A HEMA-St core-shell copolymer and its application in TPE modified materials
The preparation of HEMA-St core-shell copolymer solved the compatibility problem of inorganic salt antibacterial agents in TPE materials, improved antibacterial and mechanical properties, and achieved enhanced antibacterial effect and aesthetics of the material.
Patent Information
- Application Number
- CN202310719212.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-16
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-06-16
AI Technical Summary
The inorganic salt antibacterial agents used in existing TPE materials are irritating to the skin and have poor compatibility with TPE, resulting in decreased antibacterial performance. In addition, the material surface is slippery, making it difficult to achieve the ideal antibacterial effect.
Using HEMA-St shell-core copolymer as a compatibility aid, a stable shell-core polymer structure is formed through secondary polymerization of 2-hydroxyethyl methacrylate, styrene, ethylene glycol phenyl ether, reactive emulsifier SR-10 and initiator in a specific ratio. This improves the compatibility between ethylene glycol phenyl ether and TPE, and prepares a TPE modified material with antibacterial and bacteriostatic effects.
The antibacterial and mechanical properties of TPE materials have been improved. The material surface has good toughness, is aesthetically pleasing and does not irritate the skin, thus achieving an enhanced antibacterial effect.
Smart Images

Figure BDA0004290588470000051 
Figure BDA0004290588470000061 
Figure BDA0004290588470000071
Abstract
Description
Technical Field
[0001] The present application relates to the field of plastic modification, and more specifically, to a HEMA-St core-shell copolymer and its application in TPE modified materials. Background Art
[0002] TPE is a thermoplastic elastomer material with high strength, high resilience, injection molding, wide application range, environmental protection, non-toxic and safe, and excellent colorability. Therefore, TPE materials are generally used to manufacture handles of various equipment, stationery, toys, toothbrush handles and other covering materials. Since TPE materials need to be in frequent contact with hands, they are usually treated with antibacterial and antimicrobial agents to avoid affecting the appearance and hygiene of the handles.
[0003] Ethylene glycol phenyl ether is a new generation of environmentally friendly broad-spectrum antibacterial agent based on water-based matrix. It has good bactericidal effect, broad spectrum, strong killing and inhibitory effects on various bacteria and viruses such as Gram-positive bacteria, Gram-negative bacteria, yeast, etc., safe and non-toxic, non-corrosive, stable performance, and long bactericidal effect.
[0004] At present, the antibacterial agents commonly used in TPE are copper oxide, ammonium dihydrogen phosphate and lithium carbonate, but these inorganic salt antibacterial agents are irritating to the skin and have poor compatibility with TPE, resulting in a decrease in the antibacterial performance of TPE. Therefore, there is still room for improvement. Summary of the invention
[0005] In order to improve the compatibility between TPE and antibacterial agents, so that TPE has better antibacterial properties and does not cause any irritation to the skin, and at the same time, has better mechanical properties, the present application provides a HEMA-St core-shell copolymer and its application in TPE modified materials.
[0006] In the first aspect, the present application provides a HEMA-St core-shell copolymer, which adopts the following technical solution:
[0007] A HEMA-St core-shell copolymer, wherein the preparation method of the HEMA-St core-shell copolymer is as follows:
[0008] S1: Preparation of styrene seed emulsion
[0009] Add 20-30 parts by mass of styrene, 40-50 parts by mass of water, 0.1-0.2 parts by mass of emulsifier, and 0.8-1.0 parts by mass of reactive emulsifier into a flask, stir evenly to form a milky white solution, then heat to 70-75° C., add 0.01-0.02 parts by mass of initiator, and react for 3-4 hours to obtain a styrene seed emulsion;
[0010] S2: Preparation of premixed emulsion
[0011] First, styrene and hydroxyethyl methacrylate are uniformly mixed to obtain a mixture A, and then water, an emulsifier, a reactive emulsifier, ethylene glycol phenyl ether and an initiator are mixed, and emulsified in a homogenizer for 3-5 minutes at a speed of 5000-8000 rpm to form a premixed emulsion;
[0012] S3: Preparation of HEMA-St core-shell copolymer
[0013] Add styrene seed emulsion and water into a flask, stir and heat to 70-75°C, rotate at 200-350rpm, add the premixed emulsion dropwise, blue fluorescence appears after the reaction, continue the reaction for 3-4h to obtain HEMA-St core-shell copolymer.
[0014] By adopting the above technical solution, ethylene glycol phenyl ether is used as an antibacterial agent because it is relatively mild and safe, and is not easy to irritate the skin. However, during the research and development process, the inventors found that ethylene glycol phenyl ether is not compatible with TPE materials. If ethylene glycol phenyl ether is added directly, ethylene glycol phenyl ether will overflow to the surface of the TPE material, which will make the surface of the material too slippery and difficult to achieve the antibacterial effect.
[0015] After extensive research, it was found that the use of styrene seed emulsion acts as a core in the styrene-hydroxyethyl methacrylate copolymerization process, which is beneficial for styrene-hydroxyethyl methacrylate to form a shell-core polymerization structure, so that ethylene glycol phenyl ether can be tightly connected to the shell-core polymerization structure, making it difficult for ethylene glycol phenyl ether to overflow from the surface of the material, and improving the compatibility between ethylene glycol phenyl ether and TPE, which is beneficial to improving the antibacterial properties of TPE materials.
[0016] Therefore, the present invention uses 2-hydroxyethyl methacrylate (HEMA) and styrene (St) as main raw materials, and is prepared by secondary polymerization with emulsifier, reactive emulsifier, initiator and ethylene glycol phenyl ether (EHP). HEMA-St plays the role of compatibility aid in the modification of thermoplastic elastomer (TPE). The surface of the modified TPE material has antibacterial and antimicrobial effects, and the surface of the TPE modified material has good toughness and beautiful effects.
[0017] Preferably, the mass ratio of water to mixture A in S2 is 1-1.5:1, the amount of emulsifier is 0.2-0.5% of mixture A, the amount of reactive emulsifier is 1.5-2.5% of mixture A, the amount of ethylene glycol phenyl ether is 15-30% of mixture A, and the amount of initiator is 0.1-0.3% of mixture A.
[0018] Preferably, the mass ratio of hydroxyethyl methacrylate, styrene and ethylene glycol phenyl ether in S2 is 10:(6-8):(3-5).
[0019] By adopting the above technical scheme, hydroxyethyl methacrylate, styrene and ethylene glycol phenyl ether are compounded in a specific ratio, so that ethylene glycol phenyl ether can form a more stable shell-core polymerization structure with styrene-hydroxyethyl methacrylate, making it difficult for ethylene glycol phenyl ether to overflow from the surface of the TPE material, thereby maintaining the antibacterial properties of the TPE modified material.
[0020] Preferably, the reactive emulsifier is an allyloxypropyl alkyl alcohol ether sulfosuccinate containing an allyl bond, including one of the nonylphenol type SE / NE series and the nonylphenol free type SR / ER series.
[0021] Preferably, the reactive emulsifier is reactive emulsifier SR-10.
[0022] By adopting the above technical solution, the reactive emulsifier SR-10 can participate in the polymerization due to its allyl group, and will not be freed like the emulsifier of small molecule chain, making the HEMA-St core-shell polymer more stable.
[0023] Preferably, the emulsifier is one of Span-80, Span-60, Triton-10 and Tween series.
[0024] Preferably, the emulsifier is Span-80.
[0025] By adopting the above technical solution, the nonionic emulsifier Span-80 is anhydrous sorbitan oleate, which assists the role of the reactive emulsifier in the reaction process, forms stable micelles with styrene and hydroxyethyl methacrylate, and forms a water-in-oil shell-core polymerization state after polymerization.
[0026] Preferably, the initiator is ammonium persulfate or potassium persulfate.
[0027] In the second aspect, the present application provides an application of a HEMA-St core-shell copolymer in a TPE modified material, using the following technical solution:
[0028] Application of a HEMA-St core-shell copolymer in a TPE modified material, wherein the TPE modified material comprises the following components in parts by mass:
[0029] Hydrogenated styrene-butadiene-styrene block copolymer (SEBS): 30-40 parts;
[0030] Copolymer PP: 35-50 parts;
[0031] HEMA-St core-shell copolymer: 3-5 parts;
[0032] White oil: 7-32 parts;
[0033] Antioxidant 0.2-0.4 parts;
[0034] Additives 0.2-0.4 parts.
[0035] By adopting the above technical solution, the HEMA-St core-shell copolymer is added to the TPE modified material, so that the prepared TPE modified material has better antibacterial and antimicrobial effects and mechanical properties.
[0036] Preferably, the auxiliary agent is one or both of calcium stearate and ethylene bisstearamide.
[0037] Preferably, the antioxidant is one or more of antioxidant 1010, antioxidant 168, and antioxidant 1076.
[0038] In summary, the present application includes at least one of the following beneficial technical effects:
[0039] 1. The present application uses 2-hydroxyethyl methacrylate (HEMA) and styrene (St) as main raw materials, with emulsifier, reactive emulsifier, initiator and ethylene glycol phenyl ether (EHP), and prepares HEMA-St core-shell copolymer through secondary polymerization. HEMA-St plays the role of compatibilizer in the modification of thermoplastic elastomer (TPE). The surface of the modified TPE material has antibacterial and antimicrobial effects, and the surface of the TPE modified material has good toughness and beautiful effects.
[0040] 2. Reactive emulsifier SR-10 is used to copolymerize with 2-hydroxyethyl methacrylate, styrene, emulsifier, initiator and ethylene glycol phenyl ether. Because it contains allyl groups, it can participate in the polymerization and will not be free like the emulsifier of small molecular chains, making the HEMA-St core-shell polymer more stable. DETAILED DESCRIPTION
[0041] The present application is further described in detail below with reference to the embodiments.
[0042] Preparation Example 1
[0043] A method for preparing a HEMA-St core-shell copolymer is as follows:
[0044] S1: Preparation of styrene seed emulsion
[0045] Add 20g styrene, 50g water, 0.2g emulsifier-Span-80, and 0.8g reactive emulsifier SR-10 into a flask (with stirring, condenser, and thermometer), stir evenly at a speed of 200rpm, and form a milky white solution after five minutes. Then heat it to 70°C, add 0.02g initiator-ammonium persulfate, and react for 3h to obtain a styrene seed emulsion;
[0046] Among them, the reactive emulsifier SR-10 was purchased from Aidico; Span-80 was purchased from Croda, UK;
[0047] S2: Preparation of premixed emulsion
[0048] First, 40g of styrene and 60g of hydroxyethyl methacrylate were mixed evenly to obtain 100g of mixture A, and then 95g of mixture A, 100g of water, 0.5g of emulsifier-Span-80, 2.0g of reactive emulsifier SR-10, 30g of ethylene glycol phenyl ether and 0.2g of initiator-ammonium persulfate were mixed in sequence, the reaction temperature was 75°C, and the homogenizer was emulsified for 3min at a speed of 5000rpm to form a premixed emulsion;
[0049] Among them, hydroxyethyl methacrylate was purchased from Wanhua Chemical; ethylene glycol anisole was purchased from Liaoning Dongke;
[0050] S3: Preparation of HEMA-St core-shell copolymer
[0051] Add styrene seed emulsion and water into a flask (with stirring, condenser, thermometer, nitrogen protection), stir and heat to 70°C, then add the remaining 5g of mixture A (40g of styrene, 60g of hydroxyethyl methacrylate, mix well), add ammonium persulfate solution dropwise, and the solution exhibits light blue fluorescence; keep the rotation speed at 200rpm, add the premixed emulsion dropwise, react for 15min until blue fluorescence appears, continue the reaction for 3h, and keep warm at 70°C for 1h to obtain HEMA-St core-shell copolymer with a solid content of 52%.
[0052] Preparation Example 2
[0053] The difference from Preparation Example 1 is that the mass ratio of hydroxyethyl methacrylate, styrene and ethylene glycol phenyl ether in S2 is 10:6:3.
[0054] Preparation Example 3
[0055] The difference from Preparation Example 1 is that the mass ratio of hydroxyethyl methacrylate, styrene and ethylene glycol phenyl ether in S2 is 10:8:5.
[0056] Preparation Example 4
[0057] The difference from Preparation Example 1 is that in S2, ethylene glycol phenyl ether is replaced by an equal amount of polyethylene glycol.
[0058] Preparation Example 5
[0059] The difference from Preparation Example 1 is that in S2, hydroxyethyl methacrylate is replaced by an equal amount of hydroxyethyl acrylate.
[0060] Preparation Example 6
[0061] The difference from Preparation Example 1 is that in S2, the homogenizer is emulsified for 8 minutes at a rotation speed of 9000 rpm.
[0062] Example 1
[0063] A TPE modified material comprises the following components:
[0064] Hydrogenated styrene-butadiene-styrene block copolymer (SEBS); copolymerized PP; HEMA-St core-shell copolymer; white oil; antioxidant; auxiliary agent; the antioxidants include antioxidant 1010 and antioxidant 168, and the auxiliary agents include calcium stearate and ethylene bisstearamide (EBS); the HEMA-St core-shell copolymer adopts the HEMA-St core-shell copolymer prepared in Preparation Example 1.
[0065] Among them, copolymer PP, PPK7726H, Yanshan Petrochemical; SEBS is YH-503 or YH-503T from Sinopec Baling; white oil is 32# white oil, Foshan Shaoji Chemical Company; calcium stearate is Changfeng Chemical; EBS is P-130 from Indonesia.
[0066] A method for preparing a TPE modified material, the steps are as follows:
[0067] According to Table 1, hydrogenated styrene-butadiene-styrene block copolymer, copolymer PP, HEMA-St core-shell copolymer, white oil, antioxidant and additives were added to the mixing barrel in sequence, and then the temperature was raised to 75°C, the emulsion was mixed with the TPE material, so that the emulsion adhered to the surface of the TPE material, and then the TPE material was dried and mixed evenly, extruded and granulated in a twin-screw extruder, the extrusion temperature was 180°C, the head temperature was 200°C, and the main engine speed was 400rpm to prepare a TPE modified material.
[0068] Table 1
[0069]
[0070] Example 2
[0071] The difference from Example 1 is that the HEMA-St core-shell copolymer is the HEMA-St core-shell copolymer prepared in Preparation Example 2.
[0072] Example 3
[0073] The difference from Example 1 is that the HEMA-St core-shell copolymer is the HEMA-St core-shell copolymer prepared in Preparation Example 3.
[0074] Example 4
[0075] The difference from Example 1 is that the HEMA-St core-shell copolymer is the HEMA-St core-shell copolymer prepared in Preparation Example 4.
[0076] Example 5
[0077] The difference from Example 1 is that the HEMA-St core-shell copolymer is the HEMA-St core-shell copolymer prepared in Preparation Example 5.
[0078] Example 6
[0079] The difference from Example 1 is that the HEMA-St core-shell copolymer is the HEMA-St core-shell copolymer prepared in Preparation Example 6.
[0080] Comparative Example 1
[0081] A method for preparing a TPE modified material, the steps are as follows:
[0082] According to Table 2, hydrogenated styrene-butadiene-styrene block copolymer, copolymer PP, white oil, antioxidant and additives were added to a mixing barrel in sequence and mixed evenly, and extruded and granulated in a twin-screw extruder at an extrusion temperature of 180°C, a die temperature of 200°C, and a main engine speed of 400 rpm to prepare a TPE modified material.
[0083] Comparative Example 2
[0084] A method for preparing a TPE modified material, the steps are as follows:
[0085] According to Table 2, hydrogenated styrene-butadiene-styrene block copolymer, copolymer PP, white oil, antioxidant and additives were added to a mixing barrel in sequence and mixed evenly, and extruded and granulated in a twin-screw extruder at an extrusion temperature of 180°C, a die temperature of 200°C, and a main engine speed of 400 rpm to prepare a TPE modified material.
[0086] Comparative Example 3
[0087] A method for preparing a TPE modified material, the steps are as follows:
[0088] According to Table 2, hydrogenated styrene-butadiene-styrene block copolymer, copolymer PP, white oil, antioxidant and additives were added to a mixing barrel in sequence and mixed evenly, and extruded and granulated in a twin-screw extruder at an extrusion temperature of 180°C, a die temperature of 200°C, and a main engine speed of 400 rpm to prepare a TPE modified material.
[0089] The dosage of each component in Table 2 is kg.
[0090] Table 2
[0091]
[0092]
[0093] Experiment 1 Determination of density: ISO 1183A (23°C, tested by method A (immersion method))
[0094] Experiment 2: Tensile strength test: ISO 527, 23°C, 50 mm / min
[0095] Experiment 3: Testing of elongation at break: ISO 527, 23°C, 50 mm / min
[0096] Experiment 4: Flexural strength test: ISO 178, 23°C, 2mm / min
[0097] Experiment 5: Flexural modulus test: ISO 178, 23°C, 2 mm / min
[0098] Experiment 6: Antibacterial rate test: QB / T 2591-2018
[0099] The above experimental results are shown in Table 3
[0100] Table 3
[0101]
[0102] According to the comparison between Example 4 and Example 1 in Table 3, the tensile strength and bending strength of the TPE modified material in Example 4 are basically close to those in Example 1, but the antibacterial rate of the TPE modified material in Example 4 is much lower than that in Example 1. This is because polyethylene glycol is used to replace ethylene glycol phenyl ether in Example 4. The structure of polyethylene glycol is similar to the hydrophilic group of the reactive emulsifier SR-10, and the compatibility of the two is improved, so the mechanics of the TPE material is improved. However, the antibacterial and antimicrobial properties of polyethylene glycol are far inferior to those of ethylene glycol phenyl ether, so the antibacterial rate of Example 4 is much lower than that of Example 1.
[0103] According to the comparison between Example 5 and Example 1 in Table 3, it can be obtained that an equal amount of hydroxyethyl acrylate is used to replace hydroxyethyl methacrylate in Example 5, and the antibacterial rate of the TPE modified material in Example 5 is lower than that in Example 1. This is because hydroxyethyl acrylate and styrene-hydroxyethyl methacrylate cannot form a shell-core polymerization structure well, so that ethylene glycol phenyl ether cannot be tightly connected to the shell-core polymerization structure, and thus ethylene glycol phenyl ether is easy to overflow the surface of the material, thereby reducing the compatibility between ethylene glycol phenyl ether and TPE, which in turn affects the antibacterial properties of the TPE material.
[0104] According to the comparison between Example 6 and Example 1 in Table 3, the emulsification time and rotation speed of the homogenizer in Example 6 are not within the scope protected by the present application, and the antibacterial performance of the TPE modified material in Example 6 is lower than that in Example 1. This is because the emulsification time is too long and the rotation speed is too high, which will cause demulsification, so that ethylene glycol phenyl ether cannot be tightly connected with styrene-hydroxyethyl methacrylate, and then ethylene glycol phenyl ether overflows from the surface of the material, thereby causing the antibacterial performance of the TPE modified material to decrease.
[0105] In summary, only by using a specific ratio of ethylene glycol phenyl ether, hydroxyethyl methacrylate and reactive emulsifier SR-10, and matching a specific reaction temperature, emulsification time and rotation speed, can the HEMA-St core-shell copolymer be well compatible with TPE, thereby making the TPE modified material have better antibacterial and mechanical properties.
[0106] According to the comparison of Comparative Examples 1-3 in Table 3 with Example 1, no HEMA-St core-shell copolymer or antibacterial agent was added in Comparative Example 1, no HEMA-St core-shell copolymer was added in Comparative Example 2, and ethylene glycol phenyl ether was added, no HEMA-St core-shell copolymer was added in Comparative Example 3, and an inorganic silver ion antibacterial agent was added. The tensile strength and flexural strength of the TPE modified materials in Comparative Examples 1-3 were lower than those in Example 1, and the antibacterial rate was also lower than that in Example 1. It is shown that the synergistic combination of HEMA-St core-shell copolymer, hydrogenated styrene-butadiene-styrene block copolymer and copolymerized PP makes the TPE modified material have higher antibacterial properties and mechanical properties.
[0107] The above experiments verified that the HEMA-St core-shell copolymer prepared by the present application is well compatible with TPE, the surface of the modified TPE material has excellent antibacterial and antimicrobial effects, and the surface of the TPE modified material has good toughness and beautiful effects.
[0108] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.
Claims
1. A 2-hydroxyethyl methacrylate (HEMA)-styrene (St) core-shell copolymer, characterized in that: The preparation method of the HEMA-St core-shell copolymer is as follows: S1: Preparation of styrene seed emulsion Add 20-30 parts by mass of styrene, 40-50 parts by mass of water, 0.1-0.2 parts by mass of emulsifier, and 0.8-1.0 parts by mass of reactive emulsifier into a flask, stir evenly to form a milky white solution, then heat to 70-75° C., add 0.01-0.02 parts by mass of initiator, and react for 3-4 hours to obtain a styrene seed emulsion; S2: Preparation of premixed emulsion First, styrene and hydroxyethyl methacrylate are uniformly mixed to obtain a mixture A, and then water, an emulsifier, a reactive emulsifier, ethylene glycol phenyl ether and an initiator are added and mixed, and emulsified in a homogenizer for 3-5 minutes at a speed of 5000-8000 rpm to form a premixed emulsion; The mass ratio of hydroxyethyl methacrylate, styrene and ethylene glycol phenyl ether is 10:(6-8):(3-5); S3: Preparation of HEMA-St core-shell copolymer Add styrene seed emulsion and water into a flask, stir and heat to 70-75°C, rotate at 200-350rpm, drop the premixed emulsion, blue fluorescence appears after reaction, continue the reaction for 3-4h, and obtain HEMA-St core-shell copolymer; The reactive emulsifier is an allyloxypropyl alkyl alcohol ether sulfosuccinate containing an allyl bond, including one of the nonylphenol type SE / NE series and the nonylphenol free type SR / ER series; The emulsifier is one of Span-80, Span-60, Triton-10 and Tween series.
2. A HEMA-St core-shell copolymer according to claim 1, characterized in that: The mass ratio of water to mixture A in S2 is 1-1.5:1, the amount of emulsifier is 0.2-0.5% of mixture A, the amount of reactive emulsifier is 1.5-2.5% of mixture A, the amount of ethylene glycol phenyl ether is 15-30% of mixture A, and the amount of initiator is 0.1-0.3% of mixture A.
3. A HEMA-St core-shell copolymer according to claim 1, characterized in that: The reactive emulsifier was reactive emulsifier SR-10.
4. A HEMA-St core-shell copolymer according to claim 1, characterized in that: The emulsifier is Span-80.
5. Use of the HEMA-St core-shell copolymer according to any one of claims 1 to 4 in TPE modified materials, characterized in that: The TPE modified material comprises the following components in parts by mass: Hydrogenated styrene-butadiene-styrene block copolymer (SEBS): 30-40 parts; Copolymer PP: 35-50 parts; HEMA-St core-shell copolymer: 3-5 parts; White oil: 7-32 parts; Antioxidant 0.2-0.4 parts; Additives 0.2-0.4 parts.
6. The use of a HEMA-St core-shell copolymer in TPE modified materials according to claim 5, characterized in that: The auxiliary agent is one or two of calcium stearate and ethylene bisstearamide.
7. The use of a HEMA-St core-shell copolymer in TPE modified materials according to claim 5, characterized in that: The antioxidant is one or more of antioxidant 1010 , antioxidant 168 , and antioxidant 1076 .