A method for preparing silicon dioxide-graphite@graphene lithium ion battery negative electrode material

By mixing silicon oxide with graphite and sanding it with graphene oxide solution, silicon oxide-graphite@graphene material is prepared, which solves the problem of volume expansion and insufficient conductivity of the negative electrode material of lithium-ion battery, and achieves high capacity and stability , extends battery life and reduces costs with recycled materials.

CN116825992BActive Publication Date: 2024-11-08KUNMING UNIV OF SCI & TECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310787912.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-30
Publication Date
2024-11-08
Estimated Expiration
2043-06-30

AI Technical Summary

Technical Problem

The existing lithium-ion battery negative electrode materials have poor circulation performance due to volume expansion problems, and the conductivity of silicon oxide is poor, making it difficult to meet the needs of high capacity and stability.

Method used

Silicon oxide-graphite@graphene material is prepared by mixing silicon oxide with graphite and sanding it with graphene oxide solution. The conductivity and toughness of graphene are used to alleviate the volume expansion problem and improve the conductivity of the material. and stability.

Benefits of technology

It has achieved high specific capacity and high first-round Coulomb efficiency, and maintained high capacity after multiple cycles, extending battery life, and recycling materials from silicon solar cells and waste lithium-ion batteries, which is economical and environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116825992B_ABST
    Figure CN116825992B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for preparing a silicon oxide-graphite@graphene lithium ion battery negative electrode material, and relates to the technical field of lithium ion batteries. The present invention firstly mixes silicon oxide and graphite and performs ball milling to obtain a composite powder, and then mixes the composite powder with a graphene oxide solution and performs sand milling to obtain a silicon oxide-graphite@graphene material. The present invention has a simple preparation process, and the prepared composite material has high specific capacity and high first-cycle coulomb efficiency as a negative electrode material for a lithium ion battery, and still has an extremely high specific capacity after multiple cycles, effectively alleviating the volume expansion problem of the battery negative electrode material and ensuring the battery life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a method for preparing a silicon dioxide-graphite@graphene lithium ion battery negative electrode material. Background Art

[0002] With the development of the new energy industry, commercial graphite anode materials have a low theoretical specific capacity (372 mAhg -1 ) can no longer meet the current demand for lithium-ion batteries. Silicon has abundant reserves and a high theoretical specific capacity (4200mAhg -1 ) makes it one of the excellent negative electrode materials. However, silicon itself has a serious volume expansion problem, and pure silicon material is not suitable as a negative electrode material. Silicon dioxide (SiO) is considered to be one of the negative electrode materials with development prospects because of its high specific capacity and suitable working potential, and weaker volume expansion problem compared to silicon. However, SiO has poor conductivity because it is an oxide, and is accompanied by the problem of volume effect.

[0003] Patent CN 106784717 A combines graphite with silicon dioxide to prepare silicon-carbon negative electrode materials. The invention uses graphite and silica sol to mix and pyrolyze to obtain silicon dioxide-coated graphite powder with a maximum discharge capacity of 523 mAh g -1 However, currently, simple coating has a certain limit to suppressing the expansion of silicon materials. After several cycles, the coating layer may slowly fall off due to the expansion problem, which ultimately leads to poor battery cycle performance. Therefore, the nano-sizing of silicon oxide and the ability of carrier materials to alleviate its volume expansion are the key issues of silicon-based negative electrodes. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing a silicon dioxide-graphite@graphene lithium ion battery negative electrode material to solve the problems existing in the above-mentioned prior art, so that the prepared negative electrode material has a high capacity and effectively alleviates the volume expansion problem.

[0005] To achieve the above object, the present invention provides the following solutions:

[0006] One of the technical solutions of the present invention is to provide a method for preparing silicon dioxide-graphite@graphene material, comprising the following steps:

[0007] Step 1, mixing silicon dioxide and graphite and ball milling to obtain composite powder;

[0008] Step 2, mixing the composite powder with the graphene oxide solution in a ratio of 2kg:800-1600mL and then sand-milling to obtain the silicon dioxide-graphite@graphene material;

[0009] The concentration of the graphene oxide solution is 1 g / mL.

[0010] Furthermore, in step 1, the mixing mass ratio of silicon oxide and graphite is 1:4-1:6. After mixing and ball milling, the particle size of the composite powder is 50-70nm and the specific surface area is 20-40m 2 g -1 .

[0011] Furthermore, during the mixed ball milling process in step 1, ball milling is performed in a ratio of 1:10 between the total mass of silicon dioxide and graphite and the mass of the steel balls.

[0012] The sand grinding process in step 2 uses 0.2 mm grinding beads, the sand grinding time is 0.5-2 h, the rotation speed is 1000-2800 rpm, and the gap of the separator is 0.1-0.12 mm.

[0013] Rotation speed is an important parameter of sand grinding. High rotation speed is more conducive to reducing the particle size and is more conducive to graphite covering silicon oxide.

[0014] The second technical solution of the present invention is to provide silicon dioxide-graphite@graphene material prepared by the above preparation method.

[0015] The third technical solution of the present invention is to provide the application of the above silicon dioxide-graphite@graphene material in the negative electrode material of lithium-ion batteries.

[0016] The silicon oxide and graphite material of the invention are respectively recovered from silicon solar cell waste and waste lithium ion battery and are calcined at 600-800°C.

[0017] Specifically, the silicon oxide-graphite@graphene material, conductive carbon (Super P), carboxymethyl cellulose (CMC), and styrene-butadiene rubber (SBR) are placed in a 1000 mL beater tank at a mass ratio of 90:5:2.5:2.5, the rotation speed is 1000 rpm, and the mixture is stirred for 1 hour to finally obtain an electrode slurry; the battery slurry is coated on a copper foil current collector at a thickness of 100 microns, placed in a vacuum oven at 60°C, and dried for 12 hours to remove the solvent to obtain an electrode sheet.

[0018] The present invention discloses the following technical effects:

[0019] 1. The present invention reduces the particle size of silicon oxide-graphite by a simple sand grinding method. The reduction of the particle size alleviates the volume expansion effect of silicon oxide during the cycle and improves the first-cycle coulomb efficiency. At the same time, the fusion of graphite and silicon oxide can prevent the volume expansion from causing the pulverization of the electrode, thereby further improving the life of the battery.

[0020] 2. In order to further improve the conductivity of silicon oxide, the introduction of highly conductive, multifunctional graphene oxide as its substrate helps to improve the conductivity of the material. At the same time, due to its excellent toughness, graphene can secondary alleviate the volume change of silicon oxide, making the battery have excellent stability.

[0021] 3. The composite material prepared by the present invention is used as a negative electrode material for lithium-ion batteries, has high specific capacity and high first-cycle coulombic efficiency, and still has extremely high specific capacity after multiple cycles.

[0022] 4. The silicon oxide and graphite material used in the present invention can be recovered from silicon solar cell waste and waste lithium ion batteries respectively, which has significant economic significance. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0024] Figure 1 This is a scanning electron microscope image of silicon dioxide-graphite@graphene in Example 1 of the present invention;

[0025] Figure 2 1 is the first cycle charge and discharge curve of silicon dioxide-graphite@graphene in Example 1 of the present invention;

[0026] Figure 3 is the first cycle charge and discharge curve of graphite in Example 1 of the present invention;

[0027] Figure 4 1 is the first cycle charge and discharge curve of silicon dioxide-graphite@graphene in Example 2 of the present invention;

[0028] Figure 5 : is the first cycle charge and discharge curve of silicon dioxide-graphite@graphene in Example 3 of the present invention;

[0029] Figure 6 The first cycle charge and discharge curve of silicon dioxide-graphite@graphene of comparative example 1 of the present invention;

[0030] Figure 7 The first cycle charge and discharge curve of silicon dioxide-graphite@graphene of comparative example 2 of the present invention;

[0031] Figure 8 This is the first cycle charge and discharge curve of silicon dioxide-graphite@graphene of comparative example 3 of the present invention. DETAILED DESCRIPTION

[0032] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0033] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0034] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0035] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.

[0036] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0037] Example 1

[0038] (1) Silicon oxide and graphite raw materials are extracted from silicon solar cell waste and waste lithium-ion batteries, and the extracted silicon oxide and graphite are calcined at 800° C. to remove impurities, thereby obtaining silicon oxide and graphite powders, and the calcination atmosphere is an argon atmosphere.

[0039] (2) Place silicon oxide and graphite powder in a ball mill to reduce their particle size. The particle size of silicon oxide and graphite after ball milling is 50-70 nanometers and the specific surface area is 20-40m 2 g -1 ; The mass ratio of silicon oxide to graphite powder is 1:4, and the mass of the mixed powder is 1:10 to the mass of the steel ball.

[0040] (3) Take 2 kg of ball-milled silica-graphite composite material and 1600 mL of graphene oxide solution (1 g / mL), mix the two briefly and transfer them to a 2 L sand mill chamber, grind for 2 h at a speed of 2000 rpm, and set the separator gap to 0.1-0.12 mm. The silica-graphite@graphene composite material is silica-graphite nanoparticles supported by graphene nanosheets (see Figure 1 ).

[0041] (4) The composite material obtained in step (3) was placed in a 1000 mL beating machine tank with a mass ratio of 90:5:2.5:2.5, and the mixture was stirred at a speed of 1000 rpm for 1 h to obtain an electrode slurry. The slurry was coated on a copper foil current collector with a thickness of 100 μm, placed in a vacuum oven at 60°C, and dried for 12 h to remove the solvent to obtain an electrode sheet.

[0042] (5) The electrode plate obtained in step (4) was assembled into a half-cell with a lithium negative electrode, a Celgard 2400 separator and an electrolyte solution of 1.0 M LiPF6 in EC: DEC: DMC = 1: 1: 1 Vol%. The entire assembly process was carried out in a glove box with a high-purity argon gas atmosphere, with an oxygen content of 0.01 ppm and a water content of 0.01 ppm. The assembled battery was placed in a constant temperature room at 25°C for 12 hours and then subjected to an electrochemical test with a voltage range of 0.01-1.5 V. Its first cycle discharge capacity was 768.9 mAh g -1 High specific capacity ( Figure 2 ), and has a first-cycle coulombic efficiency of 81.5%, and still maintains 500.6mAh g after 100 cycles. -1 The specific capacity of the

[0043] Compared with pure graphite material under the same conditions ( Figure 3 ) compared with the previous research, not only the specific capacity is improved, but also the coulombic efficiency of the first cycle is improved (graphite is 77.5%), which is crucial for the negative electrode.

[0044] Example 2

[0045] (1) Silicon oxide and graphite raw materials are extracted from silicon solar cell waste and waste lithium-ion batteries, and the extracted silicon oxide and graphite are calcined at 800° C. to remove impurities, thereby obtaining silicon oxide and graphite powders, and the calcination atmosphere is an argon atmosphere.

[0046] (2) Place silicon oxide and graphite powder in a ball mill to reduce their particle size. The silicon oxide-graphite particle size after ball milling is 50-70 nanometers and the specific surface area is 20-40m2 g -1 ; The mass ratio of silicon oxide to graphite powder is 1:5, and the mass of the mixed powder is 1:10 to the mass of the steel ball.

[0047] (3) Take 1.2 kg of ball-milled silica-graphite composite material, take 1500 mL of graphene oxide solution (1 g / mL), mix the two briefly and transfer them to a 2 L sand mill chamber, the grinding beads are 0.2 mm, the sand milling is performed for 2 h, the rotation speed is 1000 rpm, and the gap of the separator is 0.1-0.12 mm. The final silica-graphite@graphene composite material is silica-graphite nanoparticles loaded with graphene nanosheets.

[0048] (4) The composite material obtained in step (3) was placed in a 1000 mL beating machine tank with conductive carbon (Super P), carboxymethyl cellulose (CMC), and styrene-butadiene rubber (SBR) in a mass ratio of 90:5:2.5:2.5, and the speed was 1000 rpm and stirred for 1 hour to finally obtain an electrode slurry. The slurry was coated on a copper foil current collector with a thickness of 100 μm, placed in a vacuum oven at 60°C, and dried for 12 hours to remove the solvent.

[0049] (5) The electrode plate obtained in step (4) was assembled into a half-cell with a lithium negative electrode, a Celgard 2400 separator and an electrolyte solution of 1.0 M LiPF6 in EC: DEC: DMC = 1: 1: 1 Vol%. The entire assembly process was carried out in a glove box with a high-purity argon gas atmosphere, with an oxygen content of 0.01 ppm and a water content of 0.01 ppm. The assembled battery was placed in a constant temperature room at 25°C for 12 hours and then subjected to an electrochemical test with a voltage range of 0.01-1.5 V. Its first cycle discharge capacity was 505 mAh g -1 The specific capacity ( Figure 4 ), the first cycle coulombic efficiency is 63.6%, and after 100 cycles, it maintains 270.8 mAh g -1 The specific capacity of the

[0050] Example 3

[0051] (1) Silicon oxide and graphite raw materials are extracted from silicon solar cell waste and waste lithium-ion batteries, and the extracted silicon oxide and graphite are calcined at 800° C. to remove impurities, thereby obtaining silicon oxide and graphite powders, and the calcination atmosphere is an argon atmosphere.

[0052] (2) Place silicon oxide and graphite powder in a ball mill to reduce their particle size. The particle size of silicon oxide and graphite after ball milling is 50-70 nanometers and the specific surface area is 20-40m 2 g -1; The mass ratio of silicon oxide to graphite powder is 1:4, and the mass of the mixed powder is 1:10 to the mass of the steel ball.

[0053] (3) Take 2 kg of ball-milled silica-graphite composite material, take 1600 mL of graphene oxide solution (1 g / mL), mix the two briefly and transfer them to a 2 L sand mill chamber, the grinding beads are 0.2 mm, the sand milling is for 1 h, the rotation speed is 2000 rpm, the gap of the separator is 0.1-0.12 mm, and the final silica-graphite@graphene composite material is silica-graphite nanoparticles loaded with graphene nanosheets.

[0054] (4) The composite material obtained in step (3) was placed in a 1000 mL beating machine tank with a mass ratio of 90:5:2.5:2.5, and the mixture was stirred at a speed of 1000 rpm for 1 h to obtain an electrode slurry. The slurry was coated on a copper foil current collector with a thickness of 100 μm, placed in a vacuum oven at 60°C, and dried for 12 h to remove the solvent to obtain an electrode sheet.

[0055] (5) Assemble a half-cell with the electrode obtained in step (4) and the lithium negative electrode, Celgard 2400 separator and 1.0M LiPF6inEC:DEC:DMC=1:1:1VoL% electrolyte. The whole assembly process is carried out in a glove box with a high-purity argon gas atmosphere, with an oxygen content of 0.01ppm and a water content of 0.01ppm. The assembled battery is placed in a constant temperature room at 25°C for 12 hours and then electrochemically tested, with a voltage range of 0.01-1.5V.

[0056] Its first cycle discharge capacity is 688.5 mAh g -1 The specific capacity of the device is 77.6% and the first cycle coulombic efficiency is 77.6%. Figure 5 ), after 100 cycles, it maintains 450.7 mAh g -1 The specific capacity of the

[0057] Comparative Example 1

[0058] (1) Silicon oxide and graphite raw materials are extracted from silicon solar cell waste and waste lithium-ion batteries, and the extracted silicon oxide and graphite are calcined at 800° C. to remove impurities, thereby obtaining silicon oxide and graphite powders, wherein the calcination atmosphere is an argon atmosphere.

[0059] (2) Place silicon oxide and graphite powder in a ball mill to reduce their particle size. The mass ratio of silicon oxide to graphite powder is 1:8, and the mass of the powder to the mass of the steel ball is 1:10. The particle size of silicon oxide-graphite after ball milling is 50-70 nanometers and the specific surface area is 20-40m2 g -1 .

[0060] (3) The composite material obtained in step (2) was placed in a 1000 mL beating machine tank with conductive carbon (Super P), carboxymethyl cellulose (CMC), and styrene-butadiene rubber (SBR) in a mass ratio of 90:5:2.5:2.5, and the speed was 1000 rpm and stirred for 1 hour to finally obtain the electrode slurry. The slurry was coated on the copper foil current collector with a thickness of 100 microns, placed in a vacuum oven at 60°C, and dried for 12 hours to remove the solvent.

[0061] (4) Assemble a half-cell with the electrode obtained in step (3) and the lithium negative electrode, Celgard 2400 separator and 1.0M LiPF6inEC:DEC:DMC=1:1:1VoL% electrolyte. The whole assembly process is carried out in a glove box with a high-purity argon gas atmosphere, with an oxygen content of 0.01ppm and a water content of 0.01ppm. The assembled battery is placed in a constant temperature room at 25°C for 12 hours and then electrochemically tested, with a voltage range of 0.01-1.5V.

[0062] Without graphene oxide as a substrate, the first cycle released 537.1 mAh g -1 The specific capacity ( Figure 6 ), but the first cycle coulomb efficiency is only 41.5%, indicating that during the charging process, SiO has a serious expansion problem, which leads to the rupture of the electrode material and seriously affects the performance of the battery. After 100 cycles, it maintains 150.1mAh g -1 Specific capacity.

[0063] Comparative Example 2

[0064] (1) Silicon oxide and graphite raw materials are extracted from silicon solar cell waste and waste lithium-ion batteries, and the extracted silicon oxide and graphite are calcined at 800° C. to remove impurities, thereby obtaining silicon oxide and graphite powders, and the calcination atmosphere is an argon atmosphere.

[0065] (2) Place silicon oxide and graphite powder in a ball mill to reduce their particle size. The particle size of silicon oxide and graphite after ball milling is 50-70 nanometers and the specific surface area is 20-40m 2 g -1 ; The mass ratio of silicon oxide to graphite powder is 1:4, and the mass of the mixed powder is 1:10 to the mass of the steel ball.

[0066] (3) Take 2 kg of ball-milled silica-graphite composite material, take 1200 mL of graphene oxide solution (1 g / mL), mix the two briefly and transfer them to a 2 L sand mill chamber, the grinding beads are 0.2 mm, the sand milling is performed for 2 h, the rotation speed is 2000 rpm, and the gap of the separator is 0.1-0.12 mm. The final silica-graphite@graphene composite material is silica-graphite nanoparticles loaded with graphene nanosheets.

[0067] (4) The composite material obtained in step (3) was placed in a 1000 mL beating machine tank with a mass ratio of 90:5:2.5:2.5, and the mixture was stirred at a speed of 1000 rpm for 1 h to obtain an electrode slurry. The slurry was coated on a copper foil current collector with a thickness of 100 μm, placed in a vacuum oven at 60°C, and dried for 12 h to remove the solvent to obtain an electrode sheet.

[0068] (5) The electrode plate obtained in step (4) was assembled into a half-cell with a lithium negative electrode, a Celgard 2400 separator and an electrolyte solution of 1.0 M LiPF6 in EC: DEC: DMC = 1: 1: 1 Vol%. The entire assembly process was carried out in a glove box with a high-purity argon gas atmosphere, with an oxygen content of 0.01 ppm and a water content of 0.01 ppm. The assembled battery was placed in a constant temperature room at 25°C for 12 hours and then subjected to an electrochemical test, with a voltage range of 0.01-1.5 V. Its first cycle discharge capacity was 505.5 mAh g -1 High specific capacity ( Figure 7 ), and has a first-cycle Coulomb efficiency of 71.4%, and still maintains 290.2 mAh g after 100 cycles. -1 The specific capacity of the

[0069] Comparative Example 3

[0070] (1) Silicon oxide and graphite raw materials are extracted from silicon solar cell waste and waste lithium-ion batteries, and the extracted silicon oxide and graphite are calcined at 800° C. to remove impurities, thereby obtaining silicon oxide and graphite powders, and the calcination atmosphere is an argon atmosphere.

[0071] (2) Place silicon oxide and graphite powder in a ball mill to reduce their particle size. The particle size of silicon oxide and graphite after ball milling is 50-70 nanometers and the specific surface area is 20-40m 2 g -1 ; The mass ratio of silicon oxide to graphite powder is 1:4, and the mass of the mixed powder is 1:10 to the mass of the steel ball.

[0072] (3) Take 2 kg of ball-milled silica-graphite composite material, take 1800 mL of graphene oxide solution (1 g / mL), mix the two briefly and transfer them to a 2 L sand mill chamber, the grinding beads are 0.2 mm, the sand milling is for 1 h, the rotation speed is 2000 rpm, the gap of the separator is 0.1-0.12 mm, and the final silica-graphite@graphene composite material is silica-graphite nanoparticles loaded with graphene nanosheets.

[0073] (4) The composite material obtained in step (3) was placed in a 1000 mL beating machine tank with a mass ratio of 90:5:2.5:2.5, and the mixture was stirred at a speed of 1000 rpm for 1 h to obtain an electrode slurry. The slurry was coated on a copper foil current collector with a thickness of 100 μm, placed in a vacuum oven at 60°C, and dried for 12 h to remove the solvent to obtain an electrode sheet.

[0074] (5) The electrode plate obtained in step (4) was assembled into a half-cell with a lithium negative electrode, a Celgard 2400 separator and an electrolyte solution of 1.0 M LiPF6 in EC: DEC: DMC = 1: 1: 1 Vol%. The entire assembly process was carried out in a glove box with a high-purity argon gas atmosphere, with an oxygen content of 0.01 ppm and a water content of 0.01 ppm. The assembled battery was placed in a constant temperature room at 25°C for 12 hours and then subjected to an electrochemical test with a voltage range of 0.01-1.5 V. Its first cycle discharge capacity was 469.4 mAh g -1 The specific capacity ( Figure 8 ), and has a first-cycle Coulomb efficiency of 73.3%, and still maintains 320.6 mAh g after 100 cycles. -1 The specific capacity of the

[0075] Table 1

[0076]

[0077] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. An application of silicon dioxide-graphite@graphene material in negative electrode material of lithium ion battery, characterized in that: The method for preparing the silicon dioxide-graphite@graphene material comprises the following steps: Step 1, mixing silicon dioxide and graphite in a mass ratio of 1:4 and ball milling to obtain a composite powder; Step 2, mixing the composite powder and the graphene oxide solution in a ratio of 2kg:1600mL and then sand-milling to obtain the silicon dioxide-graphite@graphene material; The concentration of the graphene oxide solution is 1 g / mL; After mixing and ball milling, the particle size of the composite powder is 50-70nm and the specific surface area is 20-40m 2 g -1 ; During the mixed ball milling process in step 1, ball milling is performed in a ratio of 1:10 between the total mass of silicon dioxide and graphite and the mass of steel balls.