Aerated concrete board cured by cement kiln tail gas and preparation method thereof

By using high-calcium oxide-belite-calcium sulfoaluminate cementitious materials and desulfurization and denitrification cement kiln tail flue gas curing technology, the cracking problem and high energy consumption and high emission problem of aerated concrete panels have been solved, achieving the effect of efficient utilization of flue gas heat and reduction of CO2 emissions.

CN116813371BActive Publication Date: 2024-11-05JIAHUA SPECIAL CEMENT
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210948489.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-09
Publication Date
2024-11-05
Estimated Expiration
2042-08-09

AI Technical Summary

Technical Problem

Existing aerated concrete panels suffer from cracking issues due to the difference in linear expansion coefficients between reinforcing steel and aerated concrete during the production process, as well as high energy consumption and high CO2 emissions.

Method used

By using high-calcium oxide-belite-calcium sulfoaluminate cementitious materials and desulfurized and denitrified cement kiln tail flue gas curing technology, combined with steel reinforcement corrosion inhibitors, the bonding strength is improved through hydration-heat sealing-carbonization reaction and the heat of flue gas is utilized to reduce CO2 emissions.

Benefits of technology

It reduces the difference in linear expansion coefficients between steel bars and aerated concrete, increases bonding strength, reduces CO2 emissions from cement plants, and effectively utilizes flue gas heat to meet strength and density requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116813371B_ABST
    Figure CN116813371B_ABST
Patent Text Reader

Abstract

The present invention discloses an aerated concrete board cured by cement kiln tail flue gas and a preparation method, which belongs to the technical field of concrete materials. The board is made of steel bars as a skeleton, and after the aerated concrete slurry is cast to form, it is cured by the cement kiln tail flue gas after desulfurization and denitrification, wherein the raw materials of aerated concrete include dry materials, water, and aluminum powder paste; the dry materials include high calcium oxide-belite-calcium sulfoaluminate cementitious material, fly ash and dihydrate gypsum. The present invention uses high calcium oxide-belite-calcium sulfoaluminate cementitious material to prepare aerated concrete boards and steel bar preservatives, which not only reduces the difference in linear expansion coefficients between steel bars and aerated concrete, but also increases the bonding strength between aerated concrete and steel bars. In addition, using the cement kiln tail flue gas after desulfurization and denitrification to cure the aerated concrete board not only effectively utilizes the heat in the flue gas, but also reduces the CO 2 Emissions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of concrete materials, and in particular relates to an aerated concrete plate cured by cement kiln tail flue gas and a preparation method thereof. Background Art

[0002] Aerated concrete can be made into various types of products to meet the needs of different parts of the building. When steel bars are configured in aerated concrete, it can be made into panels with different functions, mainly roof panels, floor panels, wall panels, patterned decorative panels and assembled wall panels.

[0003] In the production process of aerated concrete boards, cracks of varying degrees will appear in the finished boards. In the range of 20-200℃, the linear expansion coefficient of steel bars is 12×10 -3 mm·m -1 ℃ -1 The linear expansion coefficient of aerated concrete is 8×10 -3 mm·m -1 ℃ -1 For example, a 3m long plate is heated from 60℃ to 185℃ during curing. The length of the steel bar inside it is extended by 4.5mm, while the length of the aerated concrete is extended by 3mm. The difference in expansion between the two is 1.5mm. This is obviously one of the reasons for the cracks in the plate. In order to reduce the difference in linear expansion coefficient between steel bars and aerated concrete, the patent publication number is CN103693928B, and the patent name is a kind of autoclaved aerated concrete board prepared by using Yellow River sand and its preparation method. Magnesia (main component is MgO) is added to the aerated concrete board. The addition of magnesia can increase the thermal expansion coefficient of aerated concrete, and make it as consistent as possible with the thermal expansion coefficient of steel bars during steam curing. The plate prepared by this patent has high compressive strength, high rigidity and small deflection value. However, the calcination range of magnesite is 800~1100℃. The magnesite calcined at low temperature (800~900℃) has a fast digestion speed and does not expand during the autoclave process. Only the magnesite calcined at high temperature (1000℃~1100℃) has a digestion time of more than 8h after encountering water. During the autoclave process, the magnesite is hydrated to generate Mg(OH) 2 The expansion coefficient of aerated concrete board can only be increased by volume expansion. The patent does not describe the hydration time and calcination temperature of magnesia.

[0004] In addition, whether the steel bar can play a force-bearing role in the plate depends on the bonding force of aerated concrete to the steel bar, and the bonding force between the steel bar and concrete comes from the anti-corrosion coating. Due to the different compositions and properties of various preservatives, the bonding force is also different. In order to strengthen the bonding force between aerated concrete and steel bars, the patent publication number is CN108003708B, and the patent name is a rust inhibitor and preparation method for steel bars in autoclaved sand aerated concrete plates. The invention uses carboxylated styrene butadiene latex, red iron oxide, slaked lime, high-efficiency thickener, quartz sand, sand aerated concrete plate waste, and tap water to make a rust inhibitor to increase the bonding force between steel bars and concrete. However, carboxylated styrene butadiene latex is easy to fail and needs to be stored away from light, which is inconvenient to use.

[0005] In addition, autoclaving is the main method for aerated concrete to achieve hydrothermal synthesis and obtain strength. 6 ~1.6×10 6 kJ / m 3 The heat consumption of aerated concrete curing is high, and it is a high-energy-consuming product. The temperature of the flue gas at the end of the cement kiln is higher than 300°C. The flue gas at the end of the kiln after desulfurization and denitrification can generally be used for waste heat power generation and then discharged into the air. However, the exhaust gas is rich in CO 2 , polluting the air.

[0006] Therefore, the present invention provides an aerated concrete board cured by cement kiln tail flue gas and a preparation method thereof, and uses high calcium oxide-belite-calcium sulfoaluminate cementitious material to prepare aerated concrete boards and steel bar preservatives, which not only reduces the difference in linear expansion coefficients between steel bars and aerated concrete, but also increases the bonding strength between aerated concrete and steel bars. In addition, the use of aerated concrete boards cured by desulfurized and denitrified cement kiln tail flue gas not only effectively utilizes the heat in the flue gas, but also reduces the CO 2 Emissions. Summary of the invention

[0007] The technical problem to be solved by the present invention is to provide an aerated concrete board cured by cement kiln tail flue gas and a preparation method thereof, so as to at least solve part of the above technical problems.

[0008] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0009] An aerated concrete board cured by cement kiln tail flue gas, wherein the board is made of steel bars as a skeleton, cast with aerated concrete materials and then cured by cement kiln tail flue gas after desulfurization and denitrification, wherein the raw materials of aerated concrete include dry materials, water and aluminum powder paste;

[0010] The dry material comprises 28-40 wt.% of high calcium oxide-belite-calcium sulfoaluminate cementitious material, 54-68 wt.% of fly ash and 4-6 wt.% of dihydrate gypsum;

[0011] The aluminum powder paste dosage is 0.8‰ to 1.2‰ of the total dry material;

[0012] The amount of water used is determined by the slurry fluidity of 240±10mm.

[0013] Furthermore, the high calcium oxide-belite-calcium sulfoaluminate gelling material comprises the following components in percentage by mass:

[0014] f-CaO: 24-40wt.%;

[0015] C 2 S: 30-55wt.%;

[0016] 1~20wt.%;

[0017] C 4 AF: 0.1~10wt.%;

[0018] CaSO 4 :0.1~10wt.%.

[0019] Furthermore, the high calcium oxide-belite-calcium sulfoaluminate cementitious material is calcined at high temperature by calcium material, silicon material, aluminum material and gypsum material, the calcination temperature is 1150-1300° C., and the calcination time is 20-90 minutes.

[0020] Furthermore, the surface of the steel bar is coated with a steel bar antiseptic.

[0021] Furthermore, the steel bar preservative is prepared by mixing asphalt, high calcium oxide-belite-calcium sulfoaluminate cementitious material, fly ash, sodium methyl siliconate and water in a mass ratio of 3:1:1.4:0.02:3.

[0022] A method for preparing an aerated concrete plate using cement kiln tail flue gas curing comprises the following steps:

[0023] Step 1, coating the steel bar with a steel bar preservative, drying and assembling the steel bar into a mold, wherein the thickness of the steel bar preservative coating is 0.7 mm to 1 mm;

[0024] Step 2, weighing the raw materials of aerated concrete according to the proportions;

[0025] Step 3: Add the weighed raw materials into a mixer and mix them into a uniform material, then pour them into a mold and vibrate them;

[0026] Step 4, placing the slurry after pouring and vibrating in a hot and humid environment to stop, so as to obtain a gas-generated and hardened green body;

[0027] Step 5: dividing and trimming the hardened green body to obtain a concrete slab;

[0028] Step 6: Maintain the concrete slab.

[0029] Furthermore, in step 3, the weighed raw materials are added into a mixer and stirred into a uniform material with a fluidity of 220 to 240 mm, and then poured into a mold and vibrated for 20 seconds using an inserted vibrator;

[0030] In the step 4, the slurry after pouring and vibration is placed in a humid and hot environment of 40 to 60° C. and allowed to stand for 2 to 3 hours to obtain a gas-generated and hardened green body.

[0031] Furthermore, the step 6 comprises:

[0032] Step 61, placing the concrete slab in an autoclave and evacuating the air;

[0033] Step 62, passing the high-temperature kiln tail flue gas into a heat exchanger to prepare saturated water vapor, and slowly passing the saturated water vapor into the autoclave to increase the temperature of the autoclave;

[0034] Step 63, intermittently introduce saturated water vapor into the autoclave to maintain the temperature of the autoclave, introduce the kiln tail flue gas after heat exchange in the heat exchanger into the autoclave, open the micro-open exhaust valve on the autoclave to make the gas in the autoclave flow while ensuring the working pressure of the autoclave;

[0035] Step 64, quickly exhaust and cool down, and take out to obtain the aerated concrete board.

[0036] Furthermore, in step 62, high-temperature kiln tail flue gas is introduced into a heat exchanger to prepare saturated water vapor above 180° C.;

[0037] In step 63, saturated water vapor is intermittently introduced into the autoclave to maintain the temperature of the autoclave at 180-190° C., kiln tail flue gas after heat exchange in the boiler heat exchanger is introduced into the autoclave, and the micro-opening exhaust valve on the autoclave is opened to allow the gas in the autoclave to flow while ensuring that the working pressure of the autoclave is 1.5-1.7 MPa. The duration is 7-9 hours, and the temperature of the high-temperature kiln tail flue gas after heat exchange in the heat exchanger is 70-120° C.

[0038] Furthermore, the high-temperature kiln tail flue gas is subjected to desulfurization and denitrification treatment, and the CO in the kiln tail flue gas after desulfurization and denitrification is 2 The volume concentration is 5-20%.

[0039] The amount of steel bars used in the present invention is based on the prior art, and the amount is determined according to the properties of the plate to be made.

[0040] Compared with the prior art, the present invention has the following beneficial effects:

[0041] The invention is scientifically and reasonably designed and convenient to use. It uses high calcium oxide-belite-calcium sulfoaluminate cementitious materials to prepare aerated concrete plates and steel bar preservatives, which not only reduces the difference in linear expansion coefficients between steel bars and aerated concrete, but also increases the bonding strength between aerated concrete and steel bars. In addition, the use of aerated concrete plates cured by desulfurized and denitrified cement kiln tail flue gas not only effectively utilizes the heat in the flue gas, but also reduces the CO2 emissions from cement plants. 2 Emissions. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 This is an X-ray diffraction diagram of the aerated concrete board of the present invention after being cured by kiln tail flue gas.

[0043] Figure 2 This is a morphology diagram of lime particles in the high calcium oxide-belite-calcium sulfoaluminate cementitious material of the present invention. DETAILED DESCRIPTION

[0044] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0045] The present invention uses desulfurization and denitrification kiln tail flue gas to cure aerated concrete panels. The mechanism is as follows: During the entire curing process, each slurry in the panel undergoes a hydration-heat bonding-carbonization ternary reaction. First, in the static stage, the slurry poured into the mold undergoes a gasification, thickening, initial setting, and hardening process. In this series of processes, the high calcium oxide-belite-calcium sulfoaluminate cementitious material undergoes a hydration reaction to generate Ca(OH) 2 , AFt, CSH gel and other hydration products, the products overlap each other, promoting the hardening of the body; secondly, in the initial stage of heat preservation and smoke ventilation, the inside and outside of the concrete undergo heat sealing and carbonization reactions at the same time: on the outside of the aerated concrete body, the hydration product Ca(OH) 2 , AFt, CSH and f-CaO, C 2 S.C. 4 AF and CO in kiln tail flue gas 2 Reaction, the generated CaCO 3 Crystals, silica gel and aluminum glue fill microscopic pores to improve the strength of aerated concrete; while the concrete body undergoes a heat-sealing reaction, Ca(OH) 2, CSH gel and SiO in siliceous materials 2 、Al 2 O 3 The reaction generates tobermorite, aluminum-substituted tobermorite and water garnet, which improves the internal strength of the blank. The high-temperature kiln tail flue gas is desulfurized and denitrified to prevent SO in the flue gas. 2 and NO X The invention solves the problem of heat recovery in the flue gas at the end of cement kiln and CO in the flue gas. 2 Gas solidification problem.

[0046] The present invention uses high calcium oxide-belite-calcium sulfoaluminate cementitious material as the main raw material of aerated concrete and steel bar preservative, without the need to add additional magnesia, which reduces the difference in thermal expansion value between the aerated concrete body and the steel bar during the steam curing and heating process, and solves the problem of vertical cracks in the plate. The reason is that the high calcium oxide-belite-calcium sulfoaluminate cementitious material is f-CaO-C 2 SC 4 A 3 Gypsum system, calcination temperature is 1150℃~1300℃, a small part of f-CaO is overburned (such as attached Figure 2 As shown in Figure 2, under high temperature and high pressure conditions, overburned f-CaO reacts with water to form calcium hydroxide, which causes the volume of aerated concrete to expand. In addition, the C 4 A 3 、CaSO 4 With hydration product Ca(OH) 2 AFt is generated by dissolution and crystallization, which causes the volume of the green body to expand.

[0047] The invention adopts asphalt, high calcium oxide-belite-calcium sulfoaluminate cementitious material, fly ash and sodium methyl siliconate to prepare a steel bar preservative. Under high temperature and high pressure conditions, the high calcium oxide-belite-calcium sulfoaluminate cementitious material in the steel bar preservative generates tobermorite and hydrogarnet and other products inside, which are consistent with the main products of aerated concrete, and can not only increase the bonding force between aerated concrete and steel bars, but also its hydration products can be organically fused with asphalt, forming a skeleton composed of crystal intergrowths in asphalt, so that the strength of the outer coating of the steel bar is higher.

[0048] The reinforcement calculation of the steel bars described in the present invention is a prior art, and the reinforcement structure is determined after internal force calculation based on the load on the plate, without determining the mass ratio of the material and the steel bars.

[0049] Figure 1This is an X-ray diffraction diagram of the aerated concrete board of the present invention after being cured with kiln tail flue gas. After the aerated concrete board is cured with kiln tail flue gas, a carbonization reaction occurs on the outside, and the products mainly include aragonite, limestone, anhydrite, etc.; a hydrothermal synthesis reaction occurs on the inside, and the products mainly include tobermorite and hydrogarnet. Figure 2 This is a morphology diagram of lime particles in the high calcium oxide-belite-calcium sulfoaluminate cementitious material of the present invention. It can be seen that there is crystallization on the surface of the free calcium particles, indicating that the calcium oxide is slightly overburned.

[0050] Example 1

[0051] An aerated concrete board cured by cement kiln tail flue gas, wherein the board is made of steel bars as a skeleton, cast with aerated concrete materials and then cured by cement kiln tail flue gas after desulfurization and denitrification, wherein the raw materials of aerated concrete include dry materials, water and aluminum powder paste;

[0052] The dry materials include 40wt.% of high calcium oxide-belite-calcium sulfoaluminate cementitious material, 54wt.% of fly ash and 6wt.% of dihydrate gypsum; the aluminum powder paste content is 1.2‰ of the total dry material; the slurry fluidity of this embodiment is 240mm, and the water consumption is 50% of the total dry material.

[0053] In this embodiment, the high calcium oxide-belite-calcium sulfoaluminate cementitious material includes the following components in percentage by mass: f-CaO: 38wt.%, C 2 S: 50wt.%, C 4 A 3 :8wt.%、C 4 AF: 2wt.%, CaSO 4 :2wt.%; the high calcium oxide-belite-calcium sulfoaluminate cementitious material is formed by high-temperature calcination of calcium material, silicon material, aluminum material and gypsum material, the calcination temperature is 1300℃, and the calcination time is 30min; the surface of the steel bar is coated with a steel bar preservative; the steel bar preservative is composed of asphalt, high calcium oxide-belite-calcium sulfoaluminate cementitious material, fly ash, sodium methyl siliconate and water in a mass ratio of 3:1:1.4:0.02:3.

[0054] The method for preparing an aerated concrete board comprises the following steps:

[0055] Step 1: According to the requirements of the reinforcement structure, apply a 1mm thick steel bar preservative on the surface of the steel bar, dry it and assemble it into the mold, and weld three transverse bars at both ends of the tensile steel bar as anchor bars;

[0056] Step 2, weighing the raw materials of aerated concrete according to the proportions;

[0057] Step 3, add the weighed raw materials into a mixer and stir them into a uniform material with a fluidity of 240 mm, then pour them into the mold and vibrate them for 20 seconds using an inserted vibrator;

[0058] Step 4, placing the poured and vibrated slurry in a 60° C. hot and humid environment for 3 hours to obtain a gas-generated and hardened green body;

[0059] Step 5: dividing and trimming the hardened green body to obtain a concrete slab;

[0060] Step 6: Maintain the concrete slab.

[0061] The step 6 comprises: step 61, placing the concrete slab in an autoclave and evacuating the slab; step 62, introducing the high-temperature kiln tail flue gas after desulfurization and denitrification into a heat exchanger to prepare saturated water vapor above 180°C, slowly introducing the saturated water vapor into the autoclave to raise the temperature to above 180°C in 2.5 hours; step 63, intermittently introducing saturated water vapor into the autoclave to maintain the temperature of the autoclave at 190°C, introducing the kiln tail flue gas at 120°C after heat exchange in the heat exchanger into the autoclave, opening the micro-opening exhaust valve on the autoclave to allow the gas in the autoclave to flow while ensuring that the working pressure of the autoclave is 1.7MPa, and the duration is 9 hours; step 64, rapidly exhausting the air and cooling it down, taking it out to obtain the aerated concrete slab.

[0062] The high-temperature kiln tail flue gas is treated with desulfurization and denitrification, and the CO in the kiln tail flue gas after desulfurization and denitrification is 2 The concentration is 5%.

[0063] Example 2

[0064] An aerated concrete board cured by cement kiln tail flue gas, wherein the board is made of steel bars as a skeleton, cast with aerated concrete materials and then cured by cement kiln tail flue gas after desulfurization and denitrification, wherein the raw materials of aerated concrete include dry materials, water and aluminum powder paste;

[0065] The dry materials include 28wt.% of high calcium oxide-belite-calcium sulfoaluminate cementitious material, 68wt.% of fly ash and 4wt.% of dihydrate gypsum; the aluminum powder paste content is 0.8‰ of the total dry material; the slurry fluidity of this embodiment is 248mm, and the water consumption is 48% of the total dry material.

[0066] In this embodiment, the high calcium oxide-belite-calcium sulfoaluminate cementitious material includes the following components in percentage by mass: f-CaO: 34wt.%, C 2 S: 43wt.%, C 4 A 3 :10wt.%、C 4 AF: 7wt.%, CaSO 4: 6wt.%; the high calcium oxide-belite-calcium sulfoaluminate cementitious material is formed by high-temperature calcination of calcium material, silicon material, aluminum material and gypsum material, the calcination temperature is 1150°C, and the calcination time is 90min; the surface of the steel bar is coated with a steel bar preservative; the steel bar preservative is composed of asphalt, high calcium oxide-belite-calcium sulfoaluminate cementitious material, fly ash, sodium methyl siliconate and water in a mass ratio of 3:1:1.4:0.02:3.

[0067] The method for preparing an aerated concrete board comprises the following steps:

[0068] Step 1: According to the requirements of the reinforcement structure, apply 0.7mm thick steel bar preservative on the surface of the steel bar, dry and assemble it into the mold, and weld three transverse bars at both ends of the tensile steel bar as anchor bars;

[0069] Step 2, weighing the raw materials of aerated concrete according to the proportions;

[0070] Step 3, add the weighed raw materials into a mixer and stir them into a uniform material with a fluidity of 248 mm, then pour them into the mold and vibrate them for 20 seconds using an inserted vibrator;

[0071] Step 4, placing the poured and vibrated slurry in a 50°C hot and humid environment for 3 hours to obtain a gas-generated and hardened green body;

[0072] Step 5: dividing and trimming the hardened green body to obtain a concrete slab;

[0073] Step 6: Maintain the concrete slab.

[0074] The step 6 comprises: step 61, placing the concrete slab in an autoclave and evacuating the slab; step 62, introducing the high-temperature kiln tail flue gas after desulfurization and denitrification into a heat exchanger to prepare saturated water vapor above 180°C, slowly introducing the saturated water vapor into the autoclave to raise the temperature to above 180°C in 2 hours; step 63, intermittently introducing saturated water vapor into the autoclave to maintain the temperature of the autoclave at 185°C, introducing the kiln tail flue gas at 70°C after heat exchange in the heat exchanger into the autoclave, opening the micro-opening exhaust valve on the autoclave to allow the gas in the autoclave to flow while ensuring that the working pressure of the autoclave is 1.5MPa, and the duration is 8 hours; step 64, quickly exhausting the air and cooling it down, taking it out to obtain the aerated concrete slab.

[0075] The high-temperature kiln tail flue gas is treated with desulfurization and denitrification, and the CO in the kiln tail flue gas after desulfurization and denitrification is 2 The concentration is 20%.

[0076] Example 3

[0077] An aerated concrete board cured by cement kiln tail flue gas, wherein the board is made of steel bars as a skeleton, cast with aerated concrete materials and then cured by cement kiln tail flue gas after desulfurization and denitrification, wherein the raw materials of aerated concrete include dry materials, water and aluminum powder paste;

[0078] The dry materials include 34wt.% of high calcium oxide-belite-calcium sulfoaluminate cementitious material, 61wt.% of fly ash and 5wt.% of dihydrate gypsum; the aluminum powder paste content is 1‰ of the total dry material; the slurry fluidity of this embodiment is 235mm, and the water consumption is 43% of the total dry material.

[0079] In this embodiment, the high calcium oxide-belite-calcium sulfoaluminate cementitious material includes the following components in percentage by mass: f-CaO: 34wt.%, C 2 S: 46wt.%, C 4 A 3 :13wt.%、C 4 AF: 5wt.%, CaSO 4 :2wt.%; the high calcium oxide-belite-calcium sulfoaluminate cementitious material is formed by high-temperature calcination of calcium material, silicon material, aluminum material and gypsum material, the calcination temperature is 1300℃, and the calcination time is 20min; the surface of the steel bar is coated with a steel bar preservative; the steel bar preservative is composed of asphalt, high calcium oxide-belite-calcium sulfoaluminate cementitious material, fly ash, sodium methylsiliconate and water in a mass ratio of 3:1:1.4:0.02:3.

[0080] The method for preparing an aerated concrete board comprises the following steps:

[0081] Step 1: According to the requirements of the reinforcement structure, apply 0.8mm thick steel bar preservative on the surface of the steel bar, dry and assemble it into the mold, and weld three transverse bars at both ends of the tensile steel bar as anchor bars;

[0082] Step 2, weighing the raw materials of aerated concrete according to the proportions;

[0083] Step 3, add the weighed raw materials into a mixer and stir them into a uniform material with a fluidity of 235 mm, then pour them into the mold and vibrate them for 20 seconds using an inserted vibrator;

[0084] Step 4, placing the poured and vibrated slurry in a 40°C hot and humid environment for 3 hours to obtain a gas-generated and hardened green body;

[0085] Step 5: dividing and trimming the hardened green body to obtain a concrete slab;

[0086] Step 6: Maintain the concrete slab.

[0087] The step 6 comprises: step 61, placing the concrete slab in an autoclave and evacuating the slab; step 62, introducing the high-temperature kiln tail flue gas after desulfurization and denitrification into a heat exchanger to prepare saturated water vapor above 180°C, slowly introducing the saturated water vapor into the autoclave to raise the temperature to above 180°C in 2 hours; step 63, intermittently introducing saturated water vapor into the autoclave to maintain the temperature of the autoclave at 180°C, introducing the kiln tail flue gas at 90°C after heat exchange in the heat exchanger into the autoclave, opening the micro-opening exhaust valve on the autoclave to allow the gas in the autoclave to flow while ensuring that the working pressure of the autoclave is 1.7MPa, and the duration is 9 hours; step 64, rapidly exhausting the air and cooling it down, taking it out to obtain the aerated concrete slab.

[0088] The high-temperature kiln tail flue gas is treated with desulfurization and denitrification, and the CO in the kiln tail flue gas after desulfurization and denitrification is 2 The concentration is 10%.

[0089] Comparative Example 1

[0090] In this comparative example, the steel bar antiseptic adopts the commercially available wj301 steel bar rust inhibitor, and the other conditions are the same as those in Example 1.

[0091] Comparative Example 2

[0092] In this comparative example, the dry materials include 25wt.% of P.O42.5R cement, 15wt.% of quicklime, 54wt.% of fly ash and 6wt.% of dihydrate gypsum; the dosage of the aluminum paste is 1.2‰ of the total amount of dry materials; in this comparative example, the fluidity of the slurry is 242mm, and the water consumption is 50% of the total amount of dry materials; the surface of the steel bar is coated with a steel bar rust inhibitor, and the steel bar rust inhibitor used is wj301 type steel bar rust inhibitor, and the other conditions are the same as those in Example 1.

[0093] Comparative Example 3

[0094] In this comparative example, the dry materials include 25wt.% of P.O42.5R cement, 15wt.% of quicklime, 54wt.% of fly ash and 6wt.% of dihydrate gypsum; the amount of aluminum paste added is 1.2‰ of the total amount of dry materials; the amount of water used is 50% of the total amount of dry materials. The fluidity of the slurry in this embodiment is 242mm; the rust inhibitor used is wj301 type steel bar rust inhibitor.

[0095] Except for the curing step 6, the other steps of the preparation method are consistent with those of Example 1. In this comparative example, the curing method adopts conventional autoclave curing:

[0096] Step 6 maintenance includes:

[0097] 1. Feeding: Place the aerated concrete body in the autoclave and evacuate it;

[0098] 2. Heating: High-temperature steam is introduced into the autoclave, and the temperature of the autoclave is raised to 185°C and the pressure is 1.2MPa in 2.5h;

[0099] 3. Insulation: Saturated steam is intermittently introduced into the autoclave to maintain the autoclave temperature at 185°C. The insulation process lasts for 8 hours.

[0100] 4. Cooling: Rapid exhaust and cooling, and the aerated concrete board is obtained after taking it out.

[0101] The properties of aerated concrete prepared in Examples 1 to 3 of the present invention and Comparative Examples 1 to 3 are shown in Table 1, and the properties of aerated concrete panels are shown in Table 2:

[0102] Table 1 Physical properties of aerated concrete panels prepared in Examples 1 to 3 and Comparative Examples 1 to 3

[0103]

[0104]

[0105] Table 2 Physical properties of aerated concrete panels prepared in Examples 1 to 3 and Comparative Examples 1 to 3

[0106]

[0107] From the data in Table 1, it can be seen that after the aerated concrete made of high calcium oxide-belite-calcium sulfoaluminate cementitious material is cured by the flue gas from the tail of the desulfurization and denitrification kiln, a ternary reaction of hydration-heat bonding-carbonization occurs, and the strength and bulk density of the aerated concrete meet the requirements of GB / T 15762-2020 "Autoclaved Aerated Concrete Board"; by comparing Comparative Example 1 and Example 1, it is found that the steel bar preservative has basically no effect on the bulk density and strength; by comparing Comparative Example 2 and Example 1, it is found that under the curing conditions of the flue gas from the tail of the desulfurization and denitrification kiln, the aerated concrete prepared with conventional materials P.O42.5R and quicklime has a lower strength and the strength does not meet the requirements of the specification; by comparing Comparative Example 3 and Example 1, it is found that the aerated concrete prepared with conventional materials has a slightly higher strength and a lower bulk density after conventional curing. The reason why the bulk density of Example 1 is higher than that of Comparative Example 3 is that due to the carbon fixation effect, the aerated concrete absorbs CO in the flue gas. 2 , resulting in an increase in bulk density.

[0108] From the data in Table 2, it can be seen that the bonding strength between the steel bar and the aerated concrete in Example 1 is 0.7 MPa higher than that in Comparative Example 1, indicating that in this system, the steel bar preservative prepared by the present invention has a better bonding effect. Comparative Examples 2 and 3 use ordinary cement and quicklime, and use commercially available steel bar preservatives, and the bonding strength is improved compared with Comparative Example 1. In summary, commercially available steel bar preservatives are not suitable for the high calcium oxide-belite-calcium sulfoaluminate system.

[0109] In addition, it was observed that for the 600×200×6000 mm plates, the plates made of high calcium oxide-belite-calcium sulfoaluminate cementitious material had no cracks, while the plates made of ordinary materials had more or less vertical cracks.

[0110] Therefore, the present invention uses high calcium oxide-belite-calcium sulfoaluminate cementitious materials to prepare aerated concrete plates and steel bar preservatives, which not only reduces the difference in linear expansion coefficients between steel bars and aerated concrete, but also increases the bonding strength between aerated concrete and steel bars. In addition, the strength and bulk density of aerated concrete cured by desulfurized and denitrated cement kiln tail flue gas meet the requirements of the specifications, which not only effectively utilizes the heat in the flue gas, but also reduces the CO 2 emissions, truly achieving energy conservation and emission reduction.

[0111] Finally, it should be noted that the above embodiments are only preferred embodiments of the present invention to illustrate the technical solutions of the present invention, rather than limiting them, and certainly not limiting the patent scope of the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions recorded in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. These modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. In other words, any changes or modifications made to the main design concept and spirit of the present invention that have no substantive significance, and the technical problems they solve are still consistent with the present invention, should be included in the protection scope of the present invention. In addition, the direct or indirect application of the technical solutions of the present invention in other related technical fields is also included in the patent protection scope of the present invention.

Claims

1. An aerated concrete board cured by cement kiln tail gas, characterized in that: The plate is made of steel bars as the skeleton, and is cast with aerated concrete slurry and cured with cement kiln tail gas after desulfurization and denitration, wherein the raw materials of aerated concrete include dry materials, water, and aluminum powder paste; The dry material comprises 28-40 wt.% of high calcium oxide-belite-calcium sulfoaluminate cementitious material, 54-68 wt.% of fly ash and 4-6 wt.% of dihydrate gypsum; The aluminum powder paste dosage is 0.8‰~1.2‰ of the total dry material; The amount of water used is determined by the slurry fluidity of 240±10mm; The high calcium oxide-belite-calcium sulfoaluminate cementitious material comprises the following components in percentage by mass: f-CaO: 24~40 wt.%; C2S: 30~55 wt.%; :1~20 wt.%; C4AF: 0.1~10 wt.%; CaSO4: 0.1~10 wt.%; The high calcium oxide-belite-calcium sulfoaluminate cementitious material is prepared by calcining calcium material, silicon material, aluminum material and gypsum material at high temperature, wherein the calcination temperature is 1150-1300° C. and the calcination time is 20-90 minutes.

2. The aerated concrete board cured by cement kiln tail gas according to claim 1, characterized in that: The surface of the steel bar is coated with a steel bar antiseptic.

3. The aerated concrete board cured by cement kiln tail gas according to claim 2, characterized in that: The steel bar antiseptic is prepared from asphalt, high calcium oxide-belite-calcium sulfoaluminate cementitious material, fly ash, sodium methyl siliconate and water in a mass ratio of 3:1:1.4:0.02:

3.

4. A method for preparing an aerated concrete board using cement kiln tail gas curing according to any one of claims 1 to 3, characterized in that: The following steps are involved: Step 1, brushing the steel bar with a steel bar preservative, drying and assembling it into a mold; the steel bar preservative is coated with a thickness of 0.7 mm to 1 mm; Step 2, weighing the raw materials of aerated concrete according to the proportions; Step 3: Add the weighed raw materials into a mixer and mix them into a uniform material, then pour them into a mold and vibrate them; Step 4, placing the slurry after pouring and vibrating in a hot and humid environment to stop, so as to obtain a gas-generated and hardened green body; Step 5: dividing and trimming the hardened green body to obtain a concrete slab; Step 6: Maintain the concrete slab.

5. The method for preparing an aerated concrete board using cement kiln tail gas curing according to claim 4, characterized in that: In the step 3, the weighed raw materials are added into a mixer and stirred into a uniform material with a fluidity of 220-240 mm, and then poured into a mold and vibrated for 20 seconds using an inserted vibrator; In the step 4, the slurry after pouring and vibration is placed in a humid and hot environment of 40-60° C. and allowed to stand for 2-3 hours to obtain a gas-generated and hardened green body.

6. The method for preparing aerated concrete panels using cement kiln tail gas curing according to claim 4, characterized in that: The step 6 comprises: Step 61, placing the concrete slab in an autoclave and evacuating the air; Step 62, passing the high-temperature kiln tail flue gas into a heat exchanger to prepare saturated water vapor, and slowly passing the saturated water vapor into the autoclave to increase the temperature of the autoclave; Step 63, intermittently introduce saturated water vapor into the autoclave to maintain the temperature of the autoclave, introduce the kiln tail flue gas after heat exchange in the heat exchanger into the autoclave, open the micro-open exhaust valve on the autoclave to make the gas in the autoclave flow while ensuring the working pressure of the autoclave; Step 64, quickly exhaust and cool down, and take out to obtain the aerated concrete board.

7. The method for preparing an aerated concrete board using cement kiln tail gas curing according to claim 6, characterized in that: In step 62, high-temperature kiln tail flue gas is introduced into a heat exchanger to prepare saturated water vapor above 180° C.; In step 63, saturated water vapor is intermittently introduced into the autoclave to maintain the temperature of the autoclave at 180-190° C., kiln tail flue gas after heat exchange in the boiler heat exchanger is introduced into the autoclave, and the micro-opening exhaust valve on the autoclave is opened to allow the gas in the autoclave to flow while ensuring that the working pressure of the autoclave is 1.5-1.7 MPa. The duration is 7-9 hours, and the temperature of the high-temperature kiln tail flue gas after heat exchange in the heat exchanger is 70-120° C.

8. The preparation method according to claim 7, characterized in that: The high-temperature kiln tail flue gas is treated with desulfurization and denitrification, and the volume concentration of CO2 in the kiln tail flue gas after desulfurization and denitrification is 5~20%.