A water-based primer-surface all-in-one coating and its preparation method and application

Through the design of water-based bottom-in-one coating, using specific components and stirring steps, the problems of paint film sagging and blistering in existing water-based coatings are solved, and a high-efficiency and low-energy consumption coating solution is achieved, satisfying the High adhesion and durability requirements of construction machinery body.

CN116676033BActive Publication Date: 2024-11-12ZHUZHOU JIUHUA NEW MATERIAL COATING IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310881969.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-18
Publication Date
2024-11-12
Estimated Expiration
2043-07-18

AI Technical Summary

Technical Problem

During the construction process, existing water-based coatings have problems such as sagging, blistering, and pinholes, and require two coatings and baking and drying at high temperatures, resulting in a long coating cycle, high energy consumption and high cost.

Method used

A water-based bottom surface-integrated coating is adopted, including component A and component B. Component A is composed of a first aqueous acrylic dispersion, a second aqueous acrylic dispersion, a lithium magnesium silicate pre-coagulation slurry, a surfactant, etc. Component B consists of a curing agent and glycol butyl ether acetate, and is prepared by specific stirring and grinding steps to form a paint film with high adhesion, salt spray resistance and aging resistance.

Benefits of technology

A coating can achieve the function of primer and topcoat, reducing the coating process and energy consumption, improving construction efficiency, reducing costs, and high paint film thickness, short leveling time, no bubbles and flow The problem is that VOC emissions are low.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004345035090000101
    Figure BDA0004345035090000101
  • Figure BDA0004345035090000111
    Figure BDA0004345035090000111
  • Figure BDA0004345035090000121
    Figure BDA0004345035090000121
Patent Text Reader

Abstract

The present invention discloses a water-based bottom-surface all-in-one coating and a preparation method and application thereof, and relates to the technical field of coatings; the water-based bottom-surface all-in-one coating adopts a water-based acrylic dispersion, a color filler, an anti-rust pigment, an additive, a cosolvent and water to form a paint part. The water-based bottom-surface all-in-one coating of the present invention is suitable for the construction of workpieces such as the outer surface of the engineering machinery body, and the substrates include carbon steel, aluminum alloy, etc. The water-based bottom-surface all-in-one coating has good adhesion on the surface of each substrate, high paint film hardness, good thick coating, long service life, good salt spray resistance, aging resistance and water resistance, low VOC emission, and since only one coating layer needs to be sprayed, the coating process and energy consumption are reduced, the work efficiency is improved, and the coating cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of coatings, and in particular is a water-based primer-and-surface all-in-one coating and a preparation method and application thereof. Background Art

[0002] During the construction process of water-based paint, no organic solvents are added, and water is used as a diluent, which greatly reduces the VOC emissions of the coating construction and also improves the working environment of the coating workers. In the related technology, the coating in the field of engineering machinery has also begun to be water-based, especially in the coating construction of some urban engineering vehicles, etc., which requires the paint film to have good adhesion to various substrates, and the product is more green and environmentally friendly, with low VOC emissions, and the paint film has good water resistance, aging resistance, salt spray resistance and high paint film hardness. At the same time, it is necessary to reduce the coating process and energy consumption during the coating process, and high construction efficiency is required. The bottom-to-top integrated paint sprays a layer of coating, and the paint film thickness is more than 60μm. At the same time, the appearance is smooth, without heavy orange peels, bubbling, sagging and other paint film defects.

[0003] The construction thickness of water-based paint in related technologies is generally 30μm to 50μm for one spray dry film. If it is sprayed too thickly at one time, paint film problems such as sagging, bubbling, and pinholes are prone to occur. Generally, water-based paint for construction machinery requires two coats of primer and topcoat, and high-temperature baking and air-drying for leveling. The coating cycle is long, the energy consumption is high, and the coating cost is high. Summary of the invention

[0004] The object of the present invention is to provide a water-based primer and surface all-in-one coating to solve at least one aspect of the problems and defects raised in the above-mentioned background technology.

[0005] The invention also provides a method for preparing the coating.

[0006] The invention also provides application of the coating.

[0007] Specifically, the first aspect of the present invention provides a water-based primer-and-surface all-in-one coating, comprising component A and component B;

[0008] The A component includes the following raw materials in parts by weight:

[0009] 35 to 45 parts of the first aqueous acrylic dispersion, 12 to 15 parts of the second aqueous acrylic dispersion, 2 to 3 parts of lithium magnesium silicate pre-slurry, 2.0 to 2.5 parts of dispersant, 0.8 to 1.0 parts of surfactant, 0.2 to 0.3 parts of defoaming agent, 0.3 to 0.5 parts of wetting agent, 0.3 to 0.5 parts of leveling agent, 15 to 20 parts of color filler, 6 to 10 parts of rust-proof pigment, 0.5 to 0.8 parts of anti-sagging agent, 3 to 5 parts of cosolvent, 0.5 to 1.0 parts of anti-flash rust agent, 0.8 to 1.0 parts of ultraviolet light absorber, 0.4 to 0.6 parts of light stabilizer, 0.2 to 0.3 parts of DMEA and 8 to 12 parts of water.

[0010] According to one technical solution of the coating technical solution of the present invention, at least the following beneficial effects are achieved:

[0011] The water-based primer-and-topcoat of the present invention has the functions of a primer and a topcoat on the outer surface of the engineering machinery body through one coating. The substrates include carbon steel, aluminum alloy, etc. The water-based primer-and-topcoat has good adhesion on the surface of each substrate, high paint film hardness, good thick coating, long service life, good salt spray resistance, aging resistance, moisture and heat resistance and water resistance, and low VOC emissions. Since only one coating layer needs to be sprayed, the coating process and energy consumption are reduced, the work efficiency is improved, and the coating cost is reduced.

[0012] According to some embodiments of the present invention, the solid content of the first aqueous acrylic dispersion is 44% to 46%.

[0013] According to some embodiments of the present invention, the viscosity of the first aqueous acrylic dispersion is 500 mPa·s to 4500 mPa·s (25° C.).

[0014] According to some embodiments of the present invention, the hydroxyl content of the first aqueous acrylic dispersion is 3.0% to 3.3%.

[0015] According to some embodiments of the present invention, the first aqueous acrylic dispersion is AQUAPAC-8533 aqueous acrylic dispersion of Jiangsu Fuqisen New Materials Co., Ltd.

[0016] According to some embodiments of the present invention, the second aqueous acrylic dispersion is 3AH56W aqueous acrylic dispersion of Guangdong Tongde New Materials Co., Ltd.

[0017] According to some embodiments of the present invention, the viscosity of the second aqueous acrylic dispersion is 50 mPa·s to 2000 mPa·s (25° C.) According to some embodiments of the present invention, the solid content of the second aqueous acrylic dispersion is 40% to 44%.

[0018] According to some embodiments of the present invention, the hydroxyl value of the second aqueous acrylic dispersion is 50 mgKOH / g to 60 mgKOH / g.

[0019] According to some embodiments of the present invention, the wetting agent is a silicone twin structure wetting agent.

[0020] According to some embodiments of the present invention, the flash rust inhibitor comprises an organic carboxylate-based flash rust inhibitor.

[0021] According to some embodiments of the present invention, the dispersant is an anionic polymer dispersant.

[0022] According to some embodiments of the present invention, the anti-sagging aid is a modified polyurea solution anti-sagging aid.

[0023] According to some embodiments of the invention, the surfactant is a nonionic surfactant.

[0024] According to some embodiments of the invention, the nonionic surfactant is an acetylenic diol nonionic surfactant.

[0025] According to some embodiments of the present invention, the lithium magnesium silicate pre-slurry consists of lithium magnesium silicate and water.

[0026] According to some embodiments of the present invention, the mass ratio of lithium magnesium silicate to water in the lithium magnesium silicate pre-slurry is 1:10-15.

[0027] According to some embodiments of the present invention, the lithium magnesium silicate is obtained from Leifus (Shanghai) Chemical Co., Ltd. W2N.

[0028] According to some embodiments of the present invention, the anti-sagging agent is ANJEKA-4420 from Ezhou Anjikang Technology Co., Ltd.

[0029] According to some embodiments of the present invention, the dispersant is an anionic polymer dispersant.

[0030] According to some embodiments of the present invention, the anionic polymer dispersant is TEGO750 from TEGO Company of Germany.

[0031] According to some embodiments of the present invention, the nonionic surfactant is A04E produced by Yueyang Kaimen Water-based Additive Co., Ltd.

[0032] According to some embodiments of the present invention, the defoaming agent is a polysiloxane defoaming agent.

[0033] According to some embodiments of the present invention, the polysiloxane defoamer is BYK024 from BYK Company of Germany.

[0034] According to some embodiments of the present invention, the organosilicon twin structure wetting agent is TEGO4100Twins from TEGO Company of Germany.

[0035] According to some embodiments of the present invention, the leveling agent is an acrylic leveling agent.

[0036] According to some embodiments of the present invention, the acrylic leveling agent is BYK348 produced by German BYK Company.

[0037] According to some embodiments of the present invention, the ultraviolet light absorber is the ultraviolet light absorber Tinuvin 1130 produced by BASF of Germany.

[0038] According to some embodiments of the present invention, the light stabilizer is the light stabilizer Tinuvin 292 produced by BASF of Germany.

[0039] According to some embodiments of the present invention, the anti-flash rust agent is Tech-8876 from Tiger Polymer Technology Co., Ltd.

[0040] According to some embodiments of the present invention, the co-solvent is dipropylene glycol butyl ether.

[0041] According to some embodiments of the present invention, the pigment and filler is titanium dioxide.

[0042] According to some embodiments of the present invention, the titanium dioxide is titanium dioxide 895 produced by Longbai Group Corporation.

[0043] According to some embodiments of the present invention, the anti-rust pigment is a zinc aluminum phosphate anti-rust pigment.

[0044] According to some embodiments of the present invention, the B component includes a curing agent and ethylene glycol butyl ether acetate.

[0045] According to some embodiments of the present invention, the curing agent includes at least one of an HDI trimer curing agent and an IPDI curing agent.

[0046] According to some embodiments of the present invention, the HDI trimer curing agent is HT-100 produced by Wanhua Chemical Group Co., Ltd.

[0047] According to some embodiments of the present invention, the IPDI curing agent is Vestanat T1890E from Evonik of Germany.

[0048] According to some embodiments of the present invention, the B component includes the following preparation raw materials in parts by weight:

[0049] Isocyanate HDI curing agent: 50 parts to 60 parts, IPDI curing agent: 15 parts to 20 parts, ethylene glycol butyl ether acetate: 30 parts to 35 parts.

[0050] According to some embodiments of the present invention, the mass ratio of the component A to the component B is 5:1-2.

[0051] The second aspect of the present invention provides a method for preparing the above-mentioned water-based primer and surface all-in-one coating, comprising the following steps: mixing component A and component B.

[0052] According to some embodiments of the present invention, the method for preparing component A comprises the following steps:

[0053] S1. Mixing lithium magnesium silicate and part of water, stirring for 10 min to 15 min at a rotation speed of 800 r / min to 1000 r / min, to obtain lithium magnesium silicate pre-slurry;

[0054] S2, after mixing part of water, dispersant, pre-coagulation slurry, surfactant, defoamer, pigment and anti-rust pigment, stir at a speed of 1000r / min to 1200r / min for 20min to 30min to obtain pre-dispersed slurry;

[0055] S3, grinding the pre-dispersed slurry to a fineness of ≤15 μm, adding the first aqueous acrylic dispersion, the second aqueous acrylic dispersion, the wetting agent and the leveling agent to the ground pre-dispersed slurry, and then controlling the rotation speed to 1000 r / min to 1200 r / min, stirring for 10 min to 15 min to obtain a first dispersed slurry;

[0056] S4. Mix the anti-flash rust agent, anti-sagging agent, cosolvent, ultraviolet light absorber, light stabilizer, DMEA, water and the first dispersion slurry, and stir for 10 to 15 minutes.

[0057] According to some embodiments of the present invention, the method for preparing component B comprises the following steps: after mixing the curing agent and ethylene glycol butyl ether acetate, stirring at a rotation speed of 1000 r / min to 1200 r / min for 5 min to 10 min.

[0058] The third aspect of the present invention provides the use of the above-mentioned water-based primer and surface all-in-one coating in the preparation of engineering vehicles.

[0059] The paint film leveling time of the water-based primer and topcoat of the present invention is 0.5h, and the baking time is 2h, and the comprehensive performance is excellent, the performance can meet the customer's standard requirements, and the coating time is shortened by at least 2.5h (in the related art, water-based primer is applied, the paint film is leveled for 0.5h, baked for 2h, left to air at room temperature, and then water-based topcoat is applied, the paint film is leveled for 0.5h, and baked for 2h).

[0060] According to some embodiments of the present invention, the coating substrate of the coating is a metal substrate.

[0061] According to some embodiments of the present invention, the metal substrate is at least one of carbon steel and aluminum alloy. DETAILED DESCRIPTION

[0062] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.

[0063] In the description of the present invention, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.

[0064] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. If the manufacturers of the reagents or instruments are not specified, they are all conventional products that can be purchased commercially.

[0065] The raw materials and manufacturers of the present invention are as follows:

[0066] Aqueous acrylic dispersion I is AQUAPAC-8533 aqueous acrylic dispersion; Jiangsu Fuqisen New Materials Co., Ltd.; solid content is 44% to 46%; viscosity (mPa·s, 25°C): 500mPa·s to 4500mPa·s; hydroxyl content is: 3.3%.

[0067] The functional group hydroxyl (-OH) in the waterborne acrylic dispersion I reacts with the isocyanate (-N=C=O) in the HDI trimer and IPDI to crosslink and cure into a film, and has excellent chemical resistance and weather resistance.

[0068] Aqueous acrylic dispersion II is 3AH56W aqueous acrylic dispersion, produced by Guangdong Tongde New Materials Co., Ltd.; solid content is 40% to 44%; viscosity (mPa·s, 25°C): 50mPa·s to 2000mPa·s; hydroxyl value is: 60mgKOH / g.

[0069] Water-based acrylic dispersion II, the hydroxyl content of the resin is low, and the CO generated by the cross-linking reaction 2 It can be released without generating bubbles. At the same time, the glass transition temperature of the resin is high, the paint film is not easy to sag, and it is suitable for thick coating.

[0070] Lithium magnesium silicate W2N, produced by Leivos (Shanghai) Chemical Co., Ltd.

[0071] Lithium magnesium silicate (rheological additive) is similar in structure to natural hentolin and has unique rheological properties. The primary particles carry negative charge on the front and positive charge on the side. When added to water, the dispersed primary particles move close to each other. Due to the charge repulsion, a "house of cards" structure is formed in water-based paint. The pigment particles are suspended in a three-dimensional structure gel, and their mobility is significantly reduced, showing a more excellent anti-settling effect.

[0072] The anti-sagging additive is ANJEKA-4420, produced by Ezhou Anjikang Technology Co., Ltd.

[0073] Anti-sagging additive is a modified polyurea solution. The urea group has a large polarity and can form more hydrogen bonds, producing a three-dimensional network structure in the coating system to prevent the coating from settling and sagging. Under high shear, the thixotropic properties disappear, and the three-dimensional network structure is restored after the shear stops. It does not affect the construction spraying, but has good anti-sagging and anti-settling functions.

[0074] The dispersant is an anionic polymer dispersant; TEGO750, produced by TEGO Company of Germany.

[0075] The anionic polymer dispersant used in the present invention has a large steric effect. The charged groups produce an anchoring effect with the pigment ions, making the pigment ions more stable and not flocculating when colliding with each other. At the same time, the polymer dispersers are all macromolecules, and the macromolecular chain segments are well dissolved and unfolded, which has the effect of reducing the viscosity of the system. A small amount of water can be added to achieve the construction state, so that the coating can have a thicker film thickness after spraying.

[0076] The non-ionic surfactant is A04E, produced by Yueyang Kaimen Water-based Additive Co., Ltd.

[0077] The nonionic surfactant used in the present invention is an acetylene glycol nonionic surfactant.

[0078] Due to the special acetylenediol structure, the product has multiple functions such as wetting, defoaming, improving dispersibility, improving flow and leveling, etc. It can effectively reduce surface tension, control foam, stabilize consistency and viscosity. Compared with traditional surfactants, it has lower water sensitivity and is suitable for water-based systems. It has lower dynamic / static surface tension, can quickly reduce the dynamic / static surface tension of the system and quickly migrate to the surface to ensure good wetting of the substrate. At the same time, the dynamic surface tension of the surfactant does not change much from that in static state. This feature allows the system to still wet the substrate well during intense movement, such as spraying, rolling, brushing and other rapid interface formation processes. It can avoid some paint film defects caused by thick coating.

[0079] The defoamer is polysiloxane defoamer, BYK024, produced by BYK Company of Germany.

[0080] The wetting agent is a silicone twin structure wetting agent, TEGO4100Twins, produced by TEGO of Germany.

[0081] The organic silicon twin structure wetting agent used in the present invention has good compatibility, good recoatability, and strong anti-shrinkage cratering, can reduce the surface tension of the substrate, reduce the surface energy of water, and the water-based paint film can be better spread on the surface of the substrate, and can avoid some shrinkage craters, pinholes and other defects in the paint film, enhance the leveling performance, and at the same time have good compatibility with water and organic solvents. When the paint film is thickly applied, the surface orange stripes are reduced and the appearance is better.

[0082] The leveling agent is an acrylic leveling agent, BYK348, produced by BYK of Germany.

[0083] The ultraviolet light absorber is ultraviolet light absorber Tinuvin 1130, produced by BASF of Germany.

[0084] The light stabilizer is Tinuvin 292, produced by BASF of Germany.

[0085] The flash rust inhibitor was Tech-8876, from Tiger Polymer Technology Co., Ltd.

[0086] The flash rust inhibitor is an organic carboxylate flash rust inhibitor that can form a passivation film on the surface of the substrate to prevent electrochemical corrosion between air, moisture and the substrate. At the same time, unlike traditional nitrite flash rust inhibitors, this flash rust inhibitor is not easy to hydrolyze, ensuring the excellent salt spray resistance and water resistance of the paint film.

[0087] The cosolvent is dipropylene glycol butyl ether, produced by Shanghai Tichem Industrial Co., Ltd.

[0088] The cosolvent used in the present invention is an environmentally friendly alcohol ether ester high boiling point solvent, which has excellent dissolving ability, can reduce the glass transition temperature of the emulsion polymer, and effectively improve the adhesion of the paint film.

[0089] The pigment and filler of the present invention is titanium dioxide, and the titanium dioxide is titanium dioxide 895 produced by Longbai Group Corporation.

[0090] The anti-rust pigment is a zinc-aluminum phosphate anti-rust pigment (mixed with zinc phosphate and aluminum tripolyphosphate in a mass ratio of 1:1), zinc phosphate: Hunan Ruishi Technology Development Co., Ltd., model: zp20;

[0091] Aluminum tripolyphosphate: Hunan Ruishi Technology Development Co., Ltd., model: AP.

[0092] In the embodiment of the present invention, the ratio of the two is 1:1.

[0093] DMEA, produced by Shanghai Yihua.

[0094] The HDI trimer curing agent is HT-100, Wanhua Chemical Group Co., Ltd.

[0095] The IPDI curing agent is Vestanat T1890E, produced by Evonik of Germany.

[0096] Propylene glycol methyl ether, produced by Shanghai Tichem Industrial Co., Ltd.

[0097] IPDI curing agent has excellent optical stability and chemical resistance. Its isocyanate group has low reactivity, which can extend the service life of the coating. It is suitable for long-term coating of large workpieces. Because it has a cycloalkane structure in its molecule, the strength of the cured network structure is better than other aliphatic isocyanates, and the paint film has excellent yellowing resistance.

[0098] The pH adjuster of the present invention is dimethylethanolamine.

[0099] Dimethylethanolamine has strong alkalinity and can adjust the pH value of the water-based paint system. Compared with ammonia, it evaporates slowly and has stable performance. Only in a weakly alkaline environment can the system performance of water-based paint be most stable and the construction performance be guaranteed, including thick coating performance.

[0100] Example

[0101] The raw materials and mass fractions of the water-based primer-and-surface coatings in Examples 1 to 3 of the present invention are shown in Table 1.

[0102] Table 1 Raw materials and mass fractions of water-based primer-and-surface coatings in Examples 1 to 3 of the present invention

[0103]

[0104]

[0105] The preparation method of the water-based primer-and-surface coating in Examples 1 to 3 of the present invention comprises the following steps:

[0106] S1. Preparation of paint:

[0107] Preparation of lithium magnesium silicate pre-slurry:

[0108] First, lithium magnesium silicate powder is added to water at a mass ratio of 1:15, and stirred at high speed for 10 minutes with a disperser at a speed of 1000 r / min to prepare lithium magnesium silicate pre-slurry;

[0109] Pour water into the container, and place the container under a disperser for dispersion, adjust the speed to 800r / min, and then add dispersant, lithium magnesium silicate pre-slurry, surfactant, defoamer, color filler and anti-rust pigment in sequence under stirring; after the addition is completed, adjust the speed of the disperser to 1000r / min, stir for 30 minutes, and obtain the pre-dispersed slurry;

[0110] Then use a diaphragm pump to pump the pre-dispersed slurry into the sand mill and grind it to a fineness of ≤15μm before discharging. Then add water-based acrylic dispersion I, water-based acrylic dispersion II, wetting agent, and leveling agent. After adding, adjust the speed of the disperser to 1200r / min, stir for 15 minutes, and finally add anti-rust agent, anti-sagging agent, co-solvent, ultraviolet light absorber, light stabilizer, DMEA and deionized water, stir for 15 minutes, and finally add water to adjust the viscosity (100s~120s (coat 4# cup)), filter with a 120-mesh filter to remove mechanical impurities.

[0111] S2. Preparation of curing agent:

[0112] Add isocyanate HDI curing agent, IPDI curing agent and ethylene glycol butyl ether acetate into a container cylinder, and place the container cylinder under a disperser for dispersion. Adjust the speed of the disperser to 1200r / min and stir for 10 minutes.

[0113] S3. Preparation of water-based primer and surface all-in-one coating:

[0114] When using, stir and mix the paint and curing agent in a weight ratio of 5:1. During construction, an appropriate amount of water can be used to adjust the construction viscosity (25s~35s (coating 4# cup)).

[0115] The test standard for the water-based primer and topcoat in the embodiment of the present invention is HG / T 4339-2012. The main performance test requirements and results of water-based primer and topcoat are shown in Table 2.

[0116] The thickness of the conventional mechanical properties paint film test board is 25μm~35μm, baked at 60℃ for 2h, and left to air for 16h before testing;

[0117] Type test sample 50μm±5μm (water-resistant, acid-resistant, alkali-resistant); let stand for 16 hours before testing;

[0118] 70μm~80μm (aging resistance, heat and humidity resistance, neutral salt spray resistance), bake at 60℃ for 2h, let stand for 7d, and then test.

[0119] Table 2 Performance test results of water-based primer-top coatings in the embodiments of the present invention

[0120]

[0121]

[0122]

[0123] In summary, the paint film prepared in the embodiment of the present invention has a salt spray resistance of ≥800h and a water resistance of ≥240h. The phosphate anti-rust pigment and the organic carboxylate anti-flash rust agent are used to form a passivation film on the surface of the substrate to prevent moisture from reacting with the substrate to cause rust. At the same time, unlike the traditional nitrite anti-flash rust agent, it is not easy to hydrolyze, thereby ensuring the excellent water resistance of the paint film. Resistance to artificial accelerated aging ≥800h. The cross-linking reaction of water-based acrylic dispersion and HDI and IPDI curing agents is used to make the paint film have good chemical resistance, weather resistance, and light and color retention. The paint film has good thick coating performance. The low-hydroxyl water-based acrylic dispersion is used, and the CO generated by the cross-linking reaction 2 It can be released without generating bubbles. At the same time, the glass transition temperature of the resin is high, the paint film is not easy to sag, and it is suitable for thick coating. One coat of coating does not sag, the paint film does not bubble, and the leveling performance is good. The maximum bubble film thickness reaches 80μm. The paint film has good storage stability and anti-sagging performance. Lithium magnesium silicate and polyurea modified anti-sagging additives and lithium magnesium silicate rheological additives are selected, and they have unique rheological properties. The primary particles are negatively charged on the front and positively charged on the side. When added to water, the dispersed primary particles are close to each other. Due to the charge repulsion, a "card house" structure is formed. The pigment particles are suspended in the three-dimensional structure gel, and the mobility is significantly reduced, showing a more excellent anti-settling effect. The modified polyurea solution anti-sagging additive can form more hydrogen bonds due to the large polarity of the urea group, and produce a three-dimensional network structure in the coating system to prevent the coating from settling and sagging. Low VOC content and no solvent odor. The resin used is a water-based dispersion and a solvent-free HDI curing agent with a high solid content of IPDI curing agent. The amount of co-solvent used does not exceed 5%. The solvent used is water, which has good environmental performance. It has good comprehensive performance and can meet the requirements of the HG / T 4339-2012 standard primer and topcoat for engineering machinery coatings.

[0124] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A water-based primer-and-surface coating, characterized in that: It includes component A and component B; The A component includes the following raw materials in parts by weight: 35 to 45 parts of the first aqueous acrylic dispersion, 12 to 15 parts of the second aqueous acrylic dispersion, 2 to 3 parts of lithium magnesium silicate pre-slurry, 2.0 to 2.5 parts of a dispersant, 0.8 to 1.0 parts of a nonionic surfactant, 0.2 to 0.3 parts of a defoamer, 0.3 to 0.5 parts of a wetting agent, 0.3 to 0.5 parts of a leveling agent, 15 to 20 parts of a pigment, 6 to 10 parts of an anti-rust pigment, 0.5 to 0.8 parts of an anti-sagging agent, 3 to 5 parts of a cosolvent, 0.5 to 1.0 parts of an anti-flash rust agent, 0.8 to 1.0 parts of an ultraviolet light absorber, 0.4 to 0.6 parts of a light stabilizer, 0.2 to 0.3 parts of DMEA, and 8 to 12 parts of water; The solid content of the first aqueous acrylic dispersion is 44% to 46%; the viscosity is 500 mPa•s to 4500 mPa•s at 25°C; and the hydroxyl content is 3.0% to 3.3%; The viscosity of the second aqueous acrylic dispersion is 50 mPa•s~2000 mPa•s, 25°C; the solid content is 40%~44%; the hydroxyl value is 50mgKOH / g~60mgKOH / g; The anti-flash rust agent includes an organic carboxylate anti-flash rust agent; the dispersant is an anionic polymer dispersant; the anti-sagging agent is a modified polyurea solution anti-sagging agent; The B component includes a curing agent and ethylene glycol butyl ether acetate; The curing agent includes at least one of an HDI trimer curing agent and an IPDI curing agent.

2. The water-based primer-and-surface coating according to claim 1, characterized in that: The wetting agent is an organic silicon twin structure wetting agent.

3. The water-based primer-and-surface all-in-one coating according to claim 1, characterized in that: The nonionic surfactant is an acetylenic diol nonionic surfactant.

4. A method for preparing the water-based primer-and-surface coating according to any one of claims 1 to 3, characterized in that: The following steps are involved: Mix components A and B.

5. Use of the water-based primer-surface all-in-one coating as claimed in any one of claims 1 to 3 in the preparation of engineering vehicles.