogen temperature of 77K. Before the test, the adsorbent material was dried at 80℃ for 12h, pretreated at 150℃ and vacuum for 2h (vacuum degree of 5Pa), and then adsorbed and desorbed on liquid nitrogen at low temperature. The specific surface area, pore volume and pore size distribution of the material can be calculated based on the adsorption-desorption isotherms measured experimentally, the BET method and the BJH method.

[0071] The 2N-KIT-6-1.5 of Example 1, the composite adsorbents of Examples 1-2 and Comparative Examples 1-2 were subjected to low temperature nitrogen adsorption and desorption tests at 77K. The results are as follows: Figure 3 , Figure 4 And as shown in Table 1. Figure 3These are the adsorption-desorption isotherms of the samples after different impregnation amounts of ionic liquid [TEPA][Lys] were loaded on 2N-KIT-6-1.5. The modified samples of the ionic liquid [TEPA][Lys] series all showed narrow hysteresis loops. As can be seen from Table 1, the pore size of the samples of the 2N-K6L-X series is almost much smaller than that of the samples of the 2N-K6P-X series, which is the reason for the narrow hysteresis loop of the 2N-K6L-X series. Figure 4 It is the adsorption-desorption isotherms of 2N-KIT-6-1.5 of Example 1 and the adsorbents of Examples 1 to 2. It can be seen that the materials before and after modification show type IV adsorption isotherms, indicating that the pore structure of the material has not been changed.

[0072] Table 1 Physical properties and CO2 adsorption of 2N-KIT-6-1.5 and composite adsorbents

[0073]

[0074] As shown in Table 1, for the 2N-K6P-X series samples, with the increase of loading, the pore volume, specific surface area and pore size of the composite adsorbent are decreasing, from 0.220 cm 3 ·g -1 、40.636m 2 ·g -1 and 19.201nm down to 0.022cm 3 ·g -1 、26.991m 2 ·g -1 and 6.203nm; while for the 2N-K6L-X series samples, when the loading amount continues to increase, the corresponding pore volume and pore diameter remain basically unchanged, while the specific surface area increases from 52.628m 2 ·g -1 Down to 2.957m 2 ·g -1 .

[0075] Element analysis: The nitrogen content in the samples of Examples 1 to 2 and Comparative Examples 1 to 2 was detected using an EA2400Ⅱ element analyzer (manufacturer Per-Elmer, USA, model EA2400Ⅱ). The adsorption efficiency of the composite adsorbent for amines is as follows: Figure 5 The material was pretreated in an oven at 80°C for 8 hours before testing, and the average value of three experiments was taken as the experimental test data. Figure 5It can be seen that for the 2N-K6P-X series, with the increase of the loading amount, the corresponding material amine efficiency first increases and then decreases, and reaches a maximum value of 0.294 when the loading amount is 30%. The maximum is reached at this time because the material pores maintain good porosity while loading relatively high amine groups, which basically does not affect the diffusion of gas CO2, and the loaded amine groups provide more active sites for adsorbing CO2; but for the 2N-K6L-X series, with the increase of the loading amount, the corresponding material amine efficiency first decreases, then increases, and then decreases, reaching a maximum value of 0.319 when the loading amount is 40%. The amine efficiency of the 2N-K6P-X and 2N-K6L-X series samples is lower than that of 2N-KIT-1.5, which is 0.456. This is because when the 2N grafting amount is fixed, with the increase of [TEPA][NO3] and [TEPA][Lys] loading, the pores of the composite material are gradually filled with modifiers, and the active amine groups are accumulated and covered, thereby weakening the amine utilization efficiency.

[0076] CO2 adsorption performance test: A microcomputer differential thermal analysis balance with a sensitivity of 0.1μg (Beijing Hengjiu, HCT-1) produced by Beijing Hengjiu Instrument Factory was used to determine the CO2 adsorption performance and cyclic stability of the material. The CO2 adsorption performance of the sample was measured using the TGA thermogravimetric method. The composite adsorbent was first dried at 80°C for 12h. Before the experiment began, the instrument was turned on for ventilation and preheating, and the airflow rate on the instrument balance and display screen was stabilized. 6mg of the sample was placed in a quartz crucible on the microcomputer differential thermal analysis balance. First, high-purity N2 was introduced to heat and remove impurities such as moisture to constant weight, and then the temperature was lowered and a simulated flue gas mixture CO2 / N2 (Guangxi Ruida, purity of 5N, CO2 volume fraction in the mixed gas is 15%) was introduced to make the mass of the experimental sample material reach adsorption saturation. Finally, the CO2 adsorption amount was calculated based on the mass difference of the adsorbent sample after CO2 adsorption. The above experiments were all carried out under normal pressure. The calculation formula is:

[0077]

[0078] In formula 1, q e is the maximum adsorption capacity, mmol·g -1 ; m0 is the mass of the sample before adsorption (i.e. the mass of the sample when CO2 was initially introduced), mg, m e is the mass of the sample after adsorption saturation, mg.

[0079] The specific heating process is as follows: After the crucible is placed on the balance, firstly, high-purity nitrogen (100mL / min) is introduced and kept warm for 1h, then the temperature is raised to 110℃ at 10℃ / min, and the temperature is kept at 110℃ for 50min to remove gas impurities and moisture in the sample to be tested to eliminate background interference. Then the adsorption temperature is lowered to 60℃ and kept warm for 20min, and finally the gas flow is switched to a mixed gas N2 / CO2 (60mL / min) and introduced into the furnace balance. At this time, the sample to be tested begins to adsorb gas CO2, and the mixed gas is continuously introduced for 200min to ensure that the adsorption reaches equilibrium.

[0080] The CO2 adsorption curves of the composite adsorbents of Examples 1 to 2 and Comparative Examples 1 to 2 are as follows: Figure 6 As shown, A is Example 1 and Comparative Example 1, and B is Example 2 and Comparative Example 2. Figure 6 A shows that at 60°C, as the loading amount increases, the adsorption amount increases first and then decreases. From 2N-K6P20% to 2N-K6P30%, the CO2 adsorption amount of the composite adsorbent sample increases with the increase of the modifier loading amount; while from 2N-K6P30% to 2N-K6P50%, the CO2 adsorption amount of the composite adsorbent sample decreases with the increase of the modifier loading amount. When and only when the loading amount is 30%, the modified composite sample reaches the optimal value (1.497mmol·g -1 When the modifier loading exceeds 30%, the relatively excessive organic amine will accumulate in the pores and gaps of the material and cover the surface of the material, increasing the steric hindrance and increasing the diffusion resistance of the gas CO2, thus weakening the CO2 adsorption performance of the material.

[0081] Depend on Figure 6 B shows that at 60°C, the composite adsorbent loaded with [TEPA][NO3] exhibits the same phenomenon. With the increase of [TEPA][Lys] loading, the CO2 adsorption of the composite adsorbent increases first and then decreases. From 2N-K6L20% to 2N-K6P40%, the CO2 adsorption of the composite adsorbent sample increases with the increase of the modifier loading; while from 2N-K6P40% to 2N-K6P50%, the CO2 adsorption of the composite adsorbent sample decreases with the increase of the modifier loading. When and only when the loading is 40%, the modified composite sample reaches the optimal value (2.509mmol·g -1 adsorbent).

[0082] When the loading amount of ionic liquid increases, the CO2 adsorption capacity of its composite adsorbent shows a trend of first increasing and then decreasing. The reason is that when the loading amount of the material is relatively low, increasing the loading amount of the modifier allows the material surface to carry more amine active sites, thereby increasing the gas CO2 adsorption amount. When the loading amount continues to increase, the amine groups will agglomerate together and block the pores, increasing the diffusion resistance of the gas CO2 and reducing the adsorption performance.

[0083] Adsorption regeneration performance test: The composite adsorbent was subjected to five cycles of regeneration performance test. The adsorption temperature of the cycle experiment was set to 60°C and the desorption temperature was set to 110°C. The steps are as follows: When the sample adsorbs the mixed gas CO2 / N2 (gas flow rate 60mL / min) to reach adsorption equilibrium, the gas is switched to high-purity N2 and the temperature is raised to 110°C at a heating rate of 10°C / min to allow the adsorbent material to desorb at high temperature. When the sample is completely desorbed, the temperature is cooled to 60°C, and the gas is switched to the mixed gas CO2 / N2 (gas flow rate 60mL / min) for adsorption. This is repeated for five cycles. The experimental steps of each cycle are the same as those in the CO2 adsorption performance test to measure its adsorption regeneration performance.

[0084] The composite adsorbents of Example 1 and Example 2 were tested for their CO2 adsorption and regeneration performance at 30°C, 45°C, 60°C, 75°C, and 90°C. Figure 7 As shown, A is Example 1 and B is Example 2. For the adsorbent 2N-K6P30%, as the temperature increases, its CO2 adsorption capacity also increases, and reaches the optimal adsorption capacity of 1.871 mmol·g at 90°C. -1 For the adsorbent 2N-K6L40%, as the adsorption temperature increases, its adsorption performance also increases substantially, reaching a maximum value of 3.670mmol·g at 90℃. -1 The reaction between CO2 and amine is exothermic. If the temperature continues to increase, it will be unfavorable for the amine to adsorb gas CO2. In addition, the temperature will rise to the desorption temperature, and the adsorbed gas CO2 will desorb on the surface of the material. Therefore, the optimal adsorption temperature of both adsorbents is 90°C.

[0085] In practical applications, CO2 capture also requires factors such as efficient CO2 adsorption performance, good stability and low cost. The cycle performance was determined by the TGA method. A CO2 (15 vol%) / N2 (85 vol%) mixed gas was introduced at 60°C to simulate flue gas. The composite adsorbents 2N-K6P30% and 2N-K6L40% of Examples 1 and 2 were subjected to cyclic adsorption, desorption and regeneration experiments. The results are shown in Figure 2. Figure 8 After 5 cycles of adsorption and desorption, the saturation amounts of 2N-K6P30% and 2N-K6L40% were 1.344 mmol·g -1and 2.259mmol·g -1 Compared with the initial value, the adsorption amount decreased by 13.3% and 12.3%, respectively. In the regeneration experiment, the main reason for the reduction of the adsorption saturation capacity of the sample was the volatilization of organic amine and silane grafting agent and the incomplete desorption of CO2. In general, the regeneration performance of the modified composite adsorbent material remained stable.

[0086] Kinetic analysis: In the gas-solid phase, after amino functionalization, the adsorption process on the adsorbent surface is no longer a simple physical adsorption process, and the adsorption rate is also affected by the mass transfer process. In order to explore its adsorption mechanism, the Avrami model was used to fit the adsorption data of the modified adsorbent material at different temperatures to study its adsorption process mechanism.

[0087] The Avrami model equation is as follows:

[0088]

[0089] In formula 2, q t is the CO2 adsorption capacity at any time t, mmol·g -1 ;q e is the CO2 saturated adsorption capacity when reaching equilibrium, mmol·g -1 ;k A is the rate constant of the Avrami equation, min -1 ;n A is the Avrami equation series.

[0090] The Avrami model was used to fit the CO2 adsorption data of the composite adsorbents of Examples 1 and 2 at 30°C, 45°C, 60°C, 75°C and 90°C. Fig. 9 is the fitting result of the adsorbent at different temperatures, and the corresponding fitting data are shown in Table 2.

[0091] Table 2 Kinetic parameters of CO2 adsorption by composite adsorbent at different adsorption temperatures

[0092]

[0093] Note: e a ,q e b are experimental test value and theoretical fitting value, mmol·g -1 .

[0094] The equilibrium adsorption values ​​fitted by the Avrami model are very close to the experimentally measured adsorption amounts. At 30℃, 45℃, 60℃, 75℃ and 90℃, the fitting data of adsorbent 2N-K6P30% are 1.250mmol·g -1, 1.422mmol·g -1 、1.446mmol·g -1 、1.737mmol·g -1 , 1.854mmol·g -1 , the fitting data of 2N-K6L40% were 1.857mmol·g -1 , 2.108mmol·g -1 , 2.626mmol·g -1 , 2.224mmol·g -1 、3.732mmol·g -1 . Correlation coefficient R 2 are much higher than 0.99. Fig. 9 A and 9B show that the Avrami model fitting curve is very consistent, indicating that the model can describe the adsorption process of the adsorbent very well, indicating that the CO2 adsorption process of the modified adsorbent is also the result of physical and chemical synergy. For these two adsorbents, the adsorption process can be divided into two stages. The initial stage can be regarded as the chemical reaction between the gas CO2 in the hot furnace cavity and the amino active sites on the surface of the material to form carbamate substances; the second stage can be regarded as the excessive carbamate substances gathering on the surface of the adsorbent and blocking the carrier pores, and the gas CO2 adsorption rate decreases until the adsorption equilibrium is reached.

[0095] In the present invention, 2N is used as a grafting agent and KIT-6 is used as a carrier. A dry grafting method is first used, followed by physical impregnation of ionic liquids [TEPA][NO3] and [TEPA][Lys]. In the range of loading amount of 25-45%, at 60°C and normal pressure, 2N-K6P30% exhibits an optimal adsorption value of 1.497 mmol·g -1 The optimal loading amount of the series of samples loaded with [TEPA][Lys] was 40%, and the adsorption amount of 2N-K6L 40% was 2.509 mmol·g -1 The adsorption capacity of 2N-K6L40% at 90℃ is as high as 3.670mmol·g -1 The Avrami model was used to fit the adsorption data of the best adsorbent at different temperatures, which can better describe the adsorption process of the composite adsorbent, which is the combined effect of physical adsorption and chemical adsorption. After 5 adsorption and desorption cycles, the composite adsorbent sample still has good regeneration performance.

[0096] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. Application of a modified KIT-6 composite adsorbent in adsorbing carbon dioxide, characterized in that: The preparation method of the modified KIT-6 composite adsorbent comprises the following steps: 1) reacting KIT-6 molecular sieve, toluene and N-[3-(trimethoxysilyl)propyl]ethylenediamine to obtain a silanized modified carrier; 2) impregnating the silanized modified carrier with an anhydrous ethanol solution of ionic liquid to obtain a modified KIT-6 composite adsorbent; The ionic liquid is a tetraethylenepentamine lysine salt ionic liquid; the mass of the ionic liquid is 40% of the total mass of the ionic liquid and the silanized modified carrier.

2. The use according to claim 1, characterized in that: Step 1) The mass volume ratio of the KIT-6 molecular sieve and toluene is 1 g: 90-110 mL, and the mass volume ratio of the KIT-6 molecular sieve and N-[3-(trimethoxysilyl)propyl]ethylenediamine is 1 g: 1.2-1.8 mL.

3. The use according to claim 1 or 2, characterized in that: Step 1) The reaction temperature is 80-90°C and the reaction time is 14-18 h.