A green and environmentally friendly alkali-free and chlorine-free liquid accelerating agent and preparation method thereof
The alkali-free and chlorine-free liquid accelerator is prepared by combining aluminum sulfate and alkaline aluminum sol with stabilizers, which solves the problems of poor stability and fluorosis of alkali-free liquid accelerators, and achieves high stability and rapid condensation effects. Suitable for wet sprayed concrete construction, reducing environmental and human hazards.
Patent Information
- Application Number
- CN202310769761.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-28
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-06-28
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to a liquid accelerating setting agent, in particular to a green and environmentally friendly alkali-free and chlorine-free liquid accelerating setting agent and a preparation method thereof, belonging to the fields of chemical materials and concrete technology. Technical Background
[0002] By the end of 2017, my country's railway operating mileage has reached 127,000 kilometers, of which 25,000 kilometers of high-speed railways are open to traffic, ranking first in the world; the total mileage of highways is 4.77 million kilometers, of which 136,000 kilometers of expressways are open to traffic, ranking first in the world. Although my country is now a major transportation country, it still has a long way to go to become a strong transportation country. Under the premise of building a strong transportation country in my country, the use of accelerators as essential chemical admixtures in the construction of tunnels, subways and ground rapid projects will show an increasing trend year by year. At present, the accelerators used in my country are mainly alkaline liquid accelerators, which reduce the occurrence of dust occupational diseases after using powder accelerators; however, alkaline liquid accelerators have great harm to the strength of concrete, and will also affect the surrounding environment of construction and corrode the human body. Therefore, the research on alkali-free liquid accelerators is a hot spot in the current research on accelerators.
[0003] At present, the raw materials of commercially available alkali-free liquid accelerators are generally aluminum compounds. Aluminum ions are very likely to undergo hydrolysis-polymerization-precipitation reactions in water, and the solubility of aluminum salts is relatively low. As time goes by, alkali-free liquid accelerators are prone to unstable phenomena such as flocculation precipitation and crystallization, which leads to generally poor stability of alkali-free liquid accelerators. The shelf life is usually one week, and some are even only 3 days. How to inhibit the crystallization and hydrolysis of highly saturated aluminum solutions is the key to solving the stability of alkali-free liquid accelerators. Secondly, although alkali-free liquid accelerators can make concrete slurry coagulate quickly, the early strength of concrete is low or even no strength, and the production equipment requirements are high, the environmental process is complex, and a large amount of harmful substances are used at the same time, causing varying degrees of damage to the ecological environment, construction environment, workers' respiratory system, eyes, skin, etc. Therefore, finding an alkali-free liquid accelerator with a simple preparation method, good stability and high concrete strength is the key to realizing the application of alkali-free liquid accelerators. CN202210698180.X discloses an environmentally friendly, non-toxic, alkali-free liquid concrete accelerator, which is mainly composed of activated polyacrylamide and polyaluminum sulfate, and dissolves aluminum hydroxide with hydrofluoric acid to increase the aluminum ion concentration in the accelerator, so that the concrete can quickly gel and harden, effectively reducing the setting time, and improving the mortar strength and the stability of the accelerator. CN202010626842.3 discloses a fast-setting, high-strength alkali-free liquid accelerator, which is composed of aluminum sulfate, hydrofluoric acid, aluminum hydroxide, a pre-dispersed reinforcing component, a suspended component, a complexing component, an organic acid, and water. It has good adaptability to cement-based materials and good stability. The concrete using the accelerator has a fast setting speed, high early strength, low rebound rate, small dust volume, and good bonding effect. CN202010037086.0 provides a magnesium aluminum fluoride system alkali-free quick-setting agent without hazardous chemicals. The alkali-free quick-setting agent does not contain hydrofluoric acid and fluosilicic acid, so no harmful gases will be generated during the construction process, avoiding the impact of harmful gases on the health of construction workers and avoiding the pollution of harmful gases to the air; secondly, the alkali-free quick-setting agent prepared by the present invention has excellent stability and quick-setting effect, can effectively shorten the time of initial setting and final setting of concrete, and improve the early strength and late strength of concrete. However, the commonly used fluoride-containing substances in these alkali-free liquid quick-setting agents are hydrofluoric acid, fluosilicic acid, etc., and their addition amount is even as high as 25-30%; in addition, magnesium fluosilicate, aluminum fluoride and other substances are also added; and these fluorine-containing substances are very likely to cause fluoride poisoning, and also have a great impact on the environment. Therefore, the development of a green and environmentally friendly alkali-free and chlorine-free liquid quick-setting agent with short setting time, high compressive strength, low alkali content, and no chloride ions and fluoride ions is the key and difficulty to improve the construction quality of wet spraying concrete and reduce environmental pollution. Summary of the invention
[0004] The purpose of the present invention is to provide a green and environmentally friendly alkali-free and chlorine-free liquid setting accelerator and a preparation method thereof, in view of the fact that the alkali-free liquid setting accelerator commonly used in China currently uses fluoride, which is very likely to cause fluoride poisoning and has a great impact on the environment.
[0005] 1. Components and preparation of alkali-free and chlorine-free liquid accelerator
[0006] The green and environmentally friendly alkali-free and chlorine-free liquid accelerating setting agent of the present invention is prepared by the following raw materials and processes:
[0007] Raw materials: by weight percentage, aluminum sulfate 40.0-50.0%, alkaline aluminum sol 5.0-10.0%, enhancer 0.5-1.0%, stabilizer 1.0-3.0%, pH adjuster 0.5-2.0%, balance water;
[0008] Preparation process: first add aluminum sulfate to water, heat to 60~80 ℃, stir to completely dissolve it, recorded as solution A; then add alkaline aluminum sol to solution A and stir evenly to obtain solution B; then add enhancer and stabilizer to solution B in sequence, stir evenly, continue stirring and reacting for 1.0~3.0 h to obtain solution C; after solution C is allowed to cool to room temperature, add pH regulator and control the solution pH = 2.5~4.9, continue stirring for 2.5~4.5 h, and obtain a green and environmentally friendly alkali-free and chlorine-free liquid accelerator.
[0009] The reinforcing agent is one or more of water glass, magnesium sulfate, calcium formate, ferrous sulfate and ferrous sulfate.
[0010] The stabilizer is one or more of polyacrylamide, isopropanolamine, polypropylene glycol, polyethylene glycol, and glycerol.
[0011] The pH adjuster is one or more of monoethanolamine, triethanolamine, ammonia water and ammonium carbonate.
[0012] The green, environmentally friendly, alkali-free, chlorine-free liquid accelerator of the present invention uses aluminum sulfate and alkaline aluminum sol as the main accelerating components. Since the two have different pH values (aluminum sulfate is acidic and alkaline aluminum sol is alkaline), the dissolution rate of the two is accelerated after mixing, and the solubility of the two in the accelerator is also improved; under the action of the stabilizer, the flocculation and precipitation of aluminum ions are blocked, and the stability of the accelerator is improved. In addition, aluminum sulfate and alkaline aluminum sol are used as the main accelerating components, which are evenly dispersed in the accelerator system. The aluminum ion content in the accelerator is increased through the interaction between the two. After being added to concrete, the aluminum ions in the accelerator are hydrolyzed to generate [Al(OH)4] - , which can react with Ca generated by cement clinker mineral hydrolysis 2+It reacts quickly, generating a large amount of ettringite and colloidal calcium silicate hydrate in a short time, accelerating the hydration of cement. Under the action of stabilizer, the accelerator can be fully dispersed in the concrete system, so that the generated crystals intertwine and quickly form a network structure, which makes the cement set quickly, and has excellent setting time and strength.
[0013] 2. Performance test of alkali-free and chlorine-free liquid accelerator
[0014] The green and environmentally friendly alkali-free and chlorine-free liquid accelerator prepared by the present invention is tested for alkali content, initial setting time, final setting time, compressive strength and stability according to the standard "GB / T 35159-2017 Accelerator for Shotcrete".
[0015] 1. Alkali content, chlorine content and fluorine content
[0016] The test results show that the chlorine and fluorine contents of the green, environmentally friendly, alkali-free and chlorine-free liquid accelerator prepared by the present invention are both less than 0.1%, and the alkali content is in the range of 0.35-0.71%, which is much lower than the "GB / T 35159-2017 Accelerator for Shotcrete" standard.
[0017] 2. Setting time
[0018] Materials used for the test: 400 g cement, 140 g water (including water in the liquid accelerator), the dosage of the green and environmentally friendly alkali-free and chlorine-free liquid accelerator is 8% of the cement.
[0019] Test results: initial setting time ≤3 min, final setting time ≤8 min, which are far lower than the "GB / T 35159-2017 Accelerator for Shotcrete" standard.
[0020] 3. Compressive strength
[0021] Materials used in the experiment: 900 g cement, 450 g water (including water in the liquid accelerator), 1350 g standard sand, and the amount of green and environmentally friendly alkali-free and chlorine-free liquid accelerator added is 8% of the cement.
[0022] Test results: Mortar strength: 1-day strength is above 7.2MPa; 28-day compressive strength ratio is greater than 100%, which fully meets the "GB / T 35159-2017 Accelerator for Shotcrete" standard.
[0023] 4. Stability
[0024] Test results: The green and environmentally friendly alkali-free and chlorine-free liquid accelerator of the present invention can be stably stored for more than 3 months, and some can even be stably stored for more than 6 months, which is conducive to the use and transportation of the green and environmentally friendly alkali-free and chlorine-free liquid accelerator.
[0025] In summary, the alkali-free and chlorine-free liquid accelerator prepared by the present invention has good stability, short setting time, and high early strength and mid-to-late strength of concrete. In wet spraying concrete construction, when the doping amount of the alkali-free and chlorine-free liquid accelerator is 8%, the initial setting time, final setting time, compressive strength and other indicators of the test piece all meet the "GB / T 35159-2017 Accelerator for Shotcrete" standard, and the initial setting time and final setting time of the concrete are much lower than those of the commercially available alkali-free liquid accelerator, and are suitable for occasions where rapid setting of concrete is required; the accelerator has a low alkali content, does not contain chloride ions and fluoride ions, has less harm to the human body and the environment, and is green and environmentally friendly. DETAILED DESCRIPTION
[0026] The formulation, preparation and application performance of the green, environment-friendly, alkali-free and chlorine-free liquid quick-setting agent of the present invention are further described below through specific examples.
[0027] Example 1
[0028] Weigh 500 kg of aluminum sulfate and add it to 500 kg of water, heat it to 80 °C, stir it to dissolve it completely, and obtain solution A; take 100 kg of alkaline aluminum sol and add it to solution A, stir it evenly to obtain solution B; take 5 kg of water glass and 15 kg of polypropylene glycol and add them to solution B and stir it evenly, and continue to stir and react for 2.0 h to obtain solution C; after solution C is placed at room temperature, add 20 kg of ammonia water and stir it evenly (the pH value of solution C is in the range of 2.5~4.9); continue to stir for 2.5 h to obtain a green and environmentally friendly alkali-free and chlorine-free liquid accelerator. The performance of the alkali-free and chlorine-free liquid accelerator was determined according to the above method, and the test results are shown in Table 1.
[0029] Example 2
[0030] Weigh 400 kg of aluminum sulfate and add it to 600 kg of water, heat it to 60 °C, stir it to dissolve it completely, and obtain solution A; take 90 kg of alkaline aluminum sol and add it to solution A, stir it evenly to obtain solution B; take 10 kg of magnesium sulfate and 30 kg of isopropanolamine and add them to solution B and stir it evenly, and continue to stir and react for 3.0 h to obtain solution C; after solution C is placed at room temperature, 15 kg of ammonium carbonate is added thereto (the pH value of solution C is in the range of 2.5~4.9), and continue to stir for 2.5 h to obtain a green and environmentally friendly alkali-free and chlorine-free liquid accelerator. The performance of the alkali-free and chlorine-free liquid accelerator was determined according to the above method, and the test results are shown in Table 1.
[0031] Example 3
[0032] Weigh 450 kg of aluminum sulfate and add it to 550 kg of water, heat it to 70 °C, stir it to dissolve it completely, and obtain solution A; take 85 kg of alkaline aluminum sol and add it to solution A, stir it evenly to obtain solution B; take 8 kg of calcium formate and 10 kg of polyacrylamide and add them to solution B and stir it evenly, and continue to stir and react for 1.5 hours to obtain solution C; after solution C is placed at room temperature, add 10 kg of ammonium bicarbonate (the pH value of solution C is in the range of 2.5~4.9), continue to stir for 3.0 hours, and obtain a green and environmentally friendly alkali-free and chlorine-free liquid accelerator. The performance of the alkali-free and chlorine-free liquid accelerator was determined according to the above method, and the test results are shown in Table 1.
[0033] Example 4
[0034] Weigh 600 kg of aluminum sulfate and add it to 500 kg of water, heat it to 75 °C, stir it to dissolve it completely, and obtain solution A; take 100 kg of alkaline aluminum sol and add it to solution A and stir it evenly to obtain solution B; take 10 kg of ferrous sulfate and 15 kg of polyethylene glycol and add them to solution B and stir it evenly, and continue to stir and react for 3.0 h to obtain solution C; after solution C is placed at room temperature, add 20 kg of triethanolamine (the pH value of solution C is in the range of 2.5~4.9), continue to stir for 3.0 h, and obtain a green and environmentally friendly alkali-free and chlorine-free liquid accelerator. The performance of the alkali-free and chlorine-free liquid accelerator was determined according to the above method, and the test results are shown in Table 1.
[0035] Example 5
[0036] Weigh 500 kg of aluminum sulfate and add it to 450 kg of water, heat it to 80 ° C, stir it to dissolve it completely, and obtain solution A; take 85 kg of alkaline aluminum sol and add it to solution A, stir it evenly to obtain solution B; take 12 kg of ferrous sulfate and 15 kg of glycerol and add them to solution B and stir it evenly, and continue to stir and react for 1.0 h to obtain solution C; after solution C is placed at room temperature, add 15 kg of monoethanolamine (the pH value of solution C is in the range of 2.5~4.9), continue to stir for 4.5 h, and obtain a green and environmentally friendly alkali-free and chlorine-free liquid accelerator. The performance of the alkali-free and chlorine-free liquid accelerator was determined according to the above method, and the test results are shown in Table 1.
[0037] Example 6
[0038] Weigh 500 kg of aluminum sulfate and add it to 600 kg of water, heat it to 75 °C, stir it to dissolve it completely, and obtain solution A; take 95 kg of alkaline aluminum sol and add it to solution A, stir it evenly to obtain solution B; take 9 kg of calcium formate, 10 kg of polypropylene glycol and 5 kg of polyethylene glycol and add them to solution B and stir evenly, continue to stir and react for 2.0 h to obtain solution C; after solution C is placed at room temperature, add 15 kg of ammonia water (the pH value of solution C is in the range of 2.5~4.9), continue to stir for 4.5 h, and obtain a green and environmentally friendly alkali-free and chlorine-free liquid accelerator. The performance of the alkali-free and chlorine-free liquid accelerator was determined according to the above method, and the test results are shown in Table 1.
[0039] Example 7
[0040] Weigh 550 kg of aluminum sulfate and add it to 500 kg of water, heat it to 75 ° C, stir it to dissolve it completely, and obtain solution A; take 70 kg of alkaline aluminum sol and add it to solution A, stir it evenly to obtain solution B; take 5 kg of water glass, 5 kg of magnesium sulfate and 15 kg of glycerol and add them to solution B and stir evenly, and continue to stir and react for 1.0 h to obtain solution C; after solution C is placed at room temperature, add 20 kg of ammonium carbonate (the pH value of solution C is in the range of 2.5~4.9), continue to stir for 3.0 h, and obtain a green and environmentally friendly alkali-free and chlorine-free liquid accelerator. The performance of the alkali-free and chlorine-free liquid accelerator was determined according to the above method, and the test results are shown in Table 1.
[0041] Example 8
[0042] Weigh 450 kg of aluminum sulfate and add it to 550 kg of water, heat it to 70 ° C, stir it to dissolve it completely, and obtain solution A; take 60 kg of alkaline aluminum sol and add it to solution A, stir it evenly to obtain solution B; take 10 kg of ferrous sulfate and 15 kg of polypropylene glycol and add them to solution B. After stirring evenly, continue to stir and react for 2.5 hours to obtain solution C; after solution C is placed at room temperature, add 10 kg of sodium bicarbonate and 10 kg of triethanolamine (the pH value of solution C is in the range of 2.5~4.9), continue to stir for 4.5 hours, and obtain a green and environmentally friendly alkali-free and chlorine-free liquid accelerator. The performance of the alkali-free and chlorine-free liquid accelerator was determined according to the above method, and the test results are shown in Table 1.
[0043] Example 9
[0044] Weigh 550 kg of aluminum sulfate and add it to 450 kg of water, heat it to 80 ° C, stir it to dissolve it completely, and obtain solution A; take 80 kg of alkaline aluminum sol and add it to solution A, stir it evenly to obtain solution B; take 7 kg of ferrous sulfate, 3 kg of calcium formate, 10 kg of polyethylene glycol and 5 kg of glycerol and add them to solution B and stir evenly, and continue to stir and react for 2.0 h to obtain solution C; after solution C is placed at room temperature, 15 kg of ammonia water and 5 kg of ammonium carbonate (the pH value of solution C is in the range of 2.5~4.9) are added thereto, and stirring is continued for 4.5 h to obtain a green and environmentally friendly alkali-free and chlorine-free liquid accelerator. The performance of the alkali-free and chlorine-free liquid accelerator was determined according to the above method, and the test results are shown in Table 1.
[0045]
[0046] According to the test results in Table 1, the alkali content of the green, environmentally friendly, alkali-free, chlorine-free liquid accelerator of the present invention meets the national standard of "GB / T 35159-2017 Accelerator for Shotcrete". After the green, environmentally friendly, alkali-free, chlorine-free liquid accelerator of the present invention is added, the initial setting time, final setting time and compressive strength of the concrete all meet the national standards, and the initial setting time and final setting time of the concrete are much lower than those of the commercially available alkali-free liquid accelerator, which is suitable for occasions requiring rapid coagulation; at the same time, since the accelerator contains a large amount of stable aluminum ions, it can accelerate cement hydration, generate a large amount of calcium aluminate and colloidal hydrated calcium silicate in a short time, so that the concrete has excellent 1-day strength and 28-day compressive strength ratio (greater than 100%); the green, environmentally friendly, alkali-free, chlorine-free liquid accelerator of the present invention can be stably stored for more than 3 months, which is conducive to the use and transportation of the green, environmentally friendly, alkali-free, chlorine-free liquid accelerator.
Claims
1. A green and environmentally friendly alkali-free and chlorine-free liquid accelerating setting agent is prepared by the following raw materials and processes: Raw materials: in weight percentage, aluminum sulfate 40.0-50.0%, alkaline aluminum sol 5.0-10.0%, enhancer 0.5-1.0%, stabilizer 1.0-3.0%, pH value adjuster 0.5-2.0%, water balance; the enhancer is one or more of water glass, magnesium sulfate, calcium formate, ferrous sulfate, ferrous sulfate; the stabilizer is one or more of polyacrylamide, isopropanolamine, polypropylene glycol, polyethylene glycol, glycerol; Preparation process: first add aluminum sulfate to water, heat to 60~80 ℃, stir to completely dissolve it, recorded as solution A; then add alkaline aluminum sol to solution A and stir evenly to obtain solution B; then add enhancer and stabilizer to solution B in sequence, stir evenly, and continue stirring for 1.0~3.0 h to obtain solution C; after solution C is allowed to cool to room temperature, add pH regulator and control the solution pH = 2.5~4.9, continue stirring for 2.5~4.5 h, and obtain a green and environmentally friendly alkali-free and chlorine-free liquid accelerator.