A hydrophobic modified aerogel composite epoxy resin water-insulating coating and preparation method thereof

By combining the hydrophobic modified aerogel with epoxy resin polymer, an interpenetrating polymer network is formed, which solves the problem of insufficient fire-resistance and thermal insulation properties and mechanical properties of aqueous epoxy resin coatings, and achieves high mechanical strength and anti-flow sag Hydrophobically modified aerogel composite epoxy resin coating with properties and thermal insulation properties, suitable for high-temperature building environments.

CN116751489BActive Publication Date: 2024-11-26CHANGCHUN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310936596.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-28
Publication Date
2024-11-26
Estimated Expiration
2043-07-28

AI Technical Summary

Technical Problem

The fire-proof and thermal insulation properties and mechanical properties of existing water-based epoxy resin coatings are weak and have insufficient hydrophobicity, which limits its application scope and development.

Method used

By combining the hydrophobic modified aerogel with the epoxy resin polymer framework, an interpenetrating polymer network is formed, which enhances the hydrophobicity and thermal insulation properties of the coating. The silane coupling agent is grafted with alcohol esters and silicone compounds, forming an alcohol ester with a silane coupling agent. Hydrophobic modified aerogel particles with high mechanical strength and low surface energy, combined with water, ethanol, cellulose mixed ether, dispersant and ash calcium powder, prepare hydrophobic modified with good sag resistance and heat insulation properties. Aerogel composite epoxy resin coating.

Benefits of technology

It realizes the high mechanical strength, good sag resistance, thermal insulation and hydrophobic ability of the coating. It is suitable for building surfaces of different shapes and specifications, with good high temperature resistance and low thermal conductivity, and is suitable for below 300~600℃ High temperature environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004363603860000081
    Figure BDA0004363603860000081
  • Figure BDA0004363603860000101
    Figure BDA0004363603860000101
  • Figure BDA0004363603860000111
    Figure BDA0004363603860000111
Patent Text Reader

Abstract

The present invention discloses a hydrophobically modified aerogel composite epoxy resin water-insulating water paint and a preparation method thereof, comprising the following raw materials: water, a film-forming aid, a cellulose mixed ether, a dispersant, hydrophobically modified aerogel particles, an aqueous emulsion, an epoxy resin polymer, lime powder and wood fiber. The preparation method comprises the following steps: (1) mixing and stirring water, a film-forming aid and a cellulose mixed ether, adjusting the pH, and then sequentially adding a dispersant, a hydrophobically modified aerogel particles and an aqueous emulsion to obtain a mixed dispersion; (2) sequentially adding an epoxy resin polymer, lime powder and wood fiber to the mixed dispersion to obtain the hydrophobically modified aerogel composite epoxy resin water-insulating water paint. The water-based paint provided by the present invention has good anti-sagging properties, and at the same time, has good heat insulation performance and wear resistance, has a certain anti-corrosion function and strong hydrophobic ability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of coating preparation, and in particular relates to a hydrophobically modified aerogel composite epoxy resin water-insulating coating and a preparation method thereof. Background Art

[0002] At present, most of the coatings on the market are mainly based on artificial synthetic resins. The resulting coatings contain organic solvents and certain toxic pigments and additives, which are easy to cause environmental pollution and endanger human health. As people pay more attention to their own health and environmental issues, they pay more and more attention to the pollution and toxicity of coatings. Countries around the world have successively introduced relevant laws and regulations, and put forward strict requirements on the environmental protection of coatings. Therefore, water-based special coatings have become the research and development focus of environmentally friendly thermal insulation coatings due to their safety, environmental protection, convenience and other advantages.

[0003] Waterborne epoxy resin coating is a kind of coating with epoxy resin as base material and water as solvent or dispersion medium. It not only has the advantages of saving resources, no fire hazard, non-toxic and odorless, low pollution, strong anti-corrosion performance, easy to clean the painted surface, easy brushing construction, but also has good wear resistance. However, due to its weak fireproof and heat insulation performance, weak mechanical properties, poor hydrophobicity and other shortcomings, the application scope and further development of waterborne epoxy resin coating are limited. In the prior art, it is often modified by using other substances to compound with waterborne epoxy resin, thereby enhancing the comprehensive performance of waterborne epoxy resin coating. For example, aerogel itself already has certain heat resistance, solvent resistance, excellent hydrophobicity and other properties, and then the aerogel is further hydrophobically modified to achieve hydrophobicity. The hydrophobically modified aerogel composite epoxy resin has the excellent properties of both epoxy resin and aerogel, and has a wide range of application prospects.

[0004] Therefore, how to provide a hydrophobic modified aerogel composite epoxy resin coating with good anti-sagging properties, thermal insulation performance and hydrophobicity that meets the needs of social development is a technical problem that technical personnel in this field urgently need to solve. Summary of the invention

[0005] In order to solve the above technical problems, the present invention proposes a hydrophobic modified aerogel composite epoxy resin coating which has good anti-sagging properties, thermal insulation performance and hydrophobicity and meets the needs of social development.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] A hydrophobic modified aerogel composite epoxy resin water-insulating paint comprises the following raw materials in parts by weight:

[0008] 10 parts of water, 1 part of film-forming aid, 0.5 parts of cellulose mixed ether, 0.2-0.4 parts of dispersant, 5-10 parts of hydrophobically modified aerogel particles, 1.2 parts of aqueous emulsion, 1 part of epoxy resin polymer, 15-20 parts of lime powder and 0.5-0.7 parts of wood fiber.

[0009] Beneficial effects: The present invention first obtains a composite epoxy resin polymer skeleton, which can play a supporting role, and then uses a silane coupling agent to graft the aerogel with an organic siloxane to obtain a hydrophobically modified aerogel. Finally, the modified aerogel is grafted onto the epoxy resin polymer skeleton under the action of a coupling agent to obtain a hydrophobically modified aerogel composite epoxy resin. The epoxy resin polymer skeleton forms a network structure, which can form a relatively dense film on the surface of the substrate. When the modified aerogel is added, it is filled in the epoxy resin polymer network structure. The micro-nano protrusions maintain a large amount of air between the droplets and the surface, greatly reducing the contact area, thereby increasing the hydrophobicity.

[0010] Preferably, the preparation of the epoxy resin polymer comprises the following steps:

[0011] After mixing the silane coupling agent, water and anhydrous ethanol, the pH is adjusted, and then a fatty alcohol is added for ultrasonic dispersion and stirred for reaction, and then epoxy resin is added and stirred for reaction again to obtain the epoxy resin polymer.

[0012] Beneficial effects: The present invention mixes alcohol ester and epoxy resin through a silane coupling agent to prepare a composite polymer with an interpenetrating polymer network, and almost all properties of the polymer inherit the advantages of the raw materials, such as high mechanical strength obtained from the epoxy resin and low surface area obtained from the alcohol ester.

[0013] Preferably, the mass ratio of the silane coupling agent, water, anhydrous ethanol alcohol and epoxy resin is 0.3:1:5:1:(1.5-2.0);

[0014] The pH is adjusted to 10 using NaOH with a concentration of 1 mol / L, and after the pH is adjusted, stirring is performed at 70° C. and 200 r / min for 1 hour;

[0015] The ultrasonic temperature is room temperature, and the ultrasonic time is 10 min;

[0016] The stirring reaction time is 1h;

[0017] The epoxy resin is added at 40° C. and 200 r / min;

[0018] The stirring reaction time is 8 hours.

[0019] Beneficial effect: Stirring can ensure that the aerogel is fully and evenly dispersed in the anhydrous ethanol. 70°C and 200r / min can ensure that the silane coupling agent and the fatty alcohol can fully contact and react, which is conducive to the subsequent successful grafting of epoxy resin.

[0020] Preferably, the silane coupling agent includes one of γ-(2,3-epoxypropoxy)propyltrimethoxysilane, γ-aminopropyltriethoxysilane, vinyltriethoxysilane and methacryloxypropyltrimethylsilane;

[0021] The alcohol ester includes one of dimethylphenylsilane, polydimethylsiloxane, polymethyltriethoxysilane and polymethyldiethoxysilane.

[0022] Beneficial effects: The alcohol ester in the present invention has low surface energy, simple curing conditions, good adhesion to various substrates, and is an ideal polymer material for super hydrophobic coatings. Silane coupling agents can graft chains on alcohol esters, so that the grafted chains contain epoxy side chains, which are similar to the molecular chain structure of epoxy resins.

[0023] Preferably, the preparation of the hydrophobically modified aerogel particles comprises the following steps: adding an organosilicon compound and a silane coupling agent to an aerogel ethanol dispersion, stirring the mixture for reaction, and then centrifugally drying the mixture to obtain the hydrophobically modified aerogel particles.

[0024] Beneficial effects: Aerogel is an inorganic substance. The silane coupling agent provides a low surface energy functional group, which can serve as a bridge for inorganic substances to graft the organosilicon compound onto the aerogel to obtain aerogel particles with hydrophobic properties.

[0025] Preferably, in the aerogel ethanol dispersion, the mass ratio of aerogel particles to anhydrous ethanol is 1:5;

[0026] The mass ratio of the aerogel particles, the organosilicon compound and the silane coupling agent is 1:0.5:0.3;

[0027] When the aerogel particles are dispersed in anhydrous ethanol, they need to be ultrasonicated at room temperature for 30 minutes and then transferred to a magnetic stirrer and stirred for 30 minutes;

[0028] The stirring reaction temperature is 45°C, the solvent is removed by centrifugation after the reaction for 30 minutes, and then dried at 45°C for 6 hours;

[0029] The drying temperature is 120° C. and the drying time is 5 hours.

[0030] Preferably, the aerogel particles have an average particle size of 100 μm, and include one or any combination of silicon dioxide aerogel particles, titanium dioxide aerogel particles, copper oxide aerogel particles, zirconium dioxide aerogel particles, and aluminum oxide aerogel particles;

[0031] The organosilicon compound includes one of 1H,1H,2H,2H-perfluorodecyltriethoxysilane, 1H,1H,2H,2H-perfluorooctyltrimethylsiloxane and 1H,1H,2H,2H-perfluorooctyltriethoxysilane.

[0032] Beneficial effects: The present invention requires that the particle size of the aerogel particles be as small as possible to facilitate subsequent dispersion in anhydrous ethanol, and the inorganic aerogel is selected to facilitate enhancing the hydrophobic and thermal insulation properties of the coating. The fluorine-containing organosilicon compound can be grafted onto the aerogel through a coupling agent to enhance the hydrophobic properties of the aerogel, while reducing the surface energy and enhancing the compatibility with the polymer matrix.

[0033] Preferably, the cellulose mixed ether includes one of hydroxyethyl carboxymethyl cellulose, hydroxypropyl methyl cellulose and hydroxyethyl methyl cellulose;

[0034] The alcohol includes one of propylene glycol, alcohol ester dodecanol and hexadecanol ester;

[0035] The dispersant includes one of ammonium polycarboxylate, ammonium polyacrylate, sodium polyacrylate and potassium polyacrylate;

[0036] The aqueous emulsion includes one of styrene acrylic emulsion, acrylic emulsion and vinyl propionate emulsion;

[0037] The lime powder includes one or any combination of calcium carbonate, calcium hydroxide, titanium dioxide, talc and kaolin;

[0038] The thickener comprises one of diatomaceous earth, fumed silica and sodium-based expanded soil.

[0039] Beneficial effects: The above-mentioned cellulose mixed ether can play a certain emulsifying and stabilizing role in the coating, maintain the dispersed state of the particles in the coating, and prevent stratification. Alcohol, as an additive in the coating, can improve the performance of the coating and increase the performance and service life of the coating. Low relative molecular mass dispersants can improve the stability of the coating dispersion system. Adding water-based emulsion can obtain a good anti-sagging effect and reduce the occurrence of coagulation or flocculation. The calcium carbonate in the lime powder forms a network structure with the film-forming substance in the coating, which improves the water resistance and scour resistance of the coating.

[0040] A method for preparing a hydrophobically modified aerogel composite epoxy resin water-insulating thermal coating comprises the following steps:

[0041] (1) mixing water, ethanol and cellulose mixed ether and stirring, adjusting the pH, and then sequentially adding a dispersant, hydrophobically modified aerogel particles and an aqueous emulsion to obtain a mixed dispersion;

[0042] (2) Adding epoxy resin polymer, lime lime powder and wood fiber to the mixed dispersion in sequence to obtain the hydrophobically modified aerogel composite epoxy resin water-insulating paint.

[0043] Beneficial effects: Adjusting the pH after mixing and stirring can keep the coating stable for a long time under alkaline conditions. The pH value of the coating has a certain influence on its storage stability, anti-corruption, viscosity and coating performance.

[0044] Preferably, the mixing and stirring time in step (1) is 2 hours;

[0045] The pH is adjusted to between 9 and 10 using a buffer solution.

[0046] A coating method of a hydrophobically modified aerogel composite epoxy resin water-insulating paint comprises the following steps:

[0047] The hydrophobic modified aerogel composite epoxy resin water-insulating paint is mixed with a curing agent and then coated.

[0048] More preferably, the mass ratio of the hydrophobically modified aerogel composite epoxy resin water-insulating coating to the curing agent is 10:4.

[0049] The curing agent includes one of 4.4'-diaminodiphenyl sulfone, 4.4'-diaminodiphenylmethane and 4.4'-methylenedianiline.

[0050] The invention discloses a hydrophobically modified aerogel composite epoxy resin heat-insulating water-based coating and a preparation method thereof. The obtained water-based coating has good coating stability after film formation, so that the coating substrate is difficult to be corroded by acid and alkali. The water-based coating provided by the invention has good anti-sagging property, and at the same time has good heat-insulating property and wear resistance, has certain anti-corrosion function and strong hydrophobic ability.

[0051] The modified aerogel composite epoxy resin thermal insulation water-soluble paint provided by the invention can be directly coated or sprayed on a substrate to prepare an aerogel epoxy resin composite coating, and has the advantages of a relatively simple preparation method, easy implementation, simple operation, and little environmental pollution. The invention can be used to prepare an aerogel composite epoxy resin thermal insulation coating on the exterior walls and interior walls of buildings of different shapes and specifications. The coating has good high temperature resistance, an adjustable use temperature, and can be used for a long time below 300-600°C. The modified aerogel composite epoxy resin coating has low thermal conductivity, a thermal conductivity coefficient between 0.02 and 0.08 W / m·K, is easy to apply and brush during use, and has a smooth and bright surface, and has good application prospects in building environments requiring high temperature resistance and high efficiency thermal insulation. DETAILED DESCRIPTION

[0052] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0053] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below in conjunction with specific implementation methods.

[0054] Example 1

[0055] A method for preparing a hydrophobically modified aerogel composite epoxy resin water-insulating thermal coating comprises the following steps:

[0056] (1) Preparation of epoxy resin polymer:

[0057] First, 2.0 parts of silane coupling agent and 1 part of deionized water were mixed and dissolved in 5 parts of anhydrous ethanol, 1 mol / L NaOH solution was added to adjust the pH to 10, 1.0 part of fatty alcohol (polydimethylsiloxane) was added after mixing and stirring, and ultrasonic dispersion was performed for 10 minutes, followed by magnetic stirring at 70°C to ensure sufficient contact and reaction, and the stirring reaction was continued for 1 hour; finally, 1.6 parts of epoxy resin were added at 45°C, and magnetic stirring was performed at a stirring rate of 200 r / min for 8 hours to obtain an epoxy resin polymer;

[0058] (2) Preparation of hydrophobically modified aerogel particles:

[0059] 1.0 part of aerogel particles with an average diameter of 100 μm was dispersed in 5 parts of anhydrous ethanol, subjected to ultrasound at room temperature for 30 minutes, and then subjected to magnetic stirring for 30 minutes, and then 0.5 parts of an organic silicon compound (1H, 1H, 2H, 2H-perfluorodecyltriethoxysilane) and 0.3 parts of γ-aminopropyltriethoxysilane were added thereto, and stirred at 45°C, reacted for 30 minutes, centrifuged to remove the solvent, and then dried at 45°C for 6 hours to obtain hydrophobically modified aerogel particles;

[0060] (3) Preparation of hydrophobically modified aerogel composite epoxy resin water-insulating thermal coating:

[0061] 1) Using water as a solvent, add 1 part of a film-forming aid (propylene glycol) and 0.5 parts of a cellulose mixed ether (hydroxypropyl methylcellulose) to 10 parts of water, stir with a stirrer for 2 hours, and adjust the pH to between 9 and 10 with a buffer solution to make it a transparent solution;

[0062] 2) Add 0.2 parts of dispersant (ammonium polyacrylate) to the obtained transparent solution, stir evenly, then add 5 parts of hydrophobically modified aerogel, stir and add 1.2 parts of aqueous emulsion (acrylic emulsion) at a stirring rate of 80 r / min, add 1 part of epoxy resin polymer, stir evenly with a stirrer, and add 15 parts of lime powder and 0.5 parts of wood fiber evenly at a low speed, stir evenly, then add 0.2 parts of thickener (gas-phase SiO2), and adjust the consistency to an appropriate range to obtain a hydrophobically modified aerogel-composite epoxy resin anticorrosive and water-insulating water-based coating.

[0063] (4) Mix 1 part of the hydrophobically modified aerogel-composite epoxy resin anticorrosive and heat-insulating water-soluble coating obtained in step (3) with 0.4 parts of 4.4'-diaminodiphenylmethane and spray it on the surface of the substrate, dry it at 120°C for 30 minutes, and cure it at 80°C for 6 hours to obtain a hydrophobically modified aerogel composite epoxy resin coating. The performance indicators of the obtained coating are shown in Table 1.

[0064] Table 1

[0065]

[0066] Example 2

[0067] A method for preparing a hydrophobically modified aerogel composite epoxy resin water-insulating thermal coating comprises the following steps:

[0068] (1) Preparation of epoxy resin polymer:

[0069] First, 2.0 parts of silane coupling agent and 1 part of deionized water were mixed and dissolved in 5.0 parts of anhydrous ethanol, 1 mol / L NaOH solution was added to adjust the pH to 10, 1.0 part of fatty alcohol (polydimethylsiloxane) was added after mixing and stirring, and ultrasonic dispersion was performed for 10 minutes, followed by magnetic stirring at 70°C to ensure sufficient contact and reaction, and the stirring reaction was continued for 1 hour; finally, 1.5 parts of epoxy resin was added at 45°C, and magnetic stirring was performed at a stirring rate of 200 r / min for 8 hours to obtain an epoxy resin polymer;

[0070] (2) Preparation of hydrophobically modified aerogel particles:

[0071] 1.0 part of aerogel particles with an average diameter of 100 μm was dispersed in 5 parts of anhydrous ethanol, subjected to ultrasound at room temperature for 30 minutes, and then subjected to magnetic stirring for 30 minutes, and then 0.5 parts of an organic silicon compound (1H, 1H, 2H, 2H-perfluorodecyltriethoxysilane) and 0.3 parts of γ-aminopropyltriethoxysilane were added thereto, stirred at 45°C, reacted for 30 minutes, centrifuged to remove the solvent, and then dried at 45°C for 6 hours to obtain hydrophobically modified aerogel particles;

[0072] (3) Preparation of hydrophobically modified aerogel composite epoxy resin water-insulating thermal coating:

[0073] 1) Using water as a solvent, add 1 part of a film-forming aid (propylene glycol) and 0.5 parts of a cellulose mixed ether (hydroxypropyl methylcellulose) to 10 parts of water, stir with a stirrer for 2 hours, and adjust the pH to between 9 and 10 with a buffer solution to make it a transparent solution;

[0074] 2) Add 0.2 parts of dispersant (ammonium polyacrylate) to the obtained transparent solution, stir evenly, then add 5 parts of hydrophobically modified SiO2 aerogel, add 1.2 parts of aqueous emulsion (acrylic emulsion) under low-speed stirring, add 1 part of epoxy resin polymer, stir evenly with a stirrer, and add 15 parts of lime powder and 0.5 parts of wood fiber evenly at a low speed, stir evenly, add 0.2 parts of thickener (gas-phase SiO2), and adjust the consistency to an appropriate range to obtain a hydrophobically modified aerogel-composite epoxy resin anti-corrosion and water-insulating coating.

[0075] (4) Mix 1 part of the hydrophobically modified aerogel-composite epoxy resin anticorrosive and heat-insulating water-soluble coating obtained in step (3) with 0.4 parts of 4.4'-diaminodiphenylmethane and spray it on the surface of the substrate, dry it at 120°C for 30 minutes, and cure it at 80°C for 6 hours to obtain a hydrophobically modified aerogel composite epoxy resin coating. The performance indicators of the hydrophobically modified aerogel composite epoxy resin coating in this embodiment were tested, and the results are shown in Table 2 below.

[0076] Table 2

[0077]

[0078] Example 3

[0079] A method for preparing a hydrophobically modified aerogel composite epoxy resin water-insulating thermal coating comprises the following steps:

[0080] (1) Preparation of epoxy resin polymer:

[0081] First, 2.0 parts of silane coupling agent and 1 part of deionized water were mixed and dissolved in 5.0 parts of anhydrous ethanol, 1 mol / L NaOH solution was added to adjust the pH to 10, 1.0 part of fatty alcohol (polydimethylsiloxane) was added after mixing and stirring, and ultrasonic dispersion was performed for 10 minutes, followed by magnetic stirring at 70°C to ensure sufficient contact and reaction, and the stirring reaction was continued for 1 hour; finally, 2.0 parts of epoxy resin were added at 45°C, and magnetic stirring was performed at a stirring rate of 200 r / min for 8 hours to obtain an epoxy resin polymer;

[0082] (2) Preparation of hydrophobically modified aerogel particles:

[0083] 1.0 part of aerogel particles with an average diameter of 100 μm was dispersed in 5 parts of anhydrous ethanol, subjected to ultrasound at room temperature for 30 minutes, and then subjected to magnetic stirring for 30 minutes, and then 0.5 parts of an organic silicon compound (1H, 1H, 2H, 2H-perfluorodecyltriethoxysilane) and 0.3 parts of γ-aminopropyltriethoxysilane were added thereto, stirred at 45°C, reacted for 30 minutes, centrifuged to remove the solvent, and then dried at 45°C for 6 hours to obtain hydrophobically modified aerogel particles;

[0084] (3) Preparation of hydrophobically modified aerogel composite epoxy resin water-insulating thermal coating:

[0085] 1) Using water as a solvent, add 1 part of a film-forming aid (propylene glycol) and 0.5 parts of a cellulose mixed ether (hydroxypropyl methylcellulose) to 10 parts of water, stir with a stirrer for 2 hours, and adjust the pH to between 9 and 10 with a buffer solution to make it a transparent solution;

[0086] 2) Add 0.3 parts of dispersant (ammonium polyacrylate) to the obtained transparent solution, stir evenly, then add 5 parts of hydrophobically modified SiO2 aerogel, add 1.2 parts of aqueous emulsion (acrylic emulsion) under low-speed stirring, add 1 part of epoxy resin polymer, stir evenly with a stirrer, and add 20 parts of lime powder and 0.7 parts of wood fiber evenly at a low speed, stir evenly, add 0.2 parts of thickener (gas-phase SiO2), and adjust the consistency to an appropriate range to obtain a hydrophobically modified aerogel-composite epoxy resin anti-corrosion and water-insulating coating.

[0087] (4) Mix 1 part of the hydrophobically modified aerogel-composite epoxy resin anticorrosive and water-insulating water-soluble coating obtained in step (3) with 0.4 parts of 4.4'-diaminodiphenylmethane and spray it on the surface of the substrate, dry it at 120°C for 30 minutes, and cure it at 80°C for 6 hours to obtain a hydrophobically modified aerogel composite epoxy resin coating. The performance indicators of the hydrophobically modified aerogel composite epoxy resin coating in this embodiment were tested, and the results are shown in Table 3 below:

[0088] Table 3

[0089]

[0090] Example 4

[0091] A method for preparing a hydrophobically modified aerogel composite epoxy resin water-insulating thermal coating comprises the following steps:

[0092] (1) Preparation of epoxy resin polymer:

[0093] First, 2.0 parts of silane coupling agent and 1 part of deionized water were mixed and dissolved in 5.0 parts of anhydrous ethanol, 1 mol / L NaOH solution was added to adjust the pH to 10, 1.0 part of fatty alcohol (polydimethylsiloxane) was added after mixing and stirring, and ultrasonic dispersion was performed for 10 minutes, followed by magnetic stirring at 70°C to ensure sufficient contact and reaction, and the stirring reaction was continued for 1 hour; finally, 2.0 parts of epoxy resin were added at 45°C, and magnetic stirring was performed at a stirring rate of 200 r / min for 8 hours to obtain an epoxy resin polymer;

[0094] (2) Preparation of hydrophobically modified aerogel particles:

[0095] 1.0 part of aerogel particles with an average diameter of 100 μm was dispersed in 5 parts of anhydrous ethanol, subjected to ultrasound at room temperature for 30 minutes, and then subjected to magnetic stirring for 30 minutes, and then 0.5 parts of an organic silicon compound (1H, 1H, 2H, 2H-perfluorodecyltriethoxysilane) and 0.3 parts of γ-aminopropyltriethoxysilane were added thereto, stirred at 45°C, reacted for 30 minutes, centrifuged to remove the solvent, and then dried at 45°C for 6 hours to obtain hydrophobically modified aerogel particles;

[0096] (3) Preparation of hydrophobically modified aerogel composite epoxy resin water-insulating thermal coating:

[0097] 1) Using water as a solvent, add 1 part of a film-forming aid (propylene glycol) and 0.5 parts of a cellulose mixed ether (hydroxypropyl methylcellulose) to 10 parts of water, stir with a stirrer for 2 hours, and adjust the pH to between 9 and 10 with a buffer solution to make it a transparent solution;

[0098] 2) Add 0.4 parts of dispersant (ammonium polyacrylate) to the obtained transparent solution, stir evenly, then add 10 parts of hydrophobically modified SiO2 aerogel, add 1.2 parts of aqueous emulsion (acrylic emulsion) under low-speed stirring, add 1 part of epoxy resin polymer, stir evenly with a stirrer, and add 20 parts of lime powder and 0.5 parts of wood fiber evenly at a low speed, stir evenly, then add 0.2 parts of thickener (gas-phase SiO2), and adjust the consistency to an appropriate range to obtain a hydrophobically modified aerogel-composite epoxy resin anticorrosive and water-insulating water-based coating.

[0099] (4) Mix 1 part of the hydrophobically modified aerogel-composite epoxy resin anticorrosive and water-insulating water-soluble coating obtained in step (3) with 0.4 parts of 4.4'-diaminodiphenylmethane and spray it on the surface of the substrate, dry it at 120°C for 30 minutes, and cure it at 80°C for 6 hours to obtain a hydrophobically modified aerogel composite epoxy resin coating. The performance indicators of the hydrophobically modified aerogel composite epoxy resin coating in this embodiment were tested, and the results are shown in Table 4 below:

[0100] Table 4

[0101]

[0102]

[0103] Example 5

[0104] A method for preparing a hydrophobically modified aerogel composite epoxy resin water-insulating thermal coating comprises the following steps:

[0105] (1) Preparation of epoxy resin polymer:

[0106] First, 2.0 parts of silane coupling agent and 1 part of deionized water were mixed and dissolved in 5.0 parts of anhydrous ethanol, 1 mol / L NaOH solution was added to adjust the pH to 10, 1.0 part of fatty alcohol (polymethyltriethoxysilane) was added after mixing and stirring, and ultrasonic dispersion was performed for 10 minutes, followed by magnetic stirring at 70°C to ensure sufficient contact and reaction, and the stirring reaction was continued for 1 hour; finally, 2.0 parts of epoxy resin were added at 45°C, and magnetic stirring was performed at a stirring rate of 200 r / min for 8 hours to obtain an epoxy resin polymer;

[0107] (2) Preparation of hydrophobically modified aerogel particles:

[0108] 1.0 part of aerogel particles with an average diameter of 100 μm was dispersed in 5 parts of anhydrous ethanol, subjected to ultrasound at room temperature for 30 minutes, and then subjected to magnetic stirring for 30 minutes, and then 0.5 parts of an organic silicon compound (1H, 1H, 2H, 2H-perfluorodecyltriethoxysilane) and 0.3 parts of γ-aminopropyltriethoxysilane were added thereto, stirred at 45°C, reacted for 30 minutes, centrifuged to remove the solvent, and then dried at 45°C for 6 hours to obtain hydrophobically modified aerogel particles;

[0109] (3) Preparation of hydrophobically modified aerogel composite epoxy resin water-insulating thermal coating:

[0110] 1) Using water as a solvent, add 1 part of a film-forming aid (propylene glycol) and 0.5 parts of a cellulose mixed ether (hydroxypropyl methylcellulose) to 10 parts of water, stir with a stirrer for 2 hours, and adjust the pH to between 9 and 10 with a buffer solution to make it a transparent solution;

[0111] 2) Add 0.4 parts of dispersant (sodium polyacrylate) to the obtained transparent solution, add 10 parts of hydrophobically modified SiO2 aerogel after stirring evenly, add 1.2 parts of aqueous emulsion (acrylic emulsion) under low-speed stirring, add 1 part of epoxy resin polymer, stir evenly with a stirrer, and add 20 parts of lime powder and 0.5 parts of wood fiber evenly at a low speed, add 0.2 parts of thickener (gas-phase SiO2) after stirring evenly, and adjust the consistency to an appropriate range to obtain a hydrophobically modified aerogel-composite epoxy resin anti-corrosion and water-insulating coating.

[0112] (4) Mix 1 part of the hydrophobically modified aerogel-composite epoxy resin anticorrosive and heat-insulating water-soluble coating obtained in step (3) with 0.4 parts of 4.4'-diaminodiphenylmethane and spray it on the surface of the substrate, dry it at 120°C for 30 minutes, and cure it at 80°C for 6 hours to obtain a hydrophobically modified aerogel composite epoxy resin coating. The performance indicators of the hydrophobically modified aerogel composite epoxy resin coating in this embodiment were tested, and the results are shown in Table 5 below:

[0113] Table 5

[0114]

[0115] Example 6

[0116] A method for preparing a hydrophobically modified aerogel composite epoxy resin water-insulating thermal coating comprises the following steps:

[0117] (1) Preparation of epoxy resin polymer:

[0118] First, 2.0 parts of silane coupling agent and 1 part of deionized water were mixed and dissolved in 5.0 parts of anhydrous ethanol, 1 mol / L NaOH solution was added to adjust the pH to 10, 1.0 part of fatty alcohol (polydimethylsiloxane) was added after mixing and stirring, and ultrasonic dispersion was performed for 10 minutes, followed by magnetic stirring at 70°C to ensure sufficient contact and reaction, and the stirring reaction was continued for 1 hour; finally, 2.0 parts of epoxy resin were added at 45°C, and magnetic stirring was performed at a stirring rate of 200 r / min for 8 hours to obtain an epoxy resin polymer;

[0119] (2) Preparation of hydrophobically modified aerogel particles:

[0120] 1.0 part of aerogel particles with an average diameter of 100 μm was dispersed in 5 parts of anhydrous ethanol, subjected to ultrasound at room temperature for 30 minutes, and then subjected to magnetic stirring for 30 minutes, and then 0.5 parts of an organic silicon compound (1H, 1H, 2H, 2H-perfluorooctyl triethoxysilane) and 0.3 parts of γ-aminopropyl triethoxysilane were added thereto, stirred at 45°C, reacted for 30 minutes, centrifuged to remove the solvent, and then dried at 45°C for 6 hours to obtain hydrophobically modified aerogel particles;

[0121] (3) Preparation of hydrophobically modified aerogel composite epoxy resin water-insulating thermal coating:

[0122] 1) Using water as a solvent, add 1 part of a film-forming aid (propylene glycol) and 0.5 parts of a cellulose mixed ether (hydroxyethyl methyl cellulose) to 10 parts of water, stir with a stirrer for 2 hours, and adjust the pH to between 9 and 10 with a buffer solution to make it a transparent solution;

[0123] 2) Add 0.4 parts of dispersant (ammonium polyacrylate) to the obtained transparent solution, add 10 parts of hydrophobically modified SiO2 aerogel after stirring evenly, add 1.2 parts of aqueous emulsion (styrene acrylic emulsion) under low-speed stirring, add 1 part of epoxy resin polymer, stir evenly with a stirrer, and add 20 parts of lime powder and 0.5 parts of wood fiber evenly at a low speed, add 0.2 parts of thickener (diatomaceous earth) after stirring evenly, and adjust the consistency to an appropriate range to obtain a hydrophobically modified aerogel-composite epoxy resin anticorrosive water-insulating coating.

[0124] (4) Mix 1 part of the hydrophobically modified aerogel-composite epoxy resin anticorrosive and water-insulating water-soluble coating obtained in step (3) with 0.4 parts of 4.4'-diaminodiphenylmethane and spray it on the surface of the substrate, dry it at 120°C for 30 minutes, and cure it at 80°C for 6 hours to obtain a hydrophobically modified aerogel composite epoxy resin coating. The performance indicators of the hydrophobically modified aerogel composite epoxy resin coating in this embodiment were tested, and the results are shown in Table 6 below:

[0125] Table 6

[0126]

[0127] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.

Claims

1. A hydrophobically modified aerogel composite epoxy resin water-insulating paint, characterized in that: The invention comprises the following raw materials in parts by weight: 10 parts of water, 1 part of film-forming aid, 0.5 parts of cellulose mixed ether, 0.2-0.4 parts of dispersant, 5-10 parts of hydrophobically modified aerogel particles, 1.2 parts of aqueous emulsion, 1 part of epoxy resin polymer, 15-20 parts of filler and 0.5-0.7 parts of wood fiber; The preparation of the epoxy resin polymer comprises the following steps: After mixing the silane coupling agent, water and anhydrous ethanol, adjusting the pH, adding the silicone resin, dispersing by ultrasonication and stirring to react, then adding the epoxy resin, stirring and reacting again, to obtain the epoxy resin polymer; The organic silicon resin is one of dimethylphenylsilane, polydimethylsiloxane, polymethyltriethoxysilane and polymethyldiethoxysilane; The film-forming aid includes one of propylene glycol, alcohol ester dodecanol and hexadecanol ester; The filler is calcium carbonate; The preparation of the hydrophobically modified aerogel particles comprises the following steps: adding an organosilicon compound and a silane coupling agent to an aerogel ethanol dispersion, stirring and reacting the mixture, and then centrifugally drying the mixture to obtain the hydrophobically modified aerogel particles; The aerogel particles have an average particle size of 100 μm and include one or any combination of silicon dioxide aerogel particles, titanium dioxide aerogel particles, copper oxide aerogel particles, zirconium dioxide aerogel particles and aluminum oxide aerogel particles; The organosilicon compound includes one of 1H,1H,2H,2H-perfluorodecyltriethoxysilane, 1H,1H,2H,2H-perfluorooctyltrimethylsiloxane and 1H,1H,2H,2H-perfluorooctyltriethoxysilane.

2. The hydrophobically modified aerogel composite epoxy resin water-insulating paint according to claim 1, characterized in that: The mass ratio of the silane coupling agent, water, anhydrous ethanol, silicone resin and epoxy resin is 2:1:5:1:(1.5-2.0); The pH is adjusted to 10 using NaOH with a concentration of 1 mol / L, and after the pH is adjusted, stirring is performed at 70° C. and 200 r / min for 1 hour; The ultrasonic temperature is room temperature, and the ultrasonic time is 10 min; The stirring reaction time is 1h; The epoxy resin is added at 40° C. and 200 r / min; The stirring reaction time is 8 hours.

3. The hydrophobically modified aerogel composite epoxy resin water-insulating paint according to claim 1, characterized in that: The silane coupling agent includes one of γ-(2,3-epoxypropoxy)propyltrimethoxysilane, γ-aminopropyltriethoxysilane, vinyltriethoxysilane and methacryloxypropyltrimethylsilane.

4. The hydrophobically modified aerogel composite epoxy resin water-insulating paint according to claim 1, characterized in that: In the aerogel ethanol dispersion, the mass ratio of aerogel particles to anhydrous ethanol is 1:5; The mass ratio of the aerogel particles, the organosilicon compound and the silane coupling agent is 1:0.5:0.3; The stirring reaction temperature is 45° C. After reacting for 30 minutes, the solvent is removed by centrifugation, and then dried at 45° C. for 6 hours.

5. The hydrophobically modified aerogel composite epoxy resin water-insulating paint according to claim 1, characterized in that: The cellulose mixed ether includes one of hydroxyethyl carboxymethyl cellulose, hydroxypropyl methyl cellulose and hydroxyethyl methyl cellulose; The dispersant includes one of ammonium polycarboxylate, ammonium polyacrylate, sodium polyacrylate and potassium polyacrylate; The aqueous emulsion includes styrene acrylic emulsion and / or acrylic emulsion; The thickener includes one of diatomaceous earth, fumed silica and sodium bentonite.

6. A method for preparing a hydrophobically modified aerogel composite epoxy resin water-insulating coating according to any one of claims 1 to 5, characterized in that: The following steps are involved: (1) mixing water, a film-forming aid and a cellulose mixed ether and stirring, adjusting the pH, and then sequentially adding a dispersant, hydrophobically modified aerogel particles and an aqueous emulsion to obtain a mixed dispersion; (2) Adding epoxy resin polymer, filler and wood fiber to the mixed dispersion in sequence to obtain the hydrophobically modified aerogel composite epoxy resin water-insulating paint.

7. The method for preparing a hydrophobically modified aerogel composite epoxy resin water-insulating coating according to claim 6, characterized in that: The mixing time in step (1) is 2 hours; The pH is adjusted to between 9 and 10 using a buffer solution.