A sodium ion battery positive electrode material and its preparation method and application

By synthesizing Na4[FexFe3-x](PO4)2(P2O7)@C sodium ion battery positive electrode material using composite iron source, the problem of low specific capacity of iron-based mixed phosphate positive electrode material is solved, and electrochemical performance and cycle stability are improved , suitable for large-scale energy storage system applications.

CN116534830BActive Publication Date: 2024-12-03ANHUI XINNA MATERIAL SCIENCE & TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310619400.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-29
Publication Date
2024-12-03
Estimated Expiration
2043-05-29

AI Technical Summary

Technical Problem

The existing iron-based mixed phosphate cathode materials have lower specific capacity, limited electronic conductivity and ion diffusion, resulting in poor electrochemical performance and difficult to effectively apply in large-scale energy storage systems.

Method used

The positive electrode material of Na4[FexFe3-x](PO4)2(P2O7)@C sodium ion battery is synthesized by composite iron source, and the sodium source, phosphorus source, carbon source and different iron sources are mixed and calcined to form high crystallinity and conductivity. A composite with good properties increases the discharge specific capacity and cycle stability of the material.

Benefits of technology

It improves the discharge specific capacity and cycle stability of the material. The capacity has almost no attenuation after 500 cycles of 10C. It is suitable for large-scale production and has excellent electrochemical performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116534830B_ABST
    Figure CN116534830B_ABST
Patent Text Reader

Abstract

The present invention discloses a sodium ion battery positive electrode material and a preparation method and application thereof, belonging to the technical field of sodium ion batteries. x Fe 3‑x ](PO4)2(P2O7)@C sodium ion battery positive electrode material not only improves the crystallinity of the material but also enhances the conductivity of the electrode material, thereby improving the discharge capacity and cycle stability of the material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of sodium ion batteries, and in particular relates to a sodium ion battery positive electrode material and a preparation method and application thereof. Background Art

[0002] In recent years, global problems such as fossil fuel shortages and environmental pollution have become increasingly serious, and people are urgently developing clean energy such as solar energy, wind energy and hydropower. However, these clean energy sources have disadvantages such as large volatility, poor stability and intermittent supply, and they need to be integrated and converted by large-scale energy storage devices before they can be reasonably used. Among the existing energy storage technologies, secondary batteries are considered to be one of the ideal choices for large-scale energy storage technology due to their strong flexibility and high energy conversion efficiency. Although lithium-ion batteries have achieved great success in the fields of portable electronic devices and electric vehicles due to their high energy density and good cycle stability, they cannot meet the cheap requirements of large-scale energy storage due to the scarcity and uneven distribution of lithium resources. However, sodium-ion batteries have a similar working principle to lithium-ion batteries, and their reserves are more abundant and their distribution is more widespread. Considering the key feature that the value cost of large-scale energy storage devices is greater than the energy density, sodium-ion batteries are considered to be one of the potential candidates for large-scale energy storage systems.

[0003] A large number of sodium-ion battery cathode materials have been reported, but only a few of them have shown good electrochemical properties, such as vanadium-based phosphates, iron-based phosphates, and Prussian blue analogs. In addition, in the process of commercializing laboratory results, these materials also face some serious problems, such as the high toxicity and high cost of vanadium-based materials and the structural instability of Prussian blue analogs. Among iron-based phosphates, sodium iron phosphate pyrophosphate (Na4Fe3(PO4)2P2O7) combines the advantages of all iron-based phosphates: low cost, environmental friendliness, high theoretical capacity (129mAh g -1 ), high average operating voltage (3.1VS.Na + / Na) and low volume expansion (less than 4%), as well as iron-based mixed phosphate cathode materials, are a class of sodium-ion battery cathode materials with great commercial application potential from the perspective of raw material acquisition and structural stability. It is considered to be the most promising sodium-ion battery cathode material. However, the specific capacity of the iron-based mixed phosphate cathode material synthesized by the solid phase method is low. In addition, the large size of PO4 3- The inherent isolation properties of the groups lead to lower electronic conductivity and slow ion diffusion, which limits their specific capacity. Therefore, it is particularly important to solve the problem of low specific capacity of iron-based mixed phosphate positive electrode materials.

[0004] For example, the patent application with publication number CN112768673A discloses a Na4Fe 3-x(PO4)2P2O7 / C sodium ion battery positive electrode material and its preparation method and application; The sodium ion battery positive electrode material introduces iron defects in the structure and can be simply prepared by reducing the iron source content in the raw material, without the need for new raw materials and additional synthesis processes, with minimal impact on the existing manufacturing process and easy control. The prepared Na4Fe 3-x (PO4)2P2O7 / C has high purity, good crystallinity, high ionic and electronic conductivity, which greatly improves the specific capacity and rate performance of the positive electrode material and is suitable for large-scale production applications. Summary of the invention

[0005] In view of this, the present invention provides a Na4[Fe x Fe 3-x ](PO4)2(P2O7)@C sodium ion battery positive electrode material and preparation method and application thereof, the positive electrode material comprises Na4[Fe x Fe 3-x ](PO4)2(P2O7) and a composite amorphous carbon layer loaded on the surface of the compound. The raw material sodium source, composite iron source, phosphorus source and carbon source are uniformly mixed and then calcined. The synthesis process of the positive electrode material only uses a composite iron source in the selection of the iron source, without the need for new raw materials and additional synthesis processes, and has little impact on the existing manufacturing process. The positive electrode material synthesized using the composite iron source has the characteristics of high crystallinity, high capacity, good cycle stability, and excellent low temperature performance.

[0006] The specific technical solutions of the present invention are as follows:

[0007] A sodium ion battery positive electrode material, the general formula of the sodium ion battery positive electrode material is Na4[Fe x Fe 3-x ](PO4)2(P2O7)@C, the positive electrode material of the sodium ion battery is Na4[Fe x Fe 3-x ](PO4)2(P2O7) and C complex,

[0008] Among them, 0.9≤x<2.1, Fe x The iron source used is the first iron source, Fe 3-x The iron source used is a second iron source, and the first iron source and the second iron source are any two of ferric phosphate, ferric oxide, ferrous citrate, ferrous oxalate, ferrous acetylacetonate, ferric nitrate, ferric chloride, and ferrous sulfate;

[0009] The preparation method comprises the following steps:

[0010] (1) adding a sodium source, a phosphorus source, and a carbon source to water, mixing them evenly to form a solution, then adding a first iron source and a second iron source, mixing them evenly to form a slurry, and drying to obtain a precursor powder;

[0011] (2) calcining the precursor powder obtained in step (1) under an inert atmosphere to obtain a positive electrode material for a sodium ion battery.

[0012] According to the above scheme, Na4[Fe x Fe 3-x ]The mass ratio of (PO4)2(P2O7) and C is 98:2~97:3.

[0013] According to the above scheme, 0.9≤x≤1.5.

[0014] Specifically, in step (1),

[0015] The sodium source is at least one of sodium carbonate, sodium chloride, disodium hydrogen phosphate, sodium dihydrogen phosphate, sodium nitrate, sodium oxalate, sodium pyrophosphate, tripolyphosphoric acid, and sodium ethoxide;

[0016] The carbon source is at least one of sucrose, glucose, citric acid, polyethylene glycol, oxalic acid, sodium carbonate and ascorbic acid.

[0017] Specifically, in step (1), grinding is performed using a sand mill before drying;

[0018] The speed of the sand mill is 2000r / min, the flow rate is 200L / h, and the grinding time is 40-100min;

[0019] The solid content of the slurry after grinding is 45%-50%, and the sand grinding particle size is 300-350nm.

[0020] In step (1), the drying method is spray drying, blast drying or vacuum drying;

[0021] When the drying method is spray drying, the feed rate of spray drying is 60-90 mL / min, the frequency of the atomizing disk is 450 Hz, the feed temperature is 220° C., and the discharge temperature is 90-100° C.

[0022] Wet homogeneous sand milling combined with spray drying is an effective method for batch preparation of spherical powders with uniform particle size. It can achieve uniform dispersion of precursor salts at the nanoscale and improve the purity and electrical properties of the powders.

[0023] Preferably, in step (2), the calcination conditions are: calcination at a temperature of 500-550° C. for 10-13 hours.

[0024] The calcination parameters are more conducive to the formation of the final material. If the calcination temperature is too high, the material will be over-burned and there will be impurities. If the calcination temperature is too low, the sintering will be insufficient, resulting in low crystallinity of the material. Due to the high-temperature decomposition of sucrose in an inert atmosphere, part of the carbon is coated on the surface of the main material, and the carbon coating is conducive to increasing the conductivity of the material.

[0025] The present invention also provides a sodium ion battery positive electrode material prepared by the above preparation method.

[0026] The present invention also provides the use of the above-mentioned sodium ion battery positive electrode material in the preparation of a sodium ion battery.

[0027] The present invention also provides a sodium ion battery, comprising the sodium ion battery positive electrode material.

[0028] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0029] (1) The present invention uses a composite iron source to synthesize Na4[Fe x Fe 3-x ](PO4)2(P2O7)@C sodium ion battery positive electrode material, while improving the material crystallinity, it also enhances the conductivity of the electrode material, thereby improving the material's discharge capacity and cycle stability. x Fe 3-x The (PO4)2(P2O7)@C material is assembled into a battery. In the voltage range of 1.7 to 4.0 V, the charge and discharge capacity can reach 107 mAh g at a rate of 0.1C. -1 During the charge and discharge process, it has good cycle performance due to its stable structure. After 500 cycles at 10C, the capacity has almost no attenuation. x Fe 3-x ](PO4)2(P2O7)@C positive electrode material exhibits excellent electrochemical performance.

[0030] (2) Synthesis of Na4[Fe x Fe 3-x ](PO4)2(P2O7)@C sodium ion battery positive electrode material has no difference in process synthesis except that two different iron sources are used in the raw material input stage, and is suitable for large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is the XRD curve of the composite positive electrode material obtained in Example 2.

[0032] Figure 2 This is a scanning electron microscope (SEM) image of the composite positive electrode material prepared in Example 2.

[0033] Figure 3 This is the XRD curve of the composite positive electrode material prepared in Comparative Example 1.

[0034] Figure 4 This is a scanning electron microscope (SEM) image of the composite positive electrode material prepared in Comparative Example 1.

[0035] Figure 5 This is a scanning electron microscope (SEM) image of the composite positive electrode material prepared in Comparative Example 2. DETAILED DESCRIPTION

[0036] Example 1

[0037] A sodium ion secondary battery positive electrode material Na4[Fe x Fe 3-x ]A method for preparing (PO4)2(P2O7)@C, wherein x=0.9, comprises the following steps:

[0038] (1) According to the stoichiometric ratio, 847.9 g of sodium carbonate, 1438.8 g of diammonium phosphate, and a composite carbon source consisting of 130 g of sucrose and 180 g of polyethylene glycol were weighed and added to deionized water, and stirred to form a solution; then 543.0 g of iron phosphate and 670.7 g of iron oxide were added, and stirred to form a slurry; the slurry was poured into a storage tank, and ground in a sand mill at a speed of 2000 r / min and a flow rate of 200 L / h for 100 min, and the particle size after sand grinding was controlled between 200 and 300 nm; the molar ratio of sodium element, iron element, and phosphorus element in the mixture was 4:3:4;

[0039] (2) spray drying the slurry obtained in step (1) at an inlet temperature of 220° C. and an outlet temperature of 95° C. to obtain a precursor powder;

[0040] (3) The precursor powder obtained by spray drying was heated to 300°C at a heating rate of 2°C / min in an inert atmosphere of nitrogen, and kept at this temperature for 5 h. It was then heated to 500°C at a heating rate of 2°C / min and calcined, and kept at this temperature for 10 h. 0.9 Fe 2.1 ](PO4)2(P2O7)@C composite positive electrode material.

[0041] Example 2

[0042] A sodium ion secondary battery positive electrode material Na4[Fe x Fe 3-x ](PO4)2(P2O7)@C, wherein x=1.2, comprises the following steps:

[0043] (1) 847.9 g of sodium carbonate, 1438.8 g of ammonium dihydrogen phosphate, and a composite carbon source consisting of 130 g of sucrose and 180 g of polyethylene glycol were weighed and added to deionized water according to a stoichiometric ratio, and stirred to form a solution; 723.9 g of iron phosphate and 574.9 g of iron oxide were then added and stirred to form a slurry; the slurry was poured into a storage tank, and ground in a sand mill at a speed of 2000 r / min and a flow rate of 200 L / h for 120 min, and the particle size after sand grinding was controlled to be between 200 and 300 nm; the molar ratio of sodium element, iron element, and phosphorus element in the mixture was 4:3:4;

[0044] (2) spray drying the slurry obtained in step (1) at an inlet temperature of 220° C. and an outlet temperature of 95° C. to obtain a precursor powder;

[0045] (3) The precursor powder obtained by spray drying was heated to 300°C at a heating rate of 2°C / min in an inert atmosphere of nitrogen, and kept at this temperature for 5 h. It was then heated to 500°C at a heating rate of 2°C / min and calcined, and kept at this temperature for 10 h. 1.2 Fe 1.8 ](PO4)2(P2O7)@C composite positive electrode material.

[0046] Example 3

[0047] A sodium ion secondary battery positive electrode material Na4[Fe x Fe 3-x ](PO4)2(P2O7)@C, wherein x=1.5, comprises the following steps:

[0048] (1) 847.9 g of sodium carbonate, 1438.8 g of ammonium dihydrogen phosphate, and a composite carbon source consisting of 130 g of sucrose and 180 g of polyethylene glycol were weighed and added to deionized water according to a stoichiometric ratio, and stirred to form a solution; 904.9 g of iron phosphate and 479.1 g of iron oxide were then added, and stirred to form a slurry; the slurry was poured into a storage tank, and ground in a sand mill at a speed of 2000 r / min and a flow rate of 200 L / h for 120 min, and the particle size after sand grinding was controlled to be between 200 and 300 nm; the molar ratio of sodium element, iron element, and phosphorus element in the mixture was 4:3:4;

[0049] (2) spray drying the slurry obtained in step (1) at an inlet temperature of 220° C. and an outlet temperature of 95° C. to obtain a precursor powder;

[0050] (3) The precursor powder obtained by spray drying was heated to 300°C at a heating rate of 2°C / min in an inert atmosphere of nitrogen, and kept at this temperature for 5 h. It was then heated to 500°C at a heating rate of 2°C / min and calcined, and kept at this temperature for 10 h. 1.5 Fe 1.5 ](PO4)2(P2O7)@C composite positive electrode material.

[0051] Example 4

[0052] A sodium ion secondary battery positive electrode material Na4[Fe x Fe 3-x ](PO4)2(P2O7)@C, wherein x=1.8, comprises the following steps:

[0053] (1) 847.9 g of sodium carbonate, 1438.8 g of ammonium dihydrogen phosphate, and a composite carbon source consisting of 130 g of sucrose and 180 g of polyethylene glycol were weighed and added to deionized water according to a stoichiometric ratio, and stirred to form a solution; then 1053.3 g of iron phosphate and 383.3 g of iron oxide were added, and stirred to form a slurry; the slurry was poured into a storage tank, and ground in a sand mill at a speed of 2000 r / min and a flow rate of 200 L / h for 100 min, and the particle size after sand grinding was controlled between 200 and 300 nm; the molar ratio of sodium element, iron element, and phosphorus element in the mixture was 4:3:4;

[0054] (2) spray drying the slurry obtained in step (1) at an inlet temperature of 220° C. and an outlet temperature of 95° C. to obtain a precursor powder;

[0055] (3) The precursor powder obtained by spray drying was heated to 300°C at a heating rate of 2°C / min in an inert atmosphere of nitrogen, and kept at this temperature for 5 h. It was then heated to 500°C at a heating rate of 2°C / min and calcined, and kept at this temperature for 10 h. 1.8 Fe 1.2 ](PO4)2(P2O7)@C composite positive electrode material.

[0056] Example 5

[0057] A sodium ion secondary battery positive electrode material Na4[Fe x Fe 3-x ](PO4)2(P2O7)@C, wherein x=2.1, comprises the following steps:

[0058] (1) 847.9 g of sodium carbonate, 1438.8 g of ammonium dihydrogen phosphate, and a composite carbon source consisting of 130 g of sucrose and 180 g of polyethylene glycol were weighed and added to deionized water according to a stoichiometric ratio, and stirred to form a solution; then 1228.8 g of iron phosphate and 287.4 g of iron oxide were added, and stirred to form a slurry; the slurry was poured into a storage tank, and ground in a sand mill at a speed of 2000 r / min and a flow rate of 200 L / h for 120 min, and the particle size after sand grinding was controlled to be between 200 and 300 nm; the molar ratio of sodium element, iron element, and phosphorus element in the mixture was 4:3:4;

[0059] (2) spray drying the slurry obtained in step (1) at an inlet temperature of 220° C. and an outlet temperature of 95° C. to obtain a precursor powder;

[0060] (3) The precursor powder obtained by spray drying was heated to 300°C at a heating rate of 2°C / min in an inert atmosphere of nitrogen, and kept at this temperature for 5 h. It was then heated to 500°C at a heating rate of 2°C / min and calcined, and kept at this temperature for 10 h. 2.1 Fe 0.9 ](PO4)2(P2O7)@C composite positive electrode material.

[0061] Comparative Example 1

[0062] A sodium ion secondary battery positive electrode material Na4[Fe x Fe 3-x ](PO4)2(P2O7)@C, wherein x=3, comprises the following steps:

[0063] (1) 847.9 g of sodium carbonate, 1438.8 g of ammonium dihydrogen phosphate, and a composite carbon source consisting of 130 g of sucrose and 180 g of polyethylene glycol were weighed and added to deionized water according to a stoichiometric ratio, and stirred to form a solution; 1809.8 g of iron phosphate was then added, and stirred to form a slurry; the slurry was poured into a storage tank, and ground in a sand mill at a speed of 2000 r / min and a flow rate of 200 L / h for 100 min, and the particle size after sand grinding was controlled to be between 200 and 300 nm; the molar ratio of sodium element, iron element, and phosphorus element in the mixture was 4:3:4;

[0064] (2) spray drying the slurry obtained in step (1) at an inlet temperature of 220° C. and an outlet temperature of 95° C. to obtain a precursor powder;

[0065] (3) The precursor powder obtained by spray drying was heated to 300°C at a heating rate of 2°C / min in an inert atmosphere of nitrogen, and kept warm for 5 h. It was then heated to 500°C at a heating rate of 2°C / min and calcined, and kept warm for 10 h to obtain a Na4[Fe3Fe0](PO4)2(P2O7)@C composite positive electrode material.

[0066] Comparative Example 2

[0067] A sodium ion secondary battery positive electrode material Na4[Fe x Fe 3-x ](PO4)2(P2O7)@C, wherein x=0, comprises the following steps:

[0068] (1) 847.9 g of sodium carbonate, 1438.8 g of ammonium dihydrogen phosphate, and a composite carbon source consisting of 130 g of sucrose and 180 g of polyethylene glycol were weighed and added to deionized water according to a stoichiometric ratio, and stirred to form a solution; 958.1 g of iron oxide was then added, and stirred to form a slurry; the slurry was poured into a storage tank, and ground in a sand mill at a speed of 2000 r / min and a flow rate of 200 L / h for 120 min, and the particle size after sand grinding was controlled to be between 200 and 300 nm; the molar ratio of sodium element, iron element, and phosphorus element in the mixture was 4:3:4;

[0069] (2) spray drying the slurry obtained in step (1) at an inlet temperature of 220° C. and an outlet temperature of 95° C. to obtain a precursor powder;

[0070] (3) The precursor powder obtained by spray drying was heated to 300°C at a heating rate of 2°C / min in an inert atmosphere of nitrogen, and kept warm for 5 hours. It was then heated to 500°C at a heating rate of 2°C / min and calcined, and kept warm for 10 hours to obtain a Na4[Fe0Fe3](PO4)2(P2O7)@C composite positive electrode material.

[0071] Test Example 1

[0072] The samples prepared in Examples 1-5 and Comparative Examples 1-2 were tested for button batteries, and the results are shown in Table 1 below.

[0073] The testing method of the button cell is as follows: assembling a slurry with a mass ratio of active material: Super p: PVDF of 8:1:1 into a button cell and testing it under the condition of a cut-off voltage of 2.0V-4.0gV.

[0074] Table 1 Material test results of Examples 1-5 and Comparative Examples 1-2

[0075]

[0076] Examples 1-5 and Comparative Examples 1-2 show that the discharge capacity of the mixed iron source at 0.1C is better than the electrochemical performance of the single iron source sample. When the ratio of iron phosphate to iron oxide is 4:6, the electrochemical performance is the best. When it is lower than this ratio, the optimal electrochemical performance is not fully realized; when it is higher than this ratio, the electrochemical performance gradually decreases.

Claims

1. A method for preparing a positive electrode material for a sodium ion battery, characterized in that: The general formula of the sodium ion battery positive electrode material is Na4[Fe x Fe 3-x ](PO4)2(P2O7)@C, the positive electrode material of the sodium ion battery is Na4[Fe x Fe 3-x ](PO4)2(P2O7) and C complex, Where x=1.2, Fe x The iron source used is the first iron source, Fe 3-x The iron source used is a second iron source, the first iron source is iron phosphate, and the second iron source is iron oxide; The preparation method comprises the following steps: (1) adding a sodium source, a phosphorus source, and a carbon source into water, mixing them evenly to form a solution, then adding a first iron source and a second iron source, mixing them evenly to form a slurry, and drying to obtain a precursor powder; (2) calcining the precursor powder obtained in step (1) under an inert atmosphere to obtain a positive electrode material for a sodium ion battery; the calcination conditions are: calcining at a temperature of 500-550° C. for 10-13 h; Na4[Fe x Fe 3-x ]The mass ratio of (PO4)2(P2O7) and C is 98:2~97:3; In step (1), grinding is performed using a sand mill before drying; the speed of the sand mill is 2000 r / min, the flow rate is 200 L / h, and the grinding time is 40-100 min; The solid content of the slurry after grinding is 45%-50%, and the sand grinding particle size is 200-300nm; In step (1), the drying method is spray drying, the feed rate of spray drying is 60-90 mL / min, the frequency of the atomizing disk is 450 Hz, the feed temperature is 220° C., and the discharge temperature is 90-100° C.

2. The method for preparing a positive electrode material for a sodium ion battery according to claim 1, characterized in that: In step (1), The sodium source is at least one of sodium carbonate, sodium chloride, disodium hydrogen phosphate, sodium dihydrogen phosphate, sodium nitrate, sodium oxalate, sodium pyrophosphate, tripolyphosphoric acid, and sodium ethoxide; The carbon source is at least one of sucrose, glucose, citric acid, polyethylene glycol, oxalic acid, sodium carbonate and ascorbic acid.

3. A sodium ion battery positive electrode material prepared by the preparation method according to claim 1 or 2.

4. Use of the sodium ion battery positive electrode material according to claim 3 in the preparation of sodium ion batteries.

5. A sodium ion battery, characterized in that: Including the sodium ion battery positive electrode material as described in claim 3.