Water-based coating composition and multi-layer coating film forming method
By using water-based coating compositions containing resins containing hydroxyl and carboxyl groups, blocked polyisocyanate compounds, polycarbodiimide compounds and alkaline compounds, combined with a specific heating process, the difficulty of low-temperature baking curing technology in automotive coatings is solved. Taking into consideration the issues of coating film performance, it achieves high hardness, water resistance and good glass adhesion, and improves storage stability and adhesion.
Patent Information
- Application Number
- CN202180093225.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-16
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-12-16
AI Technical Summary
In existing automobile coatings, low-temperature baking and curing technology is difficult to balance the hardness, stone chip resistance and storage stability of the coating film, and the cohesive damage or peeling problems of the adhesive layer lead to poor adhesion of the components.
A water-based coating composition using resins containing hydroxyl and carboxyl groups, blocked polyisocyanate compounds, polycarbodiimide compounds and alkaline compounds is formulated at a specific pH value and ratio, combined with a heating and curing process of 60 to 110°C. Forms high-performance multi-layer coatings.
It achieves the performance of forming a coating film with high hardness, water resistance and good glass adhesion at a lower temperature, improves the storage stability and adhesion of the coating film, and avoids cohesive damage and peeling of the adhesive layer. .
Smart Images

Figure BDA0004382170560000431 
Figure BDA0004382170560000441 
Figure BDA0004382170560000451
Abstract
Description
Technical Field
[0001] The present invention relates to a water-based coating composition and a method for forming a multi-layer coating film. Background Art
[0002] In automobile painting, a method of forming a multilayer coating film by the following three-coat-two-bake (3C2B) method has been widely used. The three-coat-two-bake (3C2B) method is to apply the electrodeposition paint to the object to be coated, then apply the intermediate coating → bake and cure → apply the water-based base coating → preheat (preheating) → apply the clear coating → bake and cure. However, in recent years, from the viewpoint of energy saving, the following three-coat-one-bake (3C1B) method is being promoted, that is, the baking and curing step after the application of the intermediate coating is omitted, and after the electrodeposition paint is applied to the object to be coated, the water-based intermediate coating is applied → preheat (preheating) as needed → apply the water-based base coating → preheat (preheating) → apply the clear coating → bake and cure.
[0003] Furthermore, recently, in order to further reduce the energy used, it is required to lower the heating temperature in the baking and curing step.
[0004] However, a coating composition that has high curability even at a relatively low heating temperature is generally highly reactive and therefore may not be able to achieve both coating film properties such as hardness, stone chipping resistance, and water resistance and storage stability.
[0005] In addition, in the manufacturing specifications of automobiles, for glass components such as front windshields and rear windshields, an adhesive layer is usually formed on the multilayer coating film, and the components are fixed to the multilayer coating film by means of the adhesive layer. However, if the above-mentioned stone chipping resistance is improved by softening the midcoat film, the multilayer coating film under the adhesive layer may sometimes undergo cohesive failure, or peeling may occur at the interface between the electrodeposition coating film and the midcoat film, thereby causing poor adhesion to the component.
[0006] Patent document 1 describes a multilayer coating film forming method, characterized in that the following steps (1) to (4) are sequentially performed on an alloyed hot-dip galvanized steel sheet that has been electroplated: step (1): a step of applying a water-based intermediate coating material (A) on the electroplated coating film to form an intermediate coating film; step (2): a step of applying a water-based base coating material (B) on the intermediate coating film after preheating to form a base coating film; step (3): a step of applying a clear coating material (C) on the base coating film after preheating to form a clear coating film; step (4): a step of heat-curing the intermediate coating film, the base coating film, and the clear coating film formed in the steps (1) to (3), wherein the water-based intermediate coating material (A) contains: a hydroxyl-containing an acrylic resin (a1); a polyurethane resin (a2) having a polyether skeleton and a glass transition temperature (Tg) of -50°C or less; a hydroxyl-containing polyester resin (a3); a melamine resin (a4); and an active methylene-terminated polyisocyanate compound (a5), wherein the usage ratio of the hydroxyl-containing acrylic resin (a1) to the polyurethane resin (a2) is in the range of 20 / 10 to 30 / 10 in terms of solid content ratio, the elongation at break at 20°C of the coating film formed after the water-based mid-coat (A) is heated and cured is in the range of 20 to 30%, the Young's modulus is in the range of 5000 to 6000 kgf / cm2, and the Tukon hardness is in the range of 4 to 6, and the clear coating (C) contains the hydroxyl-containing acrylic resin (c1) and the allophanate-containing polyisocyanate compound (c2).
[0007] The above-mentioned multilayer coating film forming method has excellent glass adhesion, coating film performance and storage stability, but in recent years, from the viewpoint of energy saving, lowering of the heating temperature has been desired.
[0008] Prior art literature
[0009] Patent Literature
[0010] Patent Document 1: Japanese Patent Application Publication No. 2019-198861 Summary of the invention
[0011] Problem that the invention aims to solve
[0012] An object of the present invention is to provide an aqueous coating composition which has excellent storage stability and can exhibit high coating film performance and glass adhesion even when cured at a relatively low temperature.
[0013] Technical Solution
[0014] The present inventors have repeatedly conducted in-depth studies to achieve the above-mentioned purpose, and as a result, found that the above-mentioned purpose can be achieved according to the following water-based coating composition, which contains: (A) a resin containing hydroxyl groups and carboxyl groups, (B) a blocked polyisocyanate compound, (C) a polycarbodiimide compound and (D) a basic compound, wherein the basic compound (D) contains (D1) an acid dissociation constant (PKa) in the range of 7.0 to 8.5 and a boiling point in the range of 100 to 200°C, and the content ratio of the basic compound (D1) is in the range of 30 to 100% by mass based on the mass of the basic compound (D), and the pH of the water-based coating composition is in the range of 8.0 to 11.5.
[0015] According to the present invention, there are provided an aqueous coating composition and a method for forming a multilayer coating film including the following aspects.
[0016] Item 1. An aqueous coating composition comprising: (A) a resin containing hydroxyl and carboxyl groups, (B) a blocked polyisocyanate compound, (C) a polycarbodiimide compound, and (D) an alkaline compound, wherein the alkaline compound (D) contains (D1) an alkaline compound having an acid dissociation constant (PKa) in the range of 7.0 to 8.5 and a boiling point in the range of 100 to 200°C, and the content ratio of the alkaline compound (D1) is in the range of 30 to 100% by mass based on the mass of the alkaline compound (D), and the pH of the aqueous coating composition is in the range of 8.0 to 11.5.
[0017] Item 2. The aqueous coating composition according to Item 1, wherein at least a part of the blocking agent of the blocked polyisocyanate compound (B) is an active methylene-based blocking agent.
[0018] Item 3. The aqueous coating composition according to Item 1 or 2, wherein the basic compound (D1) having an acid dissociation constant (PKa) in the range of 7.0 to 8.5 and a boiling point in the range of 100 to 200° C. is N-methylmorpholine and / or N-ethylmorpholine.
[0019] Item 4. The aqueous coating composition according to any one of Items 1 to 3, further comprising a melamine resin (E).
[0020] Item 5. A method for forming a multilayer coating film, comprising performing the following steps in sequence: step (1): a step of applying an aqueous coating composition as described in any one of items 1 to 4 on a coated object to form a mid-coat film; step (2): a step of applying an aqueous base coating composition on the mid-coat film formed in the step (1) to form a base coating film; step (3): a step of applying a clear coating composition on the base coating film formed in the step (2) to form a clear coating film; and step (4): a step of simultaneously heating and curing the mid-coat film, base coating film and clear coating film formed in the steps (1) to (3) at a temperature in the range of 60 to 110°C.
[0021] Beneficial Effects
[0022] The aqueous coating composition of the present invention has excellent storage stability and can form a coating film having excellent coating film properties such as high hardness and water resistance and good glass adhesion even when cured at a relatively low temperature. DETAILED DESCRIPTION
[0023] Hereinafter, the aqueous coating composition of the present invention (hereinafter, sometimes simply referred to as "the present coating") will be described in further detail.
[0024] Waterborne coating composition
[0025] The water-based coating composition of the present invention contains: (A) a resin containing hydroxyl groups and carboxyl groups, (B) a blocked polyisocyanate compound, (C) a polycarbodiimide compound, and (D) a basic compound, wherein the basic compound (D) contains (D1) a basic compound having an acid dissociation constant (PKa) in the range of 7.0 to 8.5 and a boiling point in the range of 100 to 200° C., and the content ratio of the basic compound (D1) is in the range of 30 to 100% by mass based on the mass of the basic compound (D), and the pH of the water-based coating composition is in the range of 8.0 to 11.5.
[0026] It should be noted that, in this specification, water-based paint refers to a term contrasted with organic solvent-based paint, and generally refers to a paint formed by dispersing and / or dissolving a film-forming resin, a pigment, etc. in water or a medium (aqueous medium) with water as the main component. In addition, the above-mentioned organic solvent-based paint refers to a paint in which the solvent does not substantially contain water, or all or most of the solvent is an organic solvent.
[0027] The pH of the aqueous coating composition of the present invention is within the range of 8.0 to 11.5.
[0028] When the pH is 8.0 or higher, an aqueous coating composition having excellent storage stability can be obtained, and when the pH is 11.5 or lower, an aqueous coating composition having excellent hardness, water resistance, and glass adhesion of the formed coating film can be obtained.
[0029] Among them, the pH is preferably in the range of 8.5 to 11.0, and more preferably in the range of 9.0 to 10.5.
[0030] Resin containing hydroxyl and carboxyl groups (A)
[0031] The resin (A) containing a hydroxyl group and a carboxyl group is not particularly limited as long as it is a resin containing a hydroxyl group and a carboxyl group, and specific examples of the resin include acrylic resins, polyester resins, polyether resins, polycarbonate resins, and polyurethane resins. In particular, as the resin (A) containing a hydroxyl group and a carboxyl group, acrylic resins, polyester resins, and polyurethane resins containing a hydroxyl group and a carboxyl group can be preferably used.
[0032] Acrylic resin containing hydroxyl and carboxyl groups (A1)
[0033] The hydroxyl- and carboxyl-containing acrylic resin (A1) can be synthesized by copolymerizing a hydroxyl-containing polymerizable unsaturated monomer (M-1), a carboxyl-containing polymerizable unsaturated monomer (M-2), and other copolymerizable polymerizable unsaturated monomers (M-3) using a conventional method.
[0034] The hydroxyl-containing polymerizable unsaturated monomer (M-1) is a compound having one hydroxyl group and one polymerizable unsaturated bond in one molecule, and the hydroxyl group mainly functions as a functional group that reacts with a crosslinking agent. Specifically, the monomer is preferably a monoester of acrylic acid or methacrylic acid and a diol having 2 to 10 carbon atoms, for example, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, etc.
[0035] In addition, as the monoester of acrylic acid or methacrylic acid and a polyol, in addition to the substances listed above, there can be listed: compounds obtained by further adding a ring-opening polymer of ε-caprolactone or the like to a monoester such as 2-hydroxyethyl (meth)acrylate, for example: "PLACCEL FA-1", "PLACCEL FA-2", "PLACCEL FA-3", "PLACCEL FA-4", "PLACCEL FA-5", "PLACCEL FM-1", "PLACCEL FM-2", "PLACCEL FM-3", "PLACCEL FM-4", "PLACCEL FM-5" (all of which are trade names manufactured by Daicel Chemical Co., Ltd.); polyethylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate; 2-hydroxy-3-phenoxypropyl (meth)acrylate, 2-hydroxy-3-butoxypropyl (meth)acrylate; phthalic acid monohydroxyethyl (meth)acrylate, etc. These can be used alone or in combination of two or more.
[0036] However, in the present invention, a monomer that meets the requirements of the “(xvi) polymerizable unsaturated monomer having an ultraviolet absorbing functional group” described later should be defined as the above-mentioned “other copolymerizable polymerizable unsaturated monomers (M-3)” and excluded from the “hydroxyl-containing polymerizable unsaturated monomer (M-1)” even if it is a monomer having a hydroxyl group.
[0037] The carboxyl-containing polymerizable unsaturated monomer (M-2) is a compound having one or more carboxyl groups and one polymerizable unsaturated bond in one molecule, and examples thereof include acrylic acid, methacrylic acid, crotonic acid, itaconic acid, maleic acid, and maleic anhydride, etc. These monomers may be used alone or in combination of two or more.
[0038] Other copolymerizable polymerizable unsaturated monomers (M-3) are compounds having one or more polymerizable unsaturated bonds in one molecule other than the above-mentioned monomers (M-1) and (M-2), and specific examples thereof are listed below.
[0039] (i) Alkyl (meth)acrylate or cycloalkyl (meth)acrylate: for example, methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, n-hexyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, tridecyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, cyclohexyl (meth)acrylate, methylcyclohexyl (meth)acrylate, tert-butylcyclohexyl (meth)acrylate, cyclododecyl (meth)acrylate, tricyclodecyl (meth)acrylate, etc.
[0040] (ii) Polymerizable unsaturated monomer having an isobornyl group: isobornyl (meth)acrylate, etc.
[0041] (iii) Polymerizable unsaturated monomer having an adamantyl group: adamantyl (meth)acrylate, etc.
[0042] (iv) Polymerizable unsaturated monomer having a tricyclodecenyl group: tricyclodecenyl (meth)acrylate, etc.
[0043] (v) Aromatic ring-containing polymerizable unsaturated monomers: benzyl (meth)acrylate, styrene, α-methylstyrene, vinyltoluene, etc.
[0044] (vi) Polymerizable unsaturated monomers having an alkoxysilyl group: vinyltrimethoxysilane, vinyltriethoxysilane, vinyltri(2-methoxyethoxy)silane, γ-(meth)acryloxypropyltrimethoxysilane, γ-(meth)acryloxypropyltriethoxysilane, and the like.
[0045] (vii) Polymerizable unsaturated monomers having a fluoroalkyl group: perfluoroalkyl (meth)acrylates such as perfluorobutyl ethyl (meth)acrylate and perfluorooctyl ethyl (meth)acrylate; fluoroolefins, and the like.
[0046] (viii) A polymerizable unsaturated monomer having a photopolymerizable functional group such as a maleimide group.
[0047] (ix) Vinyl compounds: N-vinyl pyrrolidone, ethylene, butadiene, chloroprene, vinyl propionate, vinyl acetate, and the like.
[0048] (x) Nitrogen-containing polymerizable unsaturated monomers: (meth)acrylonitrile, (meth)acrylamide, N,N-dimethylaminoethyl (meth)acrylate, N,N-diethylaminoethyl (meth)acrylate, N,N-dimethylaminopropyl (meth)acrylamide, methylenebis(meth)acrylamide, ethylenebis(meth)acrylamide, addition products of glycidyl (meth)acrylate and amine compounds, etc.
[0049] (xi) Polymerizable unsaturated monomers having two or more polymerizable unsaturated groups in one molecule: allyl (meth)acrylate, ethylene glycol di(meth)acrylate, 1,4-butylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, and the like.
[0050] (xii) Epoxy-containing polymerizable unsaturated monomers: glycidyl (meth)acrylate, β-methyl glycidyl (meth)acrylate, 3,4-epoxycyclohexylmethyl (meth)acrylate, 3,4-epoxycyclohexylethyl (meth)acrylate, 3,4-epoxycyclohexylpropyl (meth)acrylate, allyl glycidyl ether, and the like.
[0051] (xiii) (meth)acrylates having a polyoxyethylene chain having an alkoxy group at a molecular terminal.
[0052] (xiv) Polymerizable unsaturated monomers having a sulfonic acid group: 2-acrylamide-2-methylpropanesulfonic acid, 2-sulfoethyl (meth)acrylate, allylsulfonic acid, 4-styrenesulfonic acid, etc.; sodium salts and ammonium salts of these sulfonic acids, etc.
[0053] (xv) Polymerizable unsaturated monomers having a phosphoric acid group: acidic phosphonooxyethyl (meth)acrylate, acidic phosphonooxypropyl (meth)acrylate, acidic phosphonooxypoly (oxyethylene) glycol (meth)acrylate, acidic phosphonooxypoly (oxypropylene) glycol (meth)acrylate, and the like.
[0054] (xvi) Polymerizable unsaturated monomers having ultraviolet absorbing functional groups: 2-hydroxy-4-(3-methacryloyloxy-2-hydroxypropoxy)benzophenone, 2-hydroxy-4-(3-acryloyloxy-2-hydroxypropoxy)benzophenone, 2,2'-dihydroxy-4-(3-methacryloyloxy-2-hydroxypropoxy)benzophenone, 2,2'-dihydroxy-4-(3-acryloyloxy-2-hydroxypropoxy)benzophenone, 2-[2-hydroxy-5-[2-(methacryloyloxy)ethyl]phenyl]-2H-benzotriazole, etc.
[0055] (xvii) Light-stable polymerizable unsaturated monomers: 4-(meth)acryloyloxy 1,2,2,6,6-pentamethylpiperidine, 4-(meth)acryloyloxy-2,2,6,6-tetramethylpiperidine, 4-cyano-4-(meth)acryloylamino-2,2,6,6-tetramethylpiperidine, 1-(meth)acryloyl-4-(meth)acryloylamino-2,2,6,6-tetramethylpiperidine, 1-(meth)acryloyl-4-cyano-4-(meth)acryloylamino-2,2,6,6-tetramethylpiperidine, 4-crotonyloxy-2,2,6,6-tetramethylpiperidine, 4-crotonylamino-2,2,6,6-tetramethylpiperidine, 1-crotonyl-4-crotonyloxy-2,2,6,6-tetramethylpiperidine, and the like.
[0056] (xviii) Polymerizable unsaturated monomers having a carbonyl group: acrolein, diacetone acrylamide, diacetone methacrylamide, acetoacetoxyethyl methacrylate, formylstyrene, vinyl alkyl ketones having 4 to 7 carbon atoms (e.g., vinyl methyl ketone, vinyl ethyl ketone, vinyl butyl ketone), etc.
[0057] (xix) Polymerizable unsaturated monomers having an acid anhydride group: maleic anhydride, itaconic anhydride, citraconic anhydride, and the like.
[0058] In the present specification, the polymerizable unsaturated group refers to an unsaturated group that can be radically polymerized. Examples of the polymerizable unsaturated group include a vinyl group and a (meth)acryloyl group.
[0059] In addition, in this specification, "(meth)acrylate" means acrylate or methacrylate. "(meth)acrylic acid" means acrylic acid or methacrylic acid. In addition, "(meth)acryloyl" means acryloyl or methacryloyl. In addition, "(meth)acrylamide" means acrylamide or methacrylamide.
[0060] The proportion of the hydroxyl-containing polymerizable unsaturated monomer (M-1) used when producing the hydroxyl- and carboxyl-containing acrylic resin (A1) is preferably 1 to 50% by mass, more preferably 2 to 40% by mass, and even more preferably 3 to 30% by mass based on the total amount of the monomer components.
[0061] From the viewpoints of the curability, stone chipping resistance, adhesion, hardness, finished product appearance, and glass adhesion of the resulting coating film, the hydroxyl value of the hydroxyl- and carboxyl-containing acrylic resin (A1) is preferably 1 to 150 mgKOH / g, more preferably 2 to 120 mgKOH / g, and even more preferably 5 to 100 mgKOH / g.
[0062] The proportion of the carboxyl-containing polymerizable unsaturated monomer (M-2) used when producing the hydroxyl- and carboxyl-containing acrylic resin (A1) is preferably 1 to 50% by mass, more preferably 2 to 40% by mass, and even more preferably 3 to 30% by mass based on the total amount of the monomer components.
[0063] Furthermore, from the viewpoints of the storage stability of the coating material, the water resistance of the obtained coating film, etc., the acid value of the above-mentioned hydroxyl group- and carboxyl group-containing acrylic resin (A1) is preferably 1 to 80 mgKOH / g, more preferably 5 to 50 mgKOH / g, and even more preferably 5 to 30 mgKOH / g.
[0064] When the aqueous coating composition of the present invention contains the above-mentioned hydroxyl- and carboxyl-containing acrylic resin (A1), the content of the hydroxyl- and carboxyl-containing acrylic resin (A1) is preferably 2 to 70% by mass, more preferably 5 to 50% by mass, and further preferably 10 to 40% by mass, based on the resin solid content in the aqueous coating composition.
[0065] Furthermore, the above-mentioned hydroxyl- and carboxyl-containing acrylic resin (A1) is preferably a hydroxyl- and carboxyl-containing acrylic resin particle (A1′) having a core-shell structure.
[0066] Core-shell structured acrylic resin particles containing hydroxyl and carboxyl groups (A1')
[0067] In the present invention, the "shell portion" of the "hydroxyl- and carboxyl-containing acrylic resin particles (A1') having a core-shell structure" refers to the polymer layer present in the outermost layer of the resin particles, the "core portion" refers to the polymer layer of the inner layer of the resin particles excluding the above-mentioned shell portion, and "having a core-shell structure" refers to a structure having the above-mentioned core portion and shell portion.
[0068] In addition, below, "the acrylic resin particles (A1') containing a hydroxyl group and a carboxyl group and having a core-shell structure" may be simply referred to as "the acrylic resin particles (A1') containing a hydroxyl group and a carboxyl group".
[0069] In the core-shell structure, generally, the core is completely covered by the shell, but depending on the mass ratio of the core to the shell, the amount of the shell may not be enough to form a layer structure. In this case, it is not necessary to have a complete layer structure as described above, and the shell may cover part of the core.
[0070] The hydroxyl- and carboxyl-containing acrylic resin particles (A1') are generally acrylic resin particles composed of a core portion and a shell portion, wherein the core portion is a copolymer (I) containing a polymerizable unsaturated monomer as a copolymer component, and the shell portion is a copolymer (II) containing a polymerizable unsaturated monomer as a copolymer component. The polymerizable unsaturated monomer can be used in appropriate combination of the polymerizable unsaturated monomers (M-1) to (M-3).
[0071] By using the polymerizable unsaturated monomer having two or more polymerizable unsaturated groups in one molecule as the above-mentioned polymerizable unsaturated monomer, a cross-linked structure can be given to the copolymer. When using the polymerizable unsaturated monomer having two or more polymerizable unsaturated groups in one molecule, its usage ratio can be appropriately determined according to the degree of cross-linking of the copolymer, and usually, it is preferably about 0.1 to 30% by mass, particularly preferably about 0.5 to 10% by mass, and further particularly preferably in the range of about 1 to 7% by mass relative to the total amount of the polymerizable unsaturated monomers (M-1) to (M-3).
[0072] The hydroxyl- and carboxyl-containing acrylic resin particles (A1′) can be obtained by subjecting a polymerizable unsaturated monomer mixture to emulsion polymerization to obtain an emulsion of a core copolymer (I), adding the polymerizable unsaturated monomer mixture to the emulsion, and further subjecting the emulsion to emulsion polymerization to prepare a shell copolymer (II).
[0073] The emulsion polymerization for preparing the emulsion of the core copolymer (I) can be carried out by a conventionally known method, for example, by emulsion polymerization of a polymerizable unsaturated monomer mixture using a polymerization initiator in the presence of an emulsifier.
[0074] As the emulsifier, an anionic emulsifier and a nonionic emulsifier can be preferably used.
[0075] Examples of the anionic emulsifier include sodium salts and ammonium salts of alkylsulfonic acid, alkylbenzenesulfonic acid, and alkylphosphoric acid. Examples of the nonionic emulsifier include polyoxyethylene oleyl ether, polyoxyethylene stearyl ether, polyoxyethylene lauryl ether, polyoxyethylene tridecyl ether, polyoxyethylene phenyl ether, polyoxyethylene nonylphenyl ether, polyoxyethylene octylphenyl ether, polyoxyethylene monolaurate, polyoxyethylene monostearate, polyoxyethylene monooleate, sorbitan monolaurate, sorbitan monostearate, sorbitan trioleate, and polyoxyethylene sorbitan monolaurate.
[0076] In addition, a polyoxyalkylene-containing anionic emulsifier having an anionic group and a polyoxyalkylene group such as a polyoxyethylene group or a polyoxypropylene group in one molecule; a reactive anionic emulsifier having an anionic group and a radical polymerizable unsaturated group in one molecule, etc. can also be used.
[0077] Examples of the reactive anionic emulsifier include sodium salts of sulfonic acid compounds having a radical polymerizable unsaturated group such as an allyl group, a methallyl group, a (meth)acryloyl group, a propenyl group, or a butenyl group, and ammonium salts of the sulfonic acid compounds.
[0078] The amount of the emulsifier used is preferably about 0.1 to 15% by mass, particularly preferably about 0.5 to 10% by mass, and even more preferably about 1 to 5% by mass, based on the total amount of all monomers used.
[0079] Examples of the polymerization initiator include organic peroxides such as benzoyl peroxide, octanoyl peroxide, lauroyl peroxide, stearoyl peroxide, cumene hydroperoxide, tert-butyl peroxide, tert-butyl peroxylaurate, tert-butyl peroxyisopropyl carbonate, tert-butyl peroxyacetate, and diisopropylbenzene hydroperoxide; azo compounds such as azobisisobutyronitrile, azobis(2,4-dimethylvaleronitrile), azobis(2-methylpropionitrile), azobis(2-methylbutyronitrile), 4,4'-azobis(4-cyanobutyric acid), dimethylazobis(2-methylpropionate), azobis[2-methyl-N-(2-hydroxyethyl)-propionamide], and azobis{2-methyl-N-[2-(1-hydroxybutyl)]-propionamide}; and persulfates such as potassium persulfate, ammonium persulfate, and sodium persulfate. These polymerization initiators may be used alone or in combination of two or more. Furthermore, the above-mentioned polymerization initiators may be used together with a reducing agent such as sugar, sodium formaldehyde sulfoxylate, or an iron complex as a redox initiator as necessary.
[0080] The amount of the polymerization initiator used is usually preferably about 0.1 to 5% by mass, particularly preferably about 0.2 to 3% by mass, relative to the total amount of all monomers used. The method of adding the polymerization initiator is not particularly limited and can be appropriately selected according to its type and amount. For example, it can be contained in the monomer mixture or aqueous medium in advance, or it can be added or added dropwise at the time of polymerization.
[0081] The hydroxyl group- and carboxyl group-containing acrylic resin particles (A1′) can be obtained by adding a polymerizable unsaturated monomer mixture to the emulsion of the core copolymer (I) obtained above, and further polymerizing the mixture to form a shell copolymer (II).
[0082] The monomer mixture forming the shell copolymer (II) may contain the polymerization initiator, chain transfer agent, reducing agent, emulsifier and other components as required. In addition, the monomer mixture may be added dropwise as it is, but it is preferably added dropwise in the form of a monomer emulsion obtained by dispersing the monomer mixture in an aqueous medium. The particle size of the monomer emulsion in this case is not particularly limited.
[0083] Examples of a method for polymerizing the monomer mixture for forming the shell copolymer (II) include a method in which the monomer mixture or an emulsion thereof is added all at once or slowly dropwise to the emulsion of the core copolymer (I), and heated to an appropriate temperature while stirring.
[0084] The hydroxyl- and carboxyl-containing acrylic resin particles (A1′) thus obtained have a multilayer structure having the copolymer (I) as a core and the copolymer (II) as a shell.
[0085] When the aqueous coating composition of the present invention contains the above-mentioned hydroxyl- and carboxyl-containing acrylic resin particles (A1'), the content of the hydroxyl- and carboxyl-containing acrylic resin particles (A1') is preferably 2 to 70% by mass, more preferably 5 to 50% by mass, and further preferably 10 to 40% by mass, based on the resin solid content in the aqueous coating composition.
[0086] In addition, when preparing the acrylic resin particles (A1') containing hydroxyl and carboxyl groups, the following step can be added between the step of obtaining the core copolymer (I) and the step of obtaining the shell copolymer (II): supplying a polymerizable unsaturated monomer (a mixture of one or more than two) for forming other resin layers and performing emulsion polymerization. Among them, it is preferred to form a gradient polymer layer as an additional layer to prepare the acrylic resin particles (A1") containing hydroxyl and carboxyl groups having a core-shell structure including the gradient polymer layer.
[0087] Core-shell structured acrylic resin particles containing hydroxyl and carboxyl groups and comprising a gradient polymer layer (A1")
[0088] In the present invention, the gradient polymer layer of "the core-shell structured acrylic resin particles containing hydroxyl and carboxyl groups (A1")" refers to a polymer layer having a layer structure in which the composition changes continuously (having a composition gradient).
[0089] More specifically, for example, it refers to a polymer layer having a composition gradient in which the monomer (monomer mixture) composition changes continuously from monomer A (monomer mixture A) to monomer B (monomer mixture B).
[0090] In addition, below, "the hydroxyl- and carboxyl-containing acrylic resin particles (A1") having a core-shell structure including a gradient polymer layer" may be simply referred to as "hydroxyl- and carboxyl-containing acrylic resin particles (A1")".
[0091] The above-mentioned gradient polymer layer can be obtained by a known polymerization method known as power feed polymerization usually. Specifically, for example, when monomer A (monomer mixture A) and monomer B (monomer mixture B) are subjected to polymerization reaction, the gradient polymer layer can be obtained by dropping monomer B (monomer mixture B) in a container containing monomer A (monomer mixture A) while monomer A (monomer mixture A) is introduced into a reaction vessel for polymerization reaction.
[0092] In the above-mentioned power feed polymerization, a gradient polymer layer having a desired composition gradient can be obtained according to the synthesis conditions (the time when the mixing of monomer A (monomer mixture A) and monomer B (monomer mixture B) starts, the rate of dripping monomer B (monomer mixture B) into the container containing monomer A (monomer mixture A) and the setting of the rate of introducing monomer A (monomer mixture A) into the reaction container, etc.).
[0093] From the viewpoint of water resistance of the obtained coating film, the ratio of the gradient polymer layer in the hydroxyl- and carboxyl-containing acrylic resin particles (A1") is preferably about 20 to 80 mass %, particularly preferably about 25 to 75 mass %, and further particularly preferably about 30 to 70 mass % relative to the total amount of all copolymer components of the hydroxyl- and carboxyl-containing acrylic resin particles (A1").
[0094] From the viewpoints of the curability, stone chipping resistance, adhesion, finished product appearance, and glass adhesion of the resulting coating film, the hydroxyl value of the hydroxyl- and carboxyl-containing acrylic resin particles (A1") is preferably 1 to 150 mgKOH / g, more preferably 2 to 120 mgKOH / g, and even more preferably 5 to 100 mgKOH / g.
[0095] From the viewpoint of water resistance and stone chipping resistance of the obtained coating film, the hydroxyl value of the core part of the hydroxyl- and carboxyl-containing acrylic resin particles (A1") is preferably 0 to 150 mgKOH / g, more preferably 5 to 120 mgKOH / g, and further preferably 10 to 100 mgKOH / g.
[0096] From the viewpoint of water resistance, stone chipping resistance and glass adhesion of the obtained coating film, the hydroxyl value of the shell part of the hydroxyl and carboxyl group-containing acrylic resin particles (A1") is preferably 0 to 150 mgKOH / g, more preferably 2 to 120 mgKOH / g, and further preferably 5 to 100 mgKOH / g.
[0097] From the viewpoint of the storage stability of the coating material, the water resistance of the obtained coating film, etc., the acid value of the hydroxyl group- and carboxyl group-containing acrylic resin particles (A1") is preferably 1 to 80 mgKOH / g, more preferably 5 to 50 mgKOH / g, and even more preferably 5 to 30 mgKOH / g.
[0098] From the viewpoint of production stability and storage stability of the coating, the acid value of the core of the hydroxyl- and carboxyl-containing acrylic resin particles (A1") is preferably 0 to 50 mgKOH / g, more preferably 0 to 30 mgKOH / g, and even more preferably 0 to 10 mgKOH / g.
[0099] From the viewpoint of storage stability of the coating material and water resistance of the obtained coating film, the acid value of the shell part of the hydroxyl group- and carboxyl group-containing acrylic resin particles (A1") is preferably 1 to 100 mgKOH / g, more preferably 5 to 80 mgKOH / g, and even more preferably 10 to 50 mgKOH / g.
[0100] From the viewpoint of water resistance, stone chipping resistance, and glass adhesion of the resulting coating film, the glass transition temperature of the hydroxyl- and carboxyl-containing acrylic resin particles (A1") is preferably -20 to 100°C, more preferably 0 to 100°C, and even more preferably 20 to 100°C.
[0101] From the viewpoint of water resistance, stone chipping resistance, and glass adhesion of the resulting coating film, the glass transition temperature of the core of the hydroxyl- and carboxyl-containing acrylic resin particles (A1") is preferably -50 to 50°C, more preferably -30 to 50°C, and even more preferably 0 to 50°C.
[0102] The glass transition temperature of the shell part of the hydroxyl- and carboxyl-containing acrylic resin particles (A1") is preferably 0 to 120°C, more preferably 20 to 100°C, and further preferably 30 to 100°C, from the viewpoint of water resistance of the obtained coating film.
[0103] In this specification, the glass transition temperature (Tg) is calculated according to the following formula.
[0104] 1 / Tg(K)=(W1 / T1)+(W2 / T2)+……(1)
[0105] Tg(℃)=Tg(K)-273(2)
[0106] In the formulae, W1, W2, ... represent the mass fractions of the monomers used for copolymerization, and T1, T2, ... represent the Tg (K) of the homopolymer of each monomer.
[0107] It should be noted that T1, T2, ... are values from pages III-139 to 179 of Polymer Hand Book (Second Edition, edited by J. Brandup μE. H. Immergut). In addition, when the Tg of the homopolymer of the monomer is unclear, the glass transition temperature (Tg) is set as the static glass transition temperature. For example, a differential scanning calorimeter "DSC-220U" (manufactured by Seiko Instrument (KK)) is used, and the sample is taken into a measuring cup, and the solvent is completely removed by vacuum suction, and then the heat change is measured in the range of -20°C to +200°C at a heating rate of 3°C / min, and the change point of the initial baseline on the low temperature side is set as the static glass transition temperature.
[0108] When the aqueous coating composition of the present invention contains the above-mentioned hydroxyl- and carboxyl-containing acrylic resin particles (A1"), the content of the hydroxyl- and carboxyl-containing acrylic resin particles (A1") is preferably 2 to 70% by mass, more preferably 5 to 50% by mass, and further preferably 10 to 40% by mass, based on the resin solid content in the aqueous coating composition.
[0109] Polyester resin containing hydroxyl and carboxyl groups (A2)
[0110] The polyester resin (A2) containing a hydroxyl group and a carboxyl group can be synthesized by subjecting a polybasic acid to an esterification reaction with a polyhydric alcohol according to a conventional method using a known method.
[0111] The polyacid is a compound having two or more carboxyl groups in one molecule, and examples thereof include phthalic acid, isophthalic acid, terephthalic acid, succinic acid, adipic acid, azelaic acid, sebacic acid, tetrahydrophthalic acid, hexahydrophthalic acid, maleic acid, fumaric acid, itaconic acid, trimellitic acid, pyromellitic acid, and anhydrides thereof. The polyol is a compound having two or more hydroxyl groups in one molecule, and examples thereof include: diols such as ethylene glycol, propylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 2,2-diethyl-1,3-propanediol, neopentyl glycol, 1,9-nonanediol, 1,4-cyclohexanediol, neopentyl glycol hydroxypivalate, 2-butyl-2-ethyl-1,3-propanediol, 3-methyl-1,5-pentanediol, 2,2,4-trimethylpentanediol, and hydrogenated bisphenol A; and trivalent or higher polyol components such as trimethylolpropane, trimethylolethane, glycerol, and pentaerythritol; and hydroxycarboxylic acids such as 2,2-dimethylolpropionic acid, 2,2-dimethylolbutanoic acid, 2,2-dimethylolpentanoic acid, 2,2-dimethylolhexanoic acid, and 2,2-dimethyloloctanoic acid.
[0112] Alternatively, epoxidized α-olefins such as propylene oxide and butylene oxide, monoepoxy compounds such as Cardura E10 (trade name, manufactured by HEXION Specialty Chemicals, glycidyl ester of synthetic highly branched saturated fatty acid), etc. may be reacted with an acid to introduce these compounds into the polyester resin.
[0113] The introduction of carboxyl groups into the polyester resin can be carried out, for example, by the following methods: after the esterification reaction between the polybasic acid and the polyol, a polybasic acid such as trimellitic acid and trimellitic anhydride and their anhydrides are further reacted; or a method of adding an acid anhydride to a hydroxyl-containing polyester to perform half-esterification.
[0114] In addition, the polyester resin (A2) containing hydroxyl and carboxyl groups may also be a fatty acid-modified polyester resin modified by the following substances: (semi) drying oil fatty acids such as linseed oil fatty acids, coconut oil fatty acids, safflower oil fatty acids, soybean oil fatty acids, sesame oil fatty acids, perilla seed oil fatty acids, hemp oil fatty acids, tall oil fatty acids, dehydrated castor oil fatty acids, etc. The modification amount of these fatty acids is usually preferably 30% by mass or less in terms of oiliness. In addition, the polyester resin (A2) containing hydroxyl and carboxyl groups may be a resin formed by reacting a portion of the polyester resin (A2) with a monobasic acid such as benzoic acid.
[0115] Furthermore, the polyester resin (A2) containing hydroxyl and carboxyl groups may be modified with fatty acid, monoepoxy compound, polyisocyanate compound, acrylic resin or the like during or after the preparation of the resin.
[0116] As the above-mentioned fatty acid, for example, coconut oil fatty acid, cottonseed oil fatty acid, hemp seed oil fatty acid, rice bran oil fatty acid, fish oil fatty acid, tall oil fatty acid, soybean oil fatty acid, linseed oil fatty acid, tung oil fatty acid, rapeseed oil fatty acid, castor oil fatty acid, dehydrated castor oil fatty acid, safflower oil fatty acid, etc. can be listed. In addition, as the above-mentioned monoepoxy compound, for example, "Cardura E10P" (trade name, HEXION company system, synthetic high-branched saturated fatty acid glycidyl ester) can be preferably used.
[0117] In addition, examples of the polyisocyanate compounds include: aliphatic diisocyanate compounds such as lysine diisocyanate, hexamethylene diisocyanate, and trimethylhexane diisocyanate; alicyclic diisocyanate compounds such as hydrogenated xylylene diisocyanate, isophorone diisocyanate, methylcyclohexane-2,4-diisocyanate, methylcyclohexane-2,6-diisocyanate, 4,4'-methylenebis(cyclohexyl isocyanate), and 1,3-(isocyanatomethyl)cyclohexane; aromatic diisocyanate compounds such as toluene diisocyanate, xylylene diisocyanate, and diphenylmethane diisocyanate; organic polyisocyanates such as trivalent or higher polyisocyanates such as lysine triisocyanate; adducts of these organic polyisocyanates with polyols, low molecular weight polyester resins, water, and the like; cyclized polymers (e.g., isocyanurates) and biuret-type adducts between these organic polyisocyanates, and the like. These polyisocyanate compounds may be used alone or in combination of two or more.
[0118] In addition, as a method for modifying the polyester resin (A2) containing hydroxyl groups and carboxyl groups with an acrylic resin, a known method can be used, for example, a method of polymerizing a mixture of a polyester resin containing a polymerizable unsaturated group and a polymerizable unsaturated monomer, a method of achieving the modification by a reaction between a polyester resin containing hydroxyl groups and carboxyl groups and an acrylic resin, etc.
[0119] The hydroxyl value of the polyester resin (A2) containing a hydroxyl group and a carboxyl group is preferably 1 to 250 mgKOH / g, more preferably 2 to 200 mgKOH / g, and even more preferably 5 to 200 mgKOH / g.
[0120] The acid value of the polyester resin (A2) containing a hydroxyl group and a carboxyl group is preferably 1 to 150 mgKOH / g, more preferably 2 to 100 mgKOH / g, and even more preferably 2 to 50 mgKOH / g.
[0121] The weight average molecular weight of the polyester resin (A2) containing a hydroxyl group and a carboxyl group is preferably 3,000 to 100,000, more preferably 4,000 to 50,000, and even more preferably 5,000 to 30,000.
[0122] It should be noted that in this specification, the average molecular weight is a value calculated based on the molecular weight of standard polystyrene according to the chromatogram measured by gel permeation chromatography. The gel permeation chromatograph used is "HLC8120GPC" (manufactured by Tosoh Corporation). As chromatographic columns, four columns "TSKgel G-4000HXL", "TSKgel G-3000HXL", "TSKgel G-2500HXL", and "TSKgel G-2000HXL" (all manufactured by Tosoh Corporation, trade names) were used, and the mobile phase was tetrahydrofuran, the measurement temperature was 40°C, the flow rate was 1 mL / min, and the detector was RI.
[0123] When the aqueous coating composition of the present invention contains the above-mentioned polyester resin (A2) containing hydroxyl groups and carboxyl groups, the content of the polyester resin (A2) containing hydroxyl groups and carboxyl groups is preferably 2 to 70% by mass, more preferably 5 to 50% by mass, and further preferably 5 to 40% by mass, based on the resin solid content in the aqueous coating composition.
[0124] Polyurethane resin containing hydroxyl and carboxyl groups (A3)
[0125] The polyurethane resin (A3) containing hydroxyl and carboxyl groups can be obtained by conventional methods, for example, by reacting a polyol with a polyisocyanate compound. In addition, after the reaction, chain extension can be carried out in the presence of a chain extender such as a diol or a diamine as a low molecular weight compound having at least two active hydrogen atoms in one molecule. In addition, the resin can be modified with an acrylic resin or the like during or after its preparation.
[0126] Examples of polyols not containing a carboxyl group include, for example, diols such as ethylene glycol, diethylene glycol, propylene glycol, butanediol, and hexamethylene glycol as low molecular weight polyols; triols such as trimethylolpropane, glycerol, and pentaerythritol as triols, etc. Examples of polyols having high molecular weights include polyether polyols, polyester polyols, acrylic polyols, and epoxy polyols. Examples of polyether polyols include polyethylene glycol, polypropylene glycol, and polytetramethylene glycol. Examples of polyester polyols include polycondensates of the above-mentioned diols, dipropylene glycol, 1,4-butanediol, 1,6-hexanediol, and neopentyl glycol with dibasic acids such as adipic acid, azelaic acid, and sebacic acid; lactone-based ring-opening polymer polyols such as polycaprolactone; and polycarbonate polyols.
[0127] Examples of the carboxyl group-containing polyol include 2,2-dimethylolpropionic acid and 2,2-dimethylolbutanoic acid, and 2,2-dimethylolpropionic acid is particularly preferred. When these are used, a small amount of a solvent such as N-methylpyrrolidone may be used to rapidly react.
[0128] Examples of the polyisocyanate compound that reacts with the polyol include aliphatic polyisocyanates such as hexamethylene diisocyanate, trimethylhexamethylene diisocyanate, dimer acid diisocyanate, and lysine diisocyanate; and biuret-type adducts and isocyanurate cycloadducts of these polyisocyanates; isophorone diisocyanate, 4,4'-methylenebis(cyclohexyl isocyanate), methylcyclohexane-2,4-(or -2,6-)diisocyanate; alicyclic diisocyanates such as 1,3-(or 1,4-)bis(isocyanatomethyl)cyclohexane, 1,4-cyclohexane diisocyanate, 1,3-cyclopentane diisocyanate, and 1,2-cyclohexane diisocyanate; and biuret-type adducts and isocyanurate cycloadducts of these polyisocyanates; xylylene diisocyanate, m-xylylene diisocyanate, tetramethylxylene diisocyanate, toluene diisocyanate, 4,4'-diphenyl Aromatic diisocyanate compounds such as methylmethane diisocyanate, 1,5-naphthalene diisocyanate, 1,4-naphthalene diisocyanate, 4,4-toluidine diisocyanate, 4,4'-diphenyl ether diisocyanate, (m- or p-)phenylene diisocyanate, 4,4'-biphenyl diisocyanate, 3,3'-dimethyl-4,4'-biphenyl diisocyanate, bis(4-isocyanatophenyl)sulfone, and isopropylidene bis(4-phenylisocyanate); and polyisocyanates thereof Biuret adducts and isocyanurate cycloadducts of isocyanates; polyisocyanates having three or more isocyanate groups in one molecule, such as triphenylmethane-4,4',4"-triisocyanate, 1,3,5-triisocyanatobenzene, 2,4,6-triisocyanatotoluene, and 4,4'-dimethyldiphenylmethane-2,2',5,5'-tetraisocyanate; and biuret adducts and isocyanurate cycloadducts of these polyisocyanate compounds.
[0129] Examples of the diol as the chain extender include ethylene glycol, 1,4-butanediol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, and cyclohexanediol. Examples of the diamine include ethylenediamine, propylenediamine, xylylenediamine, and N-(2-hydroxyethyl)ethylenediamine.
[0130] The hydroxyl value of the polyurethane resin (A3) containing a hydroxyl group and a carboxyl group is preferably 1 to 250 mgKOH / g, more preferably 2 to 200 mgKOH / g, and even more preferably 5 to 200 mgKOH / g.
[0131] From the viewpoint of production stability and water resistance of the obtained coating film, the acid value of the hydroxyl and carboxyl group-containing polyurethane resin (A3) is preferably 1 to 100 mgKOH / g, more preferably 2 to 50 mgKOH / g, and even more preferably 2 to 30 mgKOH / g.
[0132] The weight average molecular weight of the polyurethane resin (A3) containing a hydroxyl group and a carboxyl group is preferably 3,000 or more, more preferably 5,000 or more, and even more preferably 10,000 or more.
[0133] When the aqueous coating composition of the present invention contains the above-mentioned hydroxyl- and carboxyl-containing polyurethane resin (A3), the content of the hydroxyl- and carboxyl-containing polyurethane resin (A3) is preferably 2 to 70% by mass, more preferably 5 to 50% by mass, and further preferably 10 to 40% by mass, based on the resin solid content in the aqueous coating composition.
[0134] Blocked polyisocyanate compound (B)
[0135] The blocked polyisocyanate compound (B) is a compound obtained by blocking the isocyanate groups of the polyisocyanate compound (b1) with a blocking agent (b2).
[0136] Polyisocyanate compound (b1)
[0137] The polyisocyanate compound (b1) is a compound having at least two isocyanate groups in one molecule, and examples thereof include aliphatic polyisocyanates, alicyclic polyisocyanates, aromatic aliphatic polyisocyanates, aromatic polyisocyanates, and derivatives thereof, and any combination thereof.
[0138] Examples of the aliphatic polyisocyanate include trimethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate, pentamethylene diisocyanate, 1,2-propylene diisocyanate, 1,2-butylene diisocyanate, 2,3-butylene diisocyanate, 1,3-butylene diisocyanate, 2,4,4- or 2,2,4-trimethylhexamethylene diisocyanate, dimer acid diisocyanate, 2,6-diisocyanatohexanoic acid methyl ester (common name: aliphatic triisocyanates such as 2,6-diisocyanatohexanoic acid 2-isocyanatoethyl ester, 1,6-diisocyanato-3-isocyanatomethylhexane, 1,4,8-triisocyanatooctane, 1,6,11-triisocyanatoundecane, 1,8-diisocyanato-4-isocyanatomethyloctane, 1,3,6-triisocyanatohexane, 2,5,7-trimethyl-1,8-diisocyanato-5-isocyanatomethyloctane, etc.
[0139] Examples of the alicyclic polyisocyanate include 1,3-cyclopentene diisocyanate, 1,4-cyclohexane diisocyanate, 1,3-cyclohexane diisocyanate, 3-isocyanatomethyl-3,5,5-trimethylcyclohexyl isocyanate (common name: isophorone diisocyanate), 4-methyl-1,3-cyclohexylene diisocyanate (common name: hydrogenated TDI), 2-methyl-1,3-cyclohexylene diisocyanate. , 1,3- or 1,4-bis(isocyanatomethyl)cyclohexane (common name: hydrogenated benzyl diisocyanate) or mixtures thereof, methylenebis(4,1-cyclohexanediyl)diisocyanate (common name: hydrogenated MDI), norbornane diisocyanate and other alicyclic diisocyanates; 1,3,5-triisocyanatocyclohexane, 1,3,5-trimethylisocyanatocyclohexane, 2-(3-isocyanatopropyl)-2,5-di( isocyanatomethyl)-bicyclo(2.2.1)heptane, 2-(3-isocyanatopropyl)-2,6-bis(isocyanatomethyl)-bicyclo(2.2.1)heptane, 3-(3-isocyanatopropyl)-2,5-bis(isocyanatomethyl)-bicyclo(2.2.1)heptane, 5-(2-isocyanatoethyl)-2-isocyanatomethyl-3-(3-isocyanatopropyl)-bicyclo(2.2.1)heptane, 6-( alicyclic triisocyanates such as 2-isocyanatoethyl)-2-isocyanatomethyl-3-(3-isocyanatopropyl)-bicyclo(2.2.1)heptane, 5-(2-isocyanatoethyl)-2-isocyanatomethyl-2-(3-isocyanatopropyl)-bicyclo(2.2.1)heptane, and 6-(2-isocyanatoethyl)-2-isocyanatomethyl-2-(3-isocyanatopropyl)-bicyclo(2.2.1)heptane.
[0140] Examples of the aromatic aliphatic polyisocyanate include aromatic aliphatic diisocyanates such as methylenebis(4,1-phenylene) diisocyanate (common name: MDI), 1,3- or 1,4-phenylenediisocyanate or a mixture thereof, ω,ω'-diisocyanato-1,4-diethylbenzene, 1,3- or 1,4-bis(1-isocyanato-1-methylethyl)benzene (common name: tetramethylphenylenediisocyanate) or a mixture thereof; and aromatic aliphatic triisocyanates such as 1,3,5-triisocyanatotoluene.
[0141] Examples of the aromatic polyisocyanate include: aromatic diisocyanates such as m-phenylene diisocyanate, p-phenylene diisocyanate, 4,4'-diphenyl diisocyanate, 1,5-naphthalene diisocyanate, 2,4-tolylene diisocyanate (common name: 2,4-TDI) or 2,6-tolylene diisocyanate (common name: 2,6-TDI) or a mixture thereof, 4,4'-toluidine diisocyanate, and 4,4'-diphenyl ether diisocyanate; aromatic triisocyanates such as triphenylmethane-4,4',4"-triisocyanate, 1,3,5-triisocyanatobenzene, and 2,4,6-triisocyanatotoluene; and aromatic tetraisocyanates such as 4,4'-diphenylmethane-2,2',5,5'-tetraisocyanate.
[0142] Examples of the derivatives include dimers, trimers, biuret, allophanate, uretdione, uretimine, isocyanurate, oxadiazinetrione, etc., of the polyisocyanates described above, polymethylene polyphenyl polyisocyanate (crude MDI, polymeric MDI), crude TDI, and the like.
[0143] As the polyisocyanate compound (b1), from the perspective that the resulting blocked polyisocyanate compound (B) is less likely to turn yellow when heated, aliphatic diisocyanates, alicyclic diisocyanates and their derivatives are preferred, and from the perspective of improving the flexibility of the formed coating film, aliphatic diisocyanates and their derivatives are more preferred.
[0144] In addition, the polyisocyanate compound (b1) includes a prepolymer produced by reacting aliphatic polyisocyanates, alicyclic polyisocyanates, aromatic aliphatic polyisocyanates, aromatic polyisocyanates, derivatives thereof, and any combination thereof with a compound capable of reacting with the polyisocyanate under the condition that the isocyanate group is excessive. Examples of the compound capable of reacting with the polyisocyanate include compounds having active hydrogen groups such as hydroxyl groups and amino groups, and specifically, examples include polyols, low molecular weight polyester resins, amines, water, and the like.
[0145] The polyisocyanate compound (b1) includes a polymer of an isocyanate group-containing polymerizable unsaturated monomer or a copolymer of the above isocyanate group-containing polymerizable unsaturated monomer and a polymerizable unsaturated monomer other than the above isocyanate group-containing polymerizable unsaturated monomer.
[0146] From the viewpoint of the reactivity of the obtained blocked polyisocyanate compound (B) and the compatibility of the blocked polyisocyanate compound (B) with other coating components, the polyisocyanate compound (b1) may preferably have a number average molecular weight in the range of 300 to 20,000, more preferably a number average molecular weight in the range of 400 to 8,000, and further preferably a number average molecular weight in the range of 500 to 2,000.
[0147] In addition, from the viewpoint of the reactivity of the obtained blocked polyisocyanate compound (B) and the compatibility of the above-mentioned blocked polyisocyanate compound (B) with other coating components, the average number of isocyanate functional groups in one molecule of the polyisocyanate compound (b1) is preferably in the range of 2 to 100. From the viewpoint of improving the reactivity of the obtained blocked polyisocyanate compound (B), the above-mentioned average number of isocyanate functional groups is more preferably 3 or more. From the viewpoint of preventing gelation when producing the blocked polyisocyanate compound (B), the above-mentioned average number of isocyanate functional groups is more preferably 20 or less.
[0148] Capping agent (b2)
[0149] Examples of the blocking agent (b2) for blocking the isocyanate groups in the polyisocyanate compound (b1) include active methylene-based, alcohol-based, phenol-based, oxime-based, amine-based, amide-based, imidazole-based, pyridine-based, and thiol-based blocking agents. These blocking agents can be used alone or in combination of two or more.
[0150] From the viewpoint of low temperature curability, it is preferred that at least a part of the terminal blocking agent (b2) is an active methylene terminal blocking agent, and it is more preferred that the terminal blocking agent is an active methylene terminal blocking agent.
[0151] Examples of the active methylene-based end-capping agent include: malonic acid diesters such as dimethyl malonate, diethyl malonate, di-n-propyl malonate, diisopropyl malonate, di-n-butyl malonate, diisobutyl malonate, di-sec-butyl malonate, di-tert-butyl malonate, di-n-pentyl malonate, di-n-hexyl malonate, di(2-ethylhexyl) malonate, methyl isopropyl malonate, ethyl isopropyl malonate, methyl n-butyl malonate, ethyl n-butyl malonate, methyl isobutyl malonate, ethyl isobutyl malonate, methyl sec-butyl malonate, ethyl sec-butyl malonate, diphenyl malonate, and dibenzyl malonate; and methyl acetoacetate, ethyl acetoacetate, n-butyl malonate, and ethyl acetoacetate. Acetoacetates such as propyl acetoacetate, isopropyl acetoacetate, n-butyl acetoacetate, isobutyl acetoacetate, sec-butyl acetoacetate, tert-butyl acetoacetate, n-pentyl acetoacetate, n-hexyl acetoacetate, 2-ethylhexyl acetoacetate, phenyl acetoacetate and benzyl acetoacetate; isobutyrylacetate such as methyl isobutyrylacetate, ethyl isobutyrylacetate, n-propyl isobutyrylacetate, isopropyl isobutyrylacetate, n-butyl isobutyrylacetate, isobutyl isobutyrylacetate, sec-butyl isobutyrylacetate, tert-butyl isobutyrylacetate, n-pentyl isobutyrylacetate, n-hexyl isobutyrylacetate, 2-ethylhexyl isobutyrylacetate, phenyl isobutyryacetate and benzyl isobutyrylacetate, and any combination thereof.
[0152] As the above-mentioned active methylene-based capping agent, from the viewpoint of smoothness and distinctness of image of the coating film formed from the aqueous coating composition of the present invention, it is preferably at least one compound selected from the group consisting of dimethyl malonate, diethyl malonate, diisopropyl malonate, methyl acetoacetate, ethyl acetoacetate, methyl isobutyrylacetate and ethyl isobutyrylacetate.
[0153] The blocking reaction of the isocyanate group in the polyisocyanate compound (b1) may contain a reaction catalyst as desired. Examples of the reaction catalyst include: metal hydroxides, metal alkoxides, metal carboxylates, metal acetylacetonates, hydroxides of onium salts, onium carboxylates, metal salts of active methylene compounds, onium salts of active methylene compounds, aminosilanes, amines, phosphines and other basic compounds.
[0154] From the viewpoint of the low-temperature curability of the aqueous coating composition of the present invention and the water resistance of the formed coating film, the blocked polyisocyanate compound (B) preferably includes a structure derived from a spacer (b3) having at least two isocyanate-reactive functional groups.
[0155] Spacer (b3)
[0156] The spacer (b3) is a compound having at least two isocyanate-reactive functional groups.
[0157] The functional group is not particularly limited as long as it is a functional group reactive with an isocyanate group. Examples of the isocyanate-reactive functional group include a hydroxyl group, an amino group, a carboxyl group, and a thiol group. Among them, a hydroxyl group and an amino group are preferred, and a hydroxyl group is particularly preferred.
[0158] Therefore, the spacer (b3) is preferably a compound having at least two hydroxyl groups or a compound having at least two amino groups, and among them, a compound having at least two hydroxyl groups is preferred.
[0159] As the compound having at least two hydroxyl groups, for example, as a low molecular weight compound, there can be listed diols such as ethylene glycol, diethylene glycol, propylene glycol, butanediol, and hexamethylene glycol; triols such as trimethylolpropane, glycerol, and pentaerythritol, etc., and as a high molecular weight compound, there can be listed polyether polyols, polyester polyols, acrylic polyols, epoxy polyols, etc. Among them, polyether polyols are preferred from the viewpoint of water resistance and stone chipping resistance of the obtained coating film.
[0160] As the above-mentioned polyether polyol, commercially available products may be used. Examples of the commercially available products include: “PEG#200,” “PEG#300,” “PEG#400,” “PEG#600,” “PEG#1000,” “PEG#1500,” “PEG#1540,” “PEG#2000,” “PEG#4000,” and “PEG#6000” (all manufactured by NOF Corporation, polyethylene glycols); “SANNIX GP250,” “SANNIX GP400,” “SANNIX GP600,” “SANNIX GP1000,” “SANNIX GP1500,” “SANNIX GP3000,” and “SANNIX GP4000” (all manufactured by SANYO Chemical Co., Ltd., polyoxypropylene glyceryl ether); “SANNIX PP200,” “SANNIX PP400,” “SANNIX PP600,” “SANNIX PP950,” “SANNIX PP1000,” “SANNIX PP1200,” “SANNIX PP2000,” and “SANNIX GP4000” (all manufactured by SANYO Chemical Co., Ltd., polyoxypropylene glyceryl ether); PP3000", "SANNIX PP4000" (all manufactured by Sanyo Chemical Co., Ltd., polyoxypropylene glycol), "PTMG250", "PTMG650", "PTMG1000", "PTMG2000", "PTMG3000", "PTMG4000" (all manufactured by Mitsubishi Chemical Co., Ltd., polyoxytetramethylene glycol), etc.
[0161] Furthermore, examples of the compound having at least two amino groups include polyetheramines.
[0162] The polyetheramine may be a commercial product, for example, "JEFFAMINE D-400", "JEFFAMINE D-2000", "JEFFAMINE D-4000", "JEFFAMINE ED-600", "JEFFAMINE ED-900", "JEFFAMINE ED-2003", "ELASTAMINE RT-1000", "JEFFAMINE T-403", "JEFFAMINE T-3000", "JEFFAMINE T-5000" etc. manufactured by HUNTSMAN.
[0163] The molecular weight of the above-mentioned spacer (b3) is preferably in the range of 500 to 6000, more preferably in the range of 800 to 5000, and further preferably in the range of 1000 to 4000, from the viewpoint of the low-temperature curing property of the aqueous coating composition of the present invention and the hardness, stone chipping resistance and water resistance of the formed coating film.
[0164] The number of functional groups of the spacer (b3) is preferably 2 to 3, more preferably 2, from the viewpoint of the storage stability of the aqueous coating composition of the present invention.
[0165] By reacting a part of the isocyanate groups in the polyisocyanate compound (b1) with the spacer (b3), a polyisocyanate compound (b1) containing a structure derived from the spacer (b3) can be formed. In this case, from the perspective of the storage stability of the aqueous coating composition of the present invention, the hardness and water resistance of the formed coating film, and the manufacturing stability of the blocked polyisocyanate compound (B), the ratio of the polyisocyanate compound (b1) to the spacer (b3) is based on 1 mole of isocyanate groups in the polyisocyanate compound (b1), and the number of moles of active hydrogen in the spacer (b3) is preferably in the range of 0.03 to 0.6 moles. By blocking the polyisocyanate compound (b1) containing a structure derived from the spacer (b3), a blocked polyisocyanate compound (B) containing a structure derived from the spacer (b3) can be formed.
[0166] Furthermore, from the viewpoint of storage stability of the aqueous coating composition of the present invention, the blocked polyisocyanate compound (B) may include a structure derived from a hydrophilic group-containing compound (b4) having one isocyanate-reactive functional group.
[0167] Compound containing a hydrophilic group (b4)
[0168] The hydrophilic group-containing compound (b4) has an isocyanate-reactive functional group. Examples of the hydrophilic group-containing compound (b4) include nonionic hydrophilic group-containing compounds, anionic hydrophilic group-containing compounds, and cationic hydrophilic group-containing compounds, and any combination thereof. The hydrophilic group-containing compound (b4) is preferably a nonionic hydrophilic group-containing compound because it is not easy to hinder the reaction of blocking the isocyanate groups in the polyisocyanate compound (b1) by the above-mentioned blocking agent (b2).
[0169] As the above-mentioned nonionic compound containing a hydrophilic group, for example, a compound having a polyoxyalkylene group can be listed. As the above-mentioned polyoxyalkylene group, for example, polyoxyethylene, polyoxypropylene, polyoxyethyleneoxypropylene, etc. can be listed. From the viewpoint of the storage stability of the aqueous coating composition of the present invention, the above-mentioned nonionic compound containing a hydrophilic group preferably has a polyoxyethylene group.
[0170] From the viewpoint of storage stability of the aqueous coating composition of the present invention and water resistance of the formed coating film, the compound having a polyoxyethylene group preferably has 3 or more, preferably 5 to 100, more preferably 8 to 45 continuous polyoxyethylene groups, i.e., polyoxyethylene blocks.
[0171] Furthermore, the compound having a polyoxyethylene group may contain an oxyalkylene group other than the polyoxyethylene block, and examples of the oxyalkylene group other than the oxyethylene group include an oxypropylene group, an oxybutylene group, and an oxyphenylene group.
[0172] From the viewpoint of storage stability of the water-based coating composition of the present invention, the molar ratio of the oxyethylene in the above-mentioned compound having polyoxyethylene is preferably in the range of 20 to 100 mol %, and more preferably in the range of 50 to 100 mol %. If the molar ratio of the oxyethylene in the oxyalkylene is 20 mol % or more, the imparting of hydrophilicity becomes sufficient, and the storage stability of the water-based coating composition of the present invention becomes good.
[0173] In addition, from the viewpoint of the storage stability of the aqueous coating composition of the present invention and the water resistance of the formed coating film, the number average molecular weight of the nonionic hydrophilic group-containing compound is preferably in the range of 200 to 2000. From the viewpoint of the storage stability of the aqueous coating composition of the present invention, the number average molecular weight is more preferably 300 or more, and further preferably 400 or more. From the viewpoint of the water resistance of the coating film formed by the aqueous coating composition of the present invention, the number average molecular weight is more preferably 1500 or less, and further preferably 1200 or less.
[0174] Examples of the nonionic hydrophilic group-containing compound include polyethylene glycol monoalkyl ethers (also known as ω-alkoxypolyoxyethylene) such as polyethylene glycol monomethyl ether and polyethylene glycol monoethyl ether; polypropylene glycol monoalkyl ethers (also known as ω-alkoxypolyoxypropylene) such as polypropylene glycol monomethyl ether and polypropylene glycol monoethyl ether; ω-alkoxypolyoxyethylene (oxypropylene) such as ω-methoxypolyoxyethylene (oxypropylene) and ω-ethoxypolyoxyethylene (oxypropylene); polyethylene glycol (propylene glycol) monoalkyl ethers such as polyethylene glycol (propylene glycol) monomethyl ether and polyethylene glycol (propylene glycol) monoethyl ether, and any combination thereof.
[0175] As the above-mentioned nonionic hydrophilic group-containing compound, polyethylene glycol monomethyl ether and polyethylene glycol monoethyl ether are preferred, and polyethylene glycol monomethyl ether is further preferred.
[0176] It should be noted that, in the present specification, "polyethylene glycol (propylene glycol)" refers to a copolymer of ethylene glycol and propylene glycol, including a block copolymer and a random copolymer.
[0177] Examples of commercially available products of the polyethylene glycol monomethyl ether include "UNIOX M-400", "UNIOX M-550", "UNIOX M-1000" and "UNIOX M-2000" manufactured by NOF Corporation.
[0178] By reacting a part of the isocyanate groups in the polyisocyanate compound (b1) with the hydrophilic group-containing compound (b4), a polyisocyanate compound (b1) containing a structure derived from the hydrophilic group-containing compound (b4) can be formed. In this case, from the viewpoint of the storage stability of the aqueous coating composition of the present invention and the adhesion, smoothness, distinctness of image, water resistance, stone chipping resistance, and glass adhesion of the formed coating film, the ratio of the polyisocyanate compound (b1) to the hydrophilic group-containing compound (b4) is based on 1 mole of isocyanate groups in the polyisocyanate compound (b1), and the number of moles of active hydrogen in the hydrophilic group-containing compound (b4) is preferably in the range of 0.03 to 0.6 moles. By blocking the polyisocyanate compound (b1) containing a structure derived from the hydrophilic group-containing compound (b4), a blocked polyisocyanate compound (B) containing a structure derived from the hydrophilic group-containing compound (b4) can be formed.
[0179] When the isocyanate groups in the polyisocyanate compound (b1) are reacted with the blocking agent (b2) and the spacer (b3) and / or the hydrophilic group-containing compound (b4), the order of the reactions is not particularly limited.
[0180] Specifically, examples include: a method in which a part of the isocyanate groups in the polyisocyanate compound (b1) is reacted with a spacer (b3) and / or a hydrophilic group-containing compound (b4), and then the remaining isocyanate groups are blocked with a blocking agent (b2); a method in which a part of the isocyanate groups in the polyisocyanate compound (b1) is blocked with a blocking agent (b2), and then the remaining isocyanate groups are reacted with a spacer (b3) and / or a hydrophilic group-containing compound (b4); and a method in which the isocyanate groups in the polyisocyanate compound (b1) are reacted simultaneously with a blocking agent (b2), a spacer (b3) and / or a hydrophilic group-containing compound (b4).
[0181] From the viewpoints of production stability and water resistance and hardness of the formed coating film, the weight average molecular weight of the blocked polyisocyanate compound (B) is preferably in the range of 3,000 to 200,000, more preferably in the range of 10,000 to 150,000, and further preferably in the range of 30,000 to 120,000.
[0182] The content of the blocked polyisocyanate compound (B) is preferably 2 to 70% by mass, more preferably 5 to 50% by mass, and even more preferably 10 to 40% by mass based on the resin solid content in the aqueous coating composition.
[0183] Polycarbodiimide compound (C)
[0184] The polycarbodiimide compound (C) is a compound having at least two carbodiimide groups in one molecule, and for example, a compound obtained by subjecting isocyanate groups of an isocyanate group-containing compound to a decarbonation reaction can be used.
[0185] As the polycarbodiimide compound (C), a water-soluble or water-dispersible polycarbodiimide compound is preferably used from the viewpoint of excellent storage stability, forming a coating film showing excellent coating properties such as high hardness and water resistance, and good glass adhesion. As the water-soluble or water-dispersible polycarbodiimide compound, any polycarbodiimide compound that can be stably dissolved or dispersed in an aqueous medium can be used without particular limitation.
[0186] Specific examples of the water-soluble polycarbodiimide compound include "CARBODILITE SV-02", "CARBODILITE V-02", "CARBODILITE V-02-L2", "CARBODILITE V-04" (all trade names, manufactured by Nisshinbo Co., Ltd.). In addition, examples of the water-dispersible polycarbodiimide compound include "CARBODILITE E-01", "CARBODILITE E-02", "CARBODILITE E-05" (all trade names, manufactured by Nisshinbo Co., Ltd.).
[0187] The content of the polycarbodiimide compound (C) is preferably 1 to 20% by mass, more preferably 2 to 15% by mass, and even more preferably 3 to 10% by mass, based on the resin solid content in the aqueous coating composition.
[0188] Basic compounds (D)
[0189] The basic compound (D) is a compound used to neutralize the carboxyl group of the hydroxyl- and carboxyl-containing resin (A) and to adjust the pH of the aqueous coating composition. Therefore, compounds that chemically react with other functional groups, such as the diamine of the chain extender described in the description column of the hydroxyl- and carboxyl-containing polyurethane resin (A3), are excluded.
[0190] The content of the basic compound (D) can be set to an amount in which the pH of the aqueous coating composition of the present invention is within the range of 8.0 to 11.5. The content of the basic compound (D) is preferably 0.1 to 15% by mass, more preferably 0.5 to 10% by mass, and further preferably 1 to 8% by mass based on the resin solid content in the aqueous coating composition.
[0191] In the present invention, the basic compound (D) contains (D1) a basic compound having an acid dissociation constant (PKa) in the range of 7.0 to 8.5 and a boiling point in the range of 100 to 200° C., and the content of the basic compound (D1) is in the range of 30 to 100% by mass based on the mass of the basic compound (D).
[0192] Basic compounds (D1)
[0193] The acid dissociation constant (PKa) of the basic compound (D1) is in the range of 7.0 to 8.5 and the boiling point is in the range of 100 to 200°C.
[0194] When the acid dissociation constant (PKa) is 7.0 or more, an aqueous coating composition having excellent storage stability can be obtained, and when the acid dissociation constant (PKa) is 8.5 or less, an aqueous coating composition having excellent hardness and water resistance of the formed coating film can be obtained.
[0195] Among them, the acid dissociation constant (PKa) of the basic compound (D1) is preferably in the range of 7.2 to 8.2, more preferably in the range of 7.3 to 7.8.
[0196] When the boiling point is 100° C. or higher, an aqueous coating composition having excellent storage stability can be obtained, and when the boiling point is 200° C. or lower, an aqueous coating composition having excellent hardness and water resistance of the formed coating film can be obtained.
[0197] Among them, the boiling point of the basic compound (D1) is preferably in the range of 105 to 180°C, more preferably in the range of 110 to 160°C.
[0198] Examples of the basic compound (D1) include morpholine (PKa 8.4, boiling point 129° C.), allylmorpholine (PKa 7.1, boiling point 158° C.), N-methylmorpholine (PKa 7.4, boiling point 116° C.), N-ethylmorpholine (PKa 7.7, boiling point 139° C.), triallylamine (PKa 8.3, boiling point 156° C.), etc. These may be used alone or in combination of two or more.
[0199] As the above-mentioned basic compound (D1), from the viewpoint of the storage stability of the aqueous coating composition of the present invention, the hardness and water resistance of the formed coating film, it is preferred to use N-methylmorpholine (PKa 7.4, boiling point 116°C) or N-ethylmorpholine (PKa 7.7, boiling point 139°C).
[0200] The content of the basic compound (D1) in the aqueous coating composition of the present invention is in the range of 30 to 100% by mass based on the mass of the basic compound (D).
[0201] When the content of the basic compound (D1) in the aqueous coating composition of the present invention is 30% by mass or more, an aqueous coating composition excellent in storage stability, hardness and water resistance of the formed coating film, and glass adhesion can be obtained.
[0202] The content of the basic compound (D1) in the aqueous coating composition of the present invention is preferably in the range of 35 to 90% by mass, more preferably in the range of 35 to 80% by mass, based on the mass of the basic compound (D).
[0203] Examples of the basic compound (D) other than the basic compound (D1) include ammonia, triethylamine, triethanolamine, 2-(dimethylamino)ethanol, and diethylethanolamine.
[0204] The reason why the aqueous coating composition of the present invention has excellent storage stability and can form a coating film showing excellent coating properties such as high hardness and water resistance and good glass adhesion even when cured at a relatively low temperature is not clear, but it is speculated that: the acid dissociation constant (PKa) of the alkaline compound (D1) is greater than 7.0, so the carboxyl group of the hydroxyl- and carboxyl-containing resin (A) can be neutralized, and the storage stability becomes good. In addition, the acid dissociation constant (PKa) of the alkaline compound (D1) is less than 8.5, so it will not hinder the reaction of the hydroxyl- and carboxyl-containing resin (A) with the blocked polyisocyanate compound (B) and the reaction of the hydroxyl- and carboxyl-containing resin (A) with the polycarbodiimide compound (C), and can form a coating film showing excellent coating properties and good glass adhesion. It is also speculated that the boiling point of the basic compound (D1) is 100°C or higher, so the amount of volatilization of the basic compound (D1) during storage of the aqueous coating composition of the present invention is small, and the storage stability becomes good. In addition, the boiling point of the basic compound (D1) is 200°C or lower, so the amount of volatilization of the basic compound (D1) during heat curing becomes large, and the reaction of the hydroxyl- and carboxyl-containing resin (A) with the blocked polyisocyanate compound (B) and the reaction of the hydroxyl- and carboxyl-containing resin (A) with the polycarbodiimide compound (C) is not hindered, and a coating film showing excellent coating performance and good glass adhesion can be formed. It is also speculated that by adjusting the pH of the aqueous coating composition to a higher range within the range of 8.0 to 11.5, the carboxyl group of the hydroxyl- and carboxyl-containing resin (A) is neutralized, thereby suppressing the reaction of the carbodiimide compound (C) and the storage stability becomes good.
[0205] Melamine resin (E)
[0206] The aqueous coating composition of the present invention may further contain a melamine resin (E).
[0207] As the melamine resin (E), a partially methylolated melamine resin or a completely methylolated melamine resin obtained by a reaction between a melamine component and an aldehyde component can be used. Examples of the aldehyde component include formaldehyde, paraformaldehyde, acetaldehyde, and benzaldehyde.
[0208] In addition, the methylol groups of the methylolated melamine resin may be partially or completely etherified with a suitable alcohol. Examples of the alcohol used for etherification include methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, 2-ethyl-1-butanol, and 2-ethyl-1-hexanol.
[0209] The melamine resin (E) is preferably a methyl-etherified melamine resin obtained by partially or completely etherifying the methylol groups of a partially or completely methylolated melamine resin with methanol, a butyl-etherified melamine resin obtained by partially or completely etherifying the methylol groups of a partially or completely methylolated melamine resin with butanol, or a methyl-butyl mixed etherified melamine resin obtained by partially or completely etherifying the methylol groups of a partially or completely methylolated melamine resin with methanol and butanol, and more preferably a methyl-butyl mixed etherified melamine resin.
[0210] The weight average molecular weight of the melamine resin (B) is preferably 400 to 6,000, more preferably 500 to 4,000, and further preferably 600 to 3,000.
[0211] As the melamine resin (E), a commercially available item can be used. Examples of the trade names of commercially available products include: “CYMEL 202,” “CYMEL 203,” “CYMEL 204,” “CYMEL 211,” “CYMEL 212,” “CYMEL 238,” “CYMEL 251,” “CYMEL 253,” “CYMEL 254,” “CYMEL 303,” “CYMEL 323,” “CYMEL 324,” “CYMEL 325,” “CYMEL 327,” “CYMEL 350,” “CYMEL 370,” “CYMEL 380,” “CYMEL 385,” “CYMEL 1156,” “CYMEL 1158,” “CYMEL 1116,” and “CYMEL 1130” (all manufactured by Allnex Japan Co., Ltd.); 745", "Resimene746", "Resimene 747" (the above, made by MONSANTO); "U-VAN 120", "U-VAN 20HS", "U-VAN20SE", "U-VAN 2021", "U-VAN 2028", "U-VAN 28-60" (above, manufactured by Mitsui Chemicals Co., Ltd.); "Sumimal M55", "Sumimal M30W", "Sumimal M50W" (above, manufactured by Sumitomo Chemical Co., Ltd.); etc.
[0212] When the aqueous coating composition of the present invention contains the melamine resin (E), the content of the melamine resin (E) is preferably 1 to 30% by mass, more preferably 2 to 20% by mass, and even more preferably 3 to 15% by mass based on the resin solid content in the aqueous coating composition.
[0213] Other Ingredients
[0214] The aqueous coating composition of the present invention may further contain resins other than those mentioned above, pigments, organic solvents, curing catalysts, dispersants, anti-settling agents, defoamers, thickeners, ultraviolet absorbers, light stabilizers, surface conditioners, etc. as necessary.
[0215] As resins other than the above, for example, acrylic resins containing no hydroxyl group and / or carboxyl group, polyester resins containing no hydroxyl group and / or carboxyl group, polyurethane resins containing no hydroxyl group and / or carboxyl group, polyether resins containing no hydroxyl group and / or carboxyl group, polycarbonate resins containing no hydroxyl group and / or carboxyl group, epoxy resins containing no hydroxyl group and / or carboxyl group, etc. can be listed. Among them, polyurethane resins containing no hydroxyl group and carboxyl group are preferably used.
[0216] The above-mentioned hydroxyl-free carboxyl-containing polyurethane resin can be obtained by conventional methods, for example, by reacting a polyol with a polyisocyanate. In addition, after the reaction, the chain can be extended in the presence of a chain extender such as a diol or a diamine as a low molecular weight compound having at least two active hydrogen atoms in one molecule. In addition, the resin can be modified with an acrylic resin or the like during or after its preparation.
[0217] As the polyol, polyisocyanate and chain extender, the compounds described in the description column of the hydroxyl group- and carboxyl group-containing polyurethane resin (A3) can be used.
[0218] Examples of the pigment include coloring pigments, extender pigments, and bright pigments. These pigments may be used alone or in combination of two or more.
[0219] When the aqueous coating composition of the present invention contains the above-mentioned pigment, the amount of the pigment added may preferably be in the range of 1 to 200 parts by mass, more preferably 5 to 160 parts by mass, and further preferably 15 to 140 parts by mass, based on 100 parts by mass of the resin solid content in the aqueous coating composition of the present invention.
[0220] Examples of the coloring pigment include titanium oxide, zinc oxide, carbon black, molybdenum red, Prussian blue, cobalt blue, azo pigments, phthalocyanine pigments, quinacridone pigments, isoindolinone pigments, threne pigments, perylene pigments, dioxazine pigments, and diketopyrrolopyrrole pigments.
[0221] When the aqueous coating composition of the present invention contains the above-mentioned coloring pigment, the amount of the coloring pigment added may preferably be in the range of 1 to 180 parts by mass, more preferably 5 to 150 parts by mass, and further preferably 15 to 130 parts by mass, based on 100 parts by mass of the resin solid content in the aqueous coating composition of the present invention.
[0222] Examples of the extender pigment include barium sulfate, talc, clay, kaolin, barium carbonate, calcium carbonate, silicon dioxide, and alumina white. As the extender pigment, barium sulfate can be preferably used from the viewpoint of improving design properties.
[0223] When the aqueous coating composition of the present invention contains the above-mentioned extender pigment, the amount of the extender pigment blended is preferably 1 to 180 parts by mass, more preferably 5 to 140 parts by mass, and further preferably 10 to 120 parts by mass based on 100 parts by mass of the resin solid content in the aqueous coating composition of the present invention.
[0224] Examples of the bright pigment include aluminum (including vapor-deposited aluminum), copper, zinc, brass, nickel, glass flakes, aluminum oxide, mica, aluminum oxide coated with titanium oxide and / or iron oxide, and mica coated with titanium oxide and / or iron oxide. Among them, aluminum pigments are preferably used. Aluminum pigments include non-leafing aluminum pigments and leafing aluminum pigments, and both can be used.
[0225] The bright pigment is preferably in the form of flakes. In addition, the bright pigment preferably has a length dimension in the range of 1 to 100 μm, particularly preferably in the range of 5 to 40 μm, and a thickness in the range of 0.001 to 5 μm, particularly preferably in the range of 0.01 to 2 μm.
[0226] When the aqueous coating composition of the present invention contains the above-mentioned bright pigment, the amount of the bright pigment added may preferably be in the range of 0.1 to 100 parts by mass, more preferably 1 to 50 parts by mass, and further preferably 3 to 25 parts by mass, based on 100 parts by mass of the resin solid content in the aqueous coating composition of the present invention.
[0227] Examples of the organic solvent include ketone solvents such as acetone, methyl ethyl ketone, and methyl isobutyl ketone; ester solvents such as ethyl acetate, butyl acetate, methyl benzoate, ethyl ethoxypropionate, ethyl propionate, and methyl propionate; alcohol solvents such as isopropyl alcohol, n-butanol, isobutyl alcohol, and 2-ethylhexanol; ether solvents such as tetrahydrofuran, dioxane, and dimethoxyethane; glycol ether solvents such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, and 3-methoxybutyl acetate; aromatic hydrocarbon solvents, aliphatic hydrocarbon solvents, and the like.
[0228] Specifically, as the curing catalyst, for example, organic metal compounds such as tin octylate, dibutyltin diacetate, dibutyltin di(2-ethylhexanoate), dibutyltin dilaurate, dioctyltin diacetate, dioctyltin di(2-ethylhexanoate), dibutyltin oxide, dibutyltin sulfide, dioctyltin oxide, dibutyltin fatty acid salt, lead 2-ethylhexanoate, zinc octylate, zinc naphthenate, fatty acid zincs, bismuth octylate, bismuth 2-ethylhexanoate, bismuth oleate, bismuth neodecanoate, bismuth versatate, bismuth naphthenate, cobalt naphthenate, calcium octylate, copper naphthenate, and tetra(2-ethylhexyl) titanate; sulfonic acid group-containing compounds such as p-toluenesulfonic acid, dodecylbenzenesulfonic acid, and dinonylnaphthalenesulfonic acid; and phosphoric acid group-containing compounds such as monobutyl phosphate, dibutyl phosphate, mono-2-ethylhexyl phosphate, di-2-ethylhexyl phosphate, alkyl ether phosphoric acid, polyoxyethylene alkyl ether phosphoric acid, and phosphoric acid group-containing resins can be used. Among them, from the viewpoint of storage stability of the aqueous coating composition and water resistance and stone chipping resistance of the formed coating film, a phosphoric acid group-containing compound is preferred, a phosphoric acid group-containing resin is more preferred, and a phosphoric acid group-containing acrylic resin is further preferred.
[0229] The phosphoric acid group-containing acrylic resin can be synthesized by copolymerizing a polymerizable unsaturated monomer having a phosphoric acid group and other polymerizable unsaturated monomers by a conventional method.
[0230] In the phosphoric acid group-containing acrylic resin, the polymerizable unsaturated monomer having a phosphoric acid group is preferably 1 to 50% by mass, particularly preferably 5 to 40% by mass, based on the total amount of monomer components constituting the phosphoric acid group-containing acrylic resin.
[0231] From the viewpoint of finished product appearance and coating film performance, the weight average molecular weight of the phosphoric acid group-containing acrylic resin is preferably in the range of 3,000 to 30,000, more preferably in the range of 5,000 to 25,000, and further preferably in the range of 10,000 to 20,000.
[0232] When a phosphoric acid group-containing compound is used as a curing catalyst, the content thereof is preferably 0.1 to 20% by mass, more preferably 0.5 to 15% by mass, and even more preferably 1 to 10% by mass based on the resin solid content in the aqueous coating composition.
[0233] The aqueous coating composition of the present invention can be used for coating by adding water and / or an organic solvent or the like to dilute the composition as necessary and adjusting the viscosity to an appropriate level.
[0234] The appropriate viscosity varies depending on the coating composition, but when adjusted using a No. 4 Ford cup viscometer, for example, the viscosity can generally be about 20 to 100 seconds at 20° C., preferably about 25 to 70 seconds.
[0235] Furthermore, the coating solid content concentration of the aqueous coating composition of the present invention is usually preferably about 5 to 70% by mass, and more preferably about 10 to 55% by mass.
[0236] The aqueous coating composition of the present invention may be either a one-component coating or a multi-component coating, but is preferably a one-component coating from the viewpoints of not requiring a coating mixing step, being excellent in productivity, and being able to simplify the maintenance of coating machinery.
[0237] The water-based coating composition of the present invention can be applied to the object to be coated by a method known per se, such as by air spray coating, airless spray coating, rotary atomization coating, curtain coating, etc. During coating, electrostatic application can also be performed. Among them, air spray coating and rotary atomization coating are preferred. In addition, the above-mentioned coating method can be performed once or divided into multiple times to obtain the desired film thickness.
[0238] The coating amount of the aqueous coating composition of the present invention is usually an amount that gives a cured film thickness of 5 to 40 μm, preferably 7 to 35 μm, and more preferably 10 to 30 μm.
[0239] Multilayer coating film forming method
[0240] The water-based coating composition of the present invention can form a coating film showing excellent coating properties such as high hardness and water resistance and good glass adhesion even when cured at a relatively low temperature, and therefore, can be preferably used as a mid-coat coating composition. This coating can be particularly preferably used as a coating for automobiles.
[0241] As a method for forming a multilayer coating film by applying the present coating material in the form of a mid-coat coating composition, for example, the following method can be preferably used.
[0242] A method for forming a multilayer coating film, which sequentially carries out the following steps: step (1): a step of applying the aqueous coating composition of the present invention on a coated object to form a mid-coat film; step (2): a step of applying an aqueous base coating composition on the mid-coat film formed in the step (1) to form a base coating film; step (3): a step of applying a clear coating composition on the base coating film formed in the step (2) to form a clear coating film; and step (4): a step of simultaneously heating and curing the mid-coat film, base coating film and clear coating film formed in the steps (1) to (3) at a temperature in the range of 60 to 110°C.
[0243] Examples of the coated object include: outer panels of automobile bodies such as cars, trucks, motorcycles, and buses; automobile parts; and outer panels of home appliances such as mobile phones and audio equipment. Among them, outer panels of automobile bodies and automobile parts are preferred.
[0244] The materials of these coated objects are not particularly limited. For example, metal materials such as iron, aluminum, brass, copper, tin plate, stainless steel, galvanized steel, zinc alloy (Zn-Al, Zn-Ni, Zn-Fe, etc.) steel; resins such as polyethylene resin, polypropylene resin, acrylonitrile-butadiene-styrene (ABS) resin, polyamide resin, acrylic resin, vinylidene chloride resin, polycarbonate resin, polyurethane resin, epoxy resin; plastic materials such as various FRP (fiber reinforced polymer); inorganic materials such as glass, cement, concrete; wood; fiber materials such as paper and cloth, etc. Among them, metal materials and plastic materials are preferred.
[0245] In addition, the surface of the object to which the coating film is applied may be a surface of a metal substrate such as an automobile body panel, automobile parts, home appliances, or steel plates constituting them, which has been subjected to surface treatment such as phosphate treatment, chromate treatment, or composite oxide treatment.
[0246] A coating film may be further formed on an object that has been subjected to or has not been subjected to a surface treatment. For example, a coating object as a substrate may be subjected to a surface treatment as required to form a primer coating film thereon. For example, when the coating object is a car body, the primer coating film may be formed using a primer coating material that is known per se and is commonly used in the painting of car bodies.
[0247] As the primer coating material for forming the primer coating film, for example, an electrodeposition coating material can be used, and a cationic electrodeposition coating material is preferably used.
[0248] As the above-mentioned water-based base coating composition, a material obtained by coating a base resin such as acrylic resin, polyester resin, alkyd resin, urethane resin, epoxy resin, etc. having cross-linking functional groups such as carboxyl and hydroxyl groups; as well as an amino resin such as melamine resin and urea resin, a cross-linking agent such as an optionally blocked polyisocyanate compound, a pigment, a thickener, and optionally other ingredients can be used.
[0249] As the above-mentioned clear coating composition, any thermosetting clear coating composition known for coating automobile bodies, etc. can be used. Examples of the thermosetting clear coating composition include organic solvent-based thermosetting coating compositions containing a base resin having a crosslinkable functional group and a curing agent, water-based thermosetting coating compositions, and powder thermosetting coating compositions.
[0250] Examples of the crosslinkable functional group possessed by the base resin include carboxyl, hydroxyl, epoxy, and silanol groups. Examples of the type of the base resin include acrylic resins, polyester resins, alkyd resins, urethane resins, epoxy resins, and fluororesins. Examples of the curing agent include polyisocyanate compounds, blocked polyisocyanate compounds, melamine resins, urea-formaldehyde resins, carboxyl-containing compounds, carboxyl-containing resins, epoxy-containing resins, and epoxy-containing compounds.
[0251] As the combination of base resin / curing agent of the above-mentioned clear coating composition, preferred are hydroxyl-containing resin / polyisocyanate compound, carboxyl-containing resin / epoxy-containing resin, hydroxyl-containing resin / blocked polyisocyanate compound, hydroxyl-containing resin / melamine resin, etc., and hydroxyl-containing resin / polyisocyanate compound is more preferred.
[0252] The clear coating composition may be a one-component coating or a multi-component coating such as a two-component urethane resin coating.
[0253] In addition, the above-mentioned clear coating composition may contain coloring pigments, bright pigments, dyes, etc. as needed to the extent that transparency is not impaired, and may also appropriately contain extender pigments, ultraviolet absorbers, light stabilizers, defoamers, thickeners, rust inhibitors, surface conditioners, etc.
[0254] The coating method of the clear coating composition is not particularly limited, for example, a wet coating film can be formed by a coating method such as air spray coating, airless spray coating, rotary atomization coating, curtain coating, etc. In these coating methods, electrostatic application can also be performed as required. Among them, air spray coating or rotary atomization coating is particularly preferred. The coating amount of the clear coating composition can usually be set to a cured film thickness of 10 to 70 μm, preferably an amount of 20 to 50 μm.
[0255] In addition, when air spray coating, airless spray coating and rotary atomization coating are performed, it is preferred that the viscosity of the clear coating composition is appropriately adjusted in advance using a solvent such as an organic solvent to a viscosity range suitable for the coating, usually appropriately adjusted to a viscosity range of about 15 seconds to 60 seconds, particularly about 20 seconds to 50 seconds, at 20° C. in a No. 4 Ford cup viscometer.
[0256] The heating can be performed by a known means, for example, a drying furnace such as a hot air furnace, an electric furnace, an infrared induction heating furnace, etc. The heating temperature is in the range of 60 to 110° C., preferably in the range of 70 to 90° C. The heating time is not particularly limited, but is preferably in the range of 10 to 40 minutes, more preferably in the range of 20 to 40 minutes.
[0257] Example
[0258] Hereinafter, manufacturing examples, embodiments and comparative examples are listed to further specifically describe the present invention. It should be noted that these manufacturing examples, embodiments and comparative examples are only for illustration and are not intended to limit the scope of the present invention. In manufacturing examples, embodiments and comparative examples, "parts" and "%" are all weight references unless otherwise specified. In addition, the film thickness of the coating film is based on the film thickness of the cured coating film.
[0259] Production of hydroxyl- and carboxyl-containing resin (A)
[0260] Production of hydroxyl- and carboxyl-containing acrylic resin particles (A1′) having a core-shell structure Production Example 1
[0261] Into a reaction container equipped with a thermometer, a thermostat, a stirrer, a reflux condenser, a nitrogen inlet tube and a dropping device, 130 parts of deionized water and 0.52 parts of "Aqualon KH-10" (trade name, manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd., emulsifier, active ingredient 97%) were placed, stirred and mixed in a nitrogen flow, and the temperature was raised to 80°C.
[0262] Next, 1.72 parts of the following monomer emulsion (1) and 5.3 parts of a 6% aqueous solution of ammonium persulfate were introduced into a reaction container and maintained at 80°C for 15 minutes. Then, the remaining monomer emulsion (1) was added dropwise to the reaction container maintained at this temperature over 3 hours, and the mixture was aged for 1 hour after the addition was completed. Then, the following monomer emulsion (2) was added dropwise over 1 hour, and after aging for 1 hour, 20 parts of a 5% aqueous solution of N-ethylmorpholine was slowly added to the reaction container while cooling to 30°C, and the mixture was discharged while filtering with a 100-mesh nylon cloth, thereby obtaining hydroxyl- and carboxyl-containing acrylic resin particles (A1'-1) having a solid content concentration of 30%. The obtained hydroxyl- and carboxyl-containing acrylic resin particles (A1'-1) had an acid value of 16 mgKOH / g, a hydroxyl value of 66 mgKOH / g, and a glass transition temperature of 21°C.
[0263] Monomer emulsion (1): 42 parts of deionized water, 0.72 parts of "Aqualon KH-10", 2 parts of methylenebisacrylamide, 5 parts of styrene, 15 parts of methyl methacrylate, 5 parts of 2-hydroxyethyl methacrylate and 23 parts of n-butyl acrylate were mixed and stirred to obtain a monomer emulsion (1).
[0264] Monomer emulsion (2): 42 parts of deionized water, 0.72 parts of "Aqualon KH-10", 0.05 parts of ammonium persulfate, 2.5 parts of methacrylic acid, 10 parts of 2-hydroxyethyl methacrylate, 5 parts of styrene, 12.5 parts of methyl methacrylate, 10 parts of n-butyl acrylate and 10 parts of n-butyl methacrylate were mixed and stirred to obtain a monomer emulsion (2).
[0265] Production Example 2
[0266] Into a reaction container equipped with a thermometer, a thermostat, a stirrer, a reflux condenser, a nitrogen inlet tube and a dropping device, 130 parts of deionized water and 0.52 parts of "Aqualon KH-10" (trade name, manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd., emulsifier, active ingredient 97%) were placed, stirred and mixed in a nitrogen flow, and the temperature was raised to 80°C.
[0267] Next, 1.72 parts of the following monomer emulsion (1) and 5.3 parts of a 6% aqueous solution of ammonium persulfate were introduced into a reaction container and maintained at 80°C for 15 minutes. Then, the remaining monomer emulsion (1) was added dropwise to the reaction container maintained at this temperature over 3 hours, and the mixture was aged for 1 hour after the addition was completed. Then, the following monomer emulsion (2) was added dropwise over 1 hour, and after aging for 1 hour, 20 parts of a 5% aqueous solution of 2-(dimethylamino)ethanol was slowly added to the reaction container while cooling to 30°C, and the mixture was discharged while filtering with a 100-mesh nylon cloth, thereby obtaining hydroxyl- and carboxyl-containing acrylic resin particles (A1'-2) having a solid content concentration of 30%. The obtained hydroxyl- and carboxyl-containing acrylic resin particles (A1'-2) had an acid value of 16 mgKOH / g, a hydroxyl value of 66 mgKOH / g, and a glass transition temperature of 21°C.
[0268] Monomer emulsion (1): 42 parts of deionized water, 0.72 parts of "Aqualon KH-10", 2 parts of methylenebisacrylamide, 5 parts of styrene, 15 parts of methyl methacrylate, 5 parts of 2-hydroxyethyl methacrylate and 23 parts of n-butyl acrylate were mixed and stirred to obtain a monomer emulsion (1).
[0269] Monomer emulsion (2): 42 parts of deionized water, 0.72 parts of "Aqualon KH-10", 0.05 parts of ammonium persulfate, 2.5 parts of methacrylic acid, 10 parts of 2-hydroxyethyl methacrylate, 5 parts of styrene, 12.5 parts of methyl methacrylate, 10 parts of n-butyl acrylate and 10 parts of n-butyl methacrylate were mixed and stirred to obtain a monomer emulsion (2).
[0270] Preparation of hydroxyl- and carboxyl-containing acrylic resin particles (A1") having a core-shell structure and comprising a gradient polymer layer
[0271] Production Example 3
[0272] Into a reaction container equipped with a thermometer, a thermostat, a stirrer, a reflux condenser, a nitrogen inlet tube and a dropping device, 130 parts of deionized water and 0.52 parts of "Aqualon KH-10" (trade name, manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd., emulsifier, active ingredient 97%) were placed, stirred and mixed in a nitrogen flow, and the temperature was raised to 80°C.
[0273] Next, 1.72 parts of the following monomer emulsion (1) and 5.3 parts of a 6% ammonium persulfate aqueous solution were introduced into the reaction container and maintained at 80°C for 15 minutes. Then, 35.4 parts of the monomer emulsion (1) were added dropwise to the reaction container maintained at this temperature over 1 hour, and immediately after the addition was completed, the remaining 55.6 parts of the monomer emulsion (1) was added dropwise to the reaction container. At the same time, 55.6 parts of the monomer emulsion (2) was added dropwise to the monomer emulsion (1), and the addition of the monomer emulsion (1) and the monomer emulsion (2) was completed over 2 hours. Then, 37.17 parts of the remaining monomer emulsion (2) was added dropwise to the reaction container over 1 hour, and after aging for 1 hour, 20 parts of a 5% N-ethylmorpholine aqueous solution was slowly added to the reaction container while cooling to 30°C, and then the solution was discharged while filtering with a 100-mesh nylon cloth to obtain hydroxyl- and carboxyl-containing acrylic resin particles (A1"-1) having a solid content concentration of 30%. The obtained hydroxyl- and carboxyl-containing acrylic resin particles (A1"-1) had an acid value of 16 mgKOH / g, a hydroxyl value of 66 mgKOH / g, and a glass transition temperature of 21°C.
[0274] Monomer emulsion (1): 42 parts of deionized water, 0.72 parts of "Aqualon KH-10", 2 parts of methylenebisacrylamide, 5 parts of styrene, 15 parts of methyl methacrylate, 5 parts of 2-hydroxyethyl methacrylate and 23 parts of n-butyl acrylate were mixed and stirred to obtain a monomer emulsion (1).
[0275] Monomer emulsion (2): 42 parts of deionized water, 0.72 parts of "Aqualon KH-10", 0.05 parts of ammonium persulfate, 2.5 parts of methacrylic acid, 10 parts of 2-hydroxyethyl methacrylate, 5 parts of styrene, 12.5 parts of methyl methacrylate, 10 parts of n-butyl acrylate and 10 parts of n-butyl methacrylate were mixed and stirred to obtain a monomer emulsion (2).
[0276] Production of polyester resin (A2) containing hydroxyl and carboxyl groups
[0277] Production Example 4
[0278] 174 parts of trimethylolpropane, 327 parts of neopentyl glycol, 352 parts of adipic acid, 109 parts of isophthalic acid and 101 parts of 1,2-cyclohexanedicarboxylic anhydride were placed in a reaction vessel equipped with a thermometer, a thermostat, a stirring device, a reflux condenser and a water separator, and the temperature was raised from 160°C to 230°C over 3 hours, and the temperature was maintained at 230°C while the generated condensation water was distilled off by a water separator, and the reaction was performed until the acid value was 3 mgKOH / g or less. 59 parts of trimellitic anhydride was added to the reaction product, and an addition reaction was carried out at 170°C for 30 minutes, and then the reaction was cooled to 50°C or less, and 75.8 parts of N-ethylmorpholine was added for neutralization, and then deionized water was gradually added to obtain a polyester resin solution (A2-1) containing hydroxyl and carboxyl groups having a solid content concentration of 45%. The obtained polyester resin containing hydroxyl groups and carboxyl groups had a hydroxyl value of 128 mgKOH / g, an acid value of 35 mgKOH / g, and a weight average molecular weight of 13,000.
[0279] Production Example 5
[0280] In a reaction vessel equipped with a thermometer, a thermostat, a stirrer, a reflux condenser and a water separator, 174 parts of trimethylolpropane, 327 parts of neopentyl glycol, 352 parts of adipic acid, 109 parts of isophthalic acid and 101 parts of 1,2-cyclohexanedicarboxylic anhydride were charged, and the temperature was raised from 160°C to 230°C over 3 hours, and the temperature was maintained at 230°C while the generated condensation water was distilled off by a water separator, and the reaction was performed until the acid value was 3 mgKOH / g or less. 59 parts of trimellitic anhydride was added to the reaction product, and an addition reaction was performed at 170°C for 30 minutes, and then the reaction was cooled to 50°C or less, and 58.7 parts of 2-(dimethylamino)ethanol was added for neutralization, and then deionized water was gradually added to obtain a polyester resin solution (A2-2) containing hydroxyl groups and carboxyl groups having a solid content concentration of 45%. The obtained polyester resin containing hydroxyl groups and carboxyl groups had a hydroxyl value of 128 mgKOH / g, an acid value of 35 mgKOH / g, and a weight average molecular weight of 13,000.
[0281] Production of polyurethane resin (A3) containing hydroxyl and carboxyl groups
[0282] Production Example 6
[0283] Into a reaction vessel equipped with a thermometer, a stirrer and a reflux condenser, 211.9 parts of polytetramethylene glycol (number average molecular weight 1000), 11.5 parts of 2,2-dimethylolpropionic acid, 6.9 parts of trimethylolpropane, 112.2 parts of isophorone diisocyanate and 298.5 parts of methyl ethyl ketone were charged, and after the reaction system was replaced with nitrogen, the reaction was carried out at 80° C. with stirring to obtain an NCO-terminated urethane prepolymer having a free isocyanate group content of 3.2%. The obtained methyl ethyl ketone solution was cooled to 40°C, and 493.2 g of deionized water containing 9.8 parts of N-ethylmorpholine was added for emulsification. Then, 275.9 parts of a 5% aqueous solution of N-(2-hydroxyethyl)ethylenediamine was added thereto. After stirring for 60 minutes, the methyl ethyl ketone was distilled off under reduced pressure and heating, and the concentration was adjusted with deionized water to obtain a polyurethane resin dispersion (A3-1) containing hydroxyl and carboxyl groups with a solid content of 35%, an acid value of 14 mgKOH / g, a hydroxyl value of 12 mgKOH / g, and an average particle size of 120 nm.
[0284] Production Example 7
[0285] Into a reaction vessel equipped with a thermometer, a stirrer and a reflux condenser, 211.9 parts of polytetramethylene glycol (number average molecular weight 1000), 11.5 parts of 2,2-dimethylolpropionic acid, 6.9 parts of trimethylolpropane, 112.2 parts of isophorone diisocyanate and 298.5 parts of methyl ethyl ketone were charged, and after the reaction system was replaced with nitrogen, the reaction was carried out at 80° C. with stirring to obtain an NCO-terminated urethane prepolymer having a free isocyanate group content of 3.2%. The obtained methyl ethyl ketone solution was cooled to 40°C, and 493.2 g of deionized water containing 8.6 parts of triethylamine was added for emulsification. Then, 275.9 parts of a 5% aqueous solution of N-(2-hydroxyethyl)ethylenediamine was added thereto. After stirring for 60 minutes, the methyl ethyl ketone was distilled off under reduced pressure and heating, and the concentration was adjusted with deionized water to obtain a hydroxyl- and carboxyl-containing polyurethane resin dispersion (A3-2) having a solid content of 35%, an acid value of 14 mgKOH / g, a hydroxyl value of 12 mgKOH / g, and an average particle size of 120 nm.
[0286] Production of hydroxyl-free and carboxyl-containing polyurethane resin (U-1)
[0287] Production Example 8
[0288] Into a reaction vessel equipped with a thermometer, a stirrer and a reflux condenser, 211.9 parts of polytetramethylene glycol (number average molecular weight 1000), 11.5 parts of 2,2-dimethylolpropionic acid, 6.9 parts of trimethylolpropane, 112.2 parts of isophorone diisocyanate and 298.5 parts of methyl ethyl ketone were charged, and after the reaction system was replaced with nitrogen, the reaction was carried out at 80° C. with stirring to obtain an NCO-terminated urethane prepolymer having a free isocyanate group content of 3.2%. The obtained methyl ethyl ketone solution was cooled to 40°C, and 493.2 g of deionized water containing 9.8 parts of N-ethylmorpholine was added for emulsification. Then, 159.2 parts of a 5% aqueous solution of ethylenediamine was added thereto. After stirring for 60 minutes, the methyl ethyl ketone was distilled off under reduced pressure and heating, and the concentration was adjusted with deionized water to obtain a hydroxyl-free and carboxyl-containing polyurethane resin dispersion (U-1) having a solid content of 35%, an acid value of 14 mgKOH / g, and an average particle size of 120 nm.
[0289] Production of blocked polyisocyanate compound (B)
[0290] Production Example 9
[0291] Into a reaction vessel equipped with a thermometer, a thermostat, a stirrer, a reflux condenser, a nitrogen inlet tube, a dropping device, and a simple water filter valve for solvent removal, 1500 parts of "Sumidur N-3300" (trade name, manufactured by Sumika Bayer Urethane Co., Ltd., a polyisocyanate containing an isocyanurate structure derived from hexamethylene diisocyanate, solid content 100%, isocyanate group content 21.8%) and 0.9 parts of 2,6-di-tert-butyl-4-methylphenol were charged, mixed thoroughly, and heated at 130° C. for 3 hours under a nitrogen stream. Next, 1200 parts of ethyl acetate and 1300 parts of diisopropyl malonate were charged, and 14 parts of a 28% methanol solution of sodium methoxide was added while stirring under a nitrogen stream, and stirred at 65° C. for 8 hours to obtain a blocked polyisocyanate compound (B-1) having a solid content of 70% and a weight average molecular weight of 4000.
[0292] Production Example 10
[0293] Into a reaction container equipped with a thermometer, a thermostat, a stirrer, a reflux condenser, a nitrogen inlet tube, and a dropping device, 1610 parts of "Sumidur N-3300" (trade name, manufactured by Sumika Bayer Urethane Co., Ltd., a polyisocyanate containing an isocyanurate structure derived from hexamethylene diisocyanate, solid content 100%, isocyanate group content 21.8%), 1200 parts of "PTMG2000" (trade name, manufactured by MITSUBISHI CHEMICAL Co., Ltd., polytetramethylene ether glycol, average molecular weight 2000, solid content 100%) and 0.9 part of 2,6-di-tert-butyl-4-methylphenol were charged, mixed thoroughly, and heated at 130° C. for 3 hours under a nitrogen stream. Next, 1,200 parts of ethyl acetate and 1,250 parts of diisopropyl malonate were charged, and 14 parts of a 28% methanol solution of sodium methoxide was added while stirring under a nitrogen stream. The mixture was stirred at 65° C. for 8 hours, and diluted with ethyl acetate so that the final solid content became 70%, thereby obtaining a blocked polyisocyanate compound (B-2) having a solid content of 70% and a weight-average molecular weight of 50,000.
[0294] Production of acrylic resin containing phosphoric acid group
[0295] Production Example 11
[0296] A mixed solvent of 27.5 parts of methoxypropanol and 27.5 parts of isobutyl alcohol was added to a reaction container equipped with a thermometer, a thermostat, a stirrer, a reflux condenser, and a dropping device, and heated to 110° C. Next, 121.5 parts of a mixture consisting of 25 parts of styrene, 27.5 parts of n-butyl methacrylate, 20 parts of “Isostearyl Acrylate” (trade name, manufactured by Osaka Organic Chemical Industry Co., Ltd., branched higher alkyl acrylate), 7.5 parts of 4-hydroxybutyl acrylate, 15 parts of the following phosphoric acid group-containing polymerizable monomer, 12.5 parts of 2-methacryloyloxyethyl acid phosphate, 10 parts of isobutyl alcohol, and 4 parts of tert-butyl peroxyoctanoate was added to the mixed solvent over 4 hours, and a mixture consisting of 0.5 parts of tert-butyl peroxyoctanoate and 20 parts of isopropyl alcohol was further added dropwise over 1 hour. Then, the mixture was stirred and aged for 1 hour to obtain a phosphoric acid group-containing acrylic resin solution (C1′-1) having a solid content concentration of 50%. The present resin has an acid value based on phosphoric acid groups of 83 mgKOH / g, a hydroxyl value of 29 mgKOH / g, and a weight average molecular weight of 10,000.
[0297] Polymerizable monomer containing phosphoric acid group: 57.5 parts of monobutyl phosphoric acid and 41 parts of isobutyl alcohol were added to a reaction vessel equipped with a thermometer, a thermostat, a stirrer, a reflux condenser and a dropping device, and the temperature was raised to 90°C. After 42.5 parts of glycidyl methacrylate was added dropwise over 2 hours, and then stirred and aged for 1 hour. Then, 59 parts of isopropyl alcohol was added to obtain a phosphoric acid group-containing polymerizable monomer solution with a solid content concentration of 50%. The acid value of the obtained monomer based on the phosphoric acid group was 285 mgKOH / g.
[0298] Production of pigment dispersions
[0299] Production Example 12
[0300] 44.4 parts (solid content 20 parts) of the polyester resin solution (A2-1) containing hydroxyl and carboxyl groups obtained in Preparation Example 4, 100 parts of "JR-806" (trade name, manufactured by TAYCA, rutile titanium dioxide), 1 part of "Carbon MA-100" (trade name, manufactured by Mitsubishi Chemical Corporation, carbon black) and 10 parts of deionized water were mixed, and 1.2 parts of N-ethylmorpholine was added to adjust the pH to 8.0. Then, the obtained mixed solution was added to a wide-mouthed glass bottle, and a 20-ounce glass bottle with a diameter of about 1.5 mm was added as a dispersion medium. The mixture was sealed with glass beads and dispersed with a paint shaker for 30 minutes to obtain a pigment dispersion (P-1).
[0301] Production Example 13
[0302] 44.4 parts (solid content 20 parts) of the polyester resin solution (A2-2) containing hydroxyl and carboxyl groups obtained in Production Example 5, 100 parts of "JR-806" (trade name, manufactured by TAYCA, rutile titanium dioxide), 1 part of "Carbon MA-100" (trade name, manufactured by Mitsubishi Chemical Corporation, carbon black) and 10 parts of deionized water were mixed, and 0.7 parts of 2-(dimethylamino)ethanol was added to adjust the pH to 8.0. Then, the obtained mixed solution was added to a wide-mouthed glass bottle, and a glass with a diameter of about 1.5 mm was added as a dispersion medium. The mixture was sealed with glass beads and dispersed with a paint shaker for 30 minutes to obtain a pigment dispersion (P-2).
[0303] Production of waterborne coating compositions
[0304] Example 1
[0305] 155.9 parts of the pigment dispersion (P-1) obtained in Preparation Example 12, 83.3 parts (solid content 25 parts) of the hydroxyl and carboxyl group-containing acrylic resin particles (A1'-1) obtained in Preparation Example 1, 57.1 parts (solid content 20 parts) of the hydroxyl and carboxyl group-containing polyurethane resin dispersion (A3-1) obtained in Preparation Example 6, 42.9 parts (solid content 30 parts) of the blocked polyisocyanate compound (B-1) obtained in Preparation Example 9, 12.5 parts (solid content 5 parts) of "CARBODILITE SV02" (trade name, manufactured by Nisshinbo Co., Ltd., carbodiimide compound, solid content 40%, carbodiimide equivalent per unit solid content 429) and 4 parts (solid content 2 parts) of the phosphoric acid group-containing acrylic resin solution obtained in Preparation Example 11 were uniformly mixed. Next, 1.6 parts of N-ethylmorpholine as a basic compound (D) for pH adjustment was added to adjust the pH to 8.2. Next, "UH-752" (trade name, manufactured by ADEKA, thickener) and deionized water were added to obtain aqueous coating composition No. 1 having a pH of 8.2, a coating solid content of 48%, and a viscosity of 30 seconds as measured by a No. 4 Ford cup at 20°C.
[0306] Examples 2 to 18, Comparative Examples 1 to 6
[0307] Aqueous coating compositions Nos. 2 to 24 having a viscosity of 30 seconds in a No. 4 Ford cup at 20° C. were obtained in the same manner as in Example 1 except that the blending compositions were set as shown in Tables 1-1 to 1-4 below.
[0308] The storage stability of the aqueous coating compositions Nos. 1 to 24 was evaluated based on the viscosity change rate.
[0309] Viscosity change rate: Evaluation was made based on the viscosity after 1 minute at 60 rpm measured with "LVDV-I" (trade name, manufactured by Brookfield, B-type viscometer) and the change rate between the viscosity immediately after production and the viscosity after standing at 40°C for 10 days.
[0310] Viscosity change rate (%) = |(viscosity after standing at 40°C for 10 days / viscosity immediately after production) - 1 | × 100
[0311] ◎ and 0 are qualified.
[0312] ◎: The viscosity change rate is less than 20%.
[0313] ○: The viscosity change rate is 20% or more and less than 50%.
[0314] ×: The viscosity change rate is 50% or more.
[0315] The results of storage stability are collectively shown in Tables 1-1 to 1-4.
[0316] [Table 1-1]
[0317]
[0318] [Table 1-2]
[0319]
[0320] [Table 1-3]
[0321]
[0322] [Table 1-4]
[0323]
[0324] Preparation of test coatings
[0325] A thermosetting epoxy resin-based cationic electrodeposition coating composition (trade name "ELECRON GT-10", manufactured by KANSAI Paint Co., Ltd.) was electrodeposited onto a cold-rolled steel sheet treated with zinc phosphate to a film thickness of 20 μm, and cured by heating at 170° C. for 30 minutes. In this way, a coated article having an electrodeposition coating film formed on a steel sheet was produced.
[0326] Preparation of test coated panels
[0327] Embodiment 19
[0328] The water-based coating composition No. 1 obtained in Example 1 was electrostatically applied to the test object using a rotary atomizing electrostatic coating machine so that the cured film thickness became 20 μm, and left to stand for 5 minutes to form an uncured intermediate coating film.
[0329] Next, a rotary atomizing electrostatic coating machine was used to electrostatically coat "WBC-713T No. 202" (trade name, manufactured by KANSAI Paint Co., Ltd., acrylic melamine resin-based water-based base coating paint, black paint) on the uncured mid-coat film in a manner such that the dry film thickness became 15 μm. After standing for 5 minutes, the film was preheated at 80° C. for 3 minutes to form an uncured base coating film.
[0330] Next, "Soflex #520 Clear" (a trade name manufactured by KANSAI Paint Co., Ltd., a two-component acrylic urethane organic solvent-based clear coating material containing a hydroxyl-containing acrylic resin and a polyisocyanate compound) was electrostatically coated on the uncured base coating film so that the dry film thickness became 35 μm, and the film was left to stand for 7 minutes to form a clear coating film.
[0331] Next, it was heated at 80°C for 30 minutes to heat-cure the intermediate coat film, the base coat film, and the transparent film, thereby producing a test coating board.
[0332] Examples 20 to 38, Comparative Examples 7 to 12
[0333] In Example 19, the types of the aqueous coating compositions and the heating temperatures were changed as described in Table 2 below. Other than that, test boards were produced in the same manner as in Example 19.
[0334] Each of the test boards obtained above was evaluated by the following test methods. The evaluation results are shown in Table 2 below.
[0335] (Test Methods)
[0336] Low-temperature curability: According to JIS K 5600-5-4 (1999) "Scratch hardness (pencil method)", the pencil hardness of the test boards obtained in the above Examples and Comparative Examples was measured. The pencil hardness is in the order of 3B < 2B < B < HB < F. If the pencil hardness is HB or higher, it is considered qualified. The evaluation results are shown in Table 2.
[0337] Water resistance adhesion: The test boards obtained in the above Examples and Comparative Examples were immersed in warm water at 40°C for 240 hours. After being taken out and wiping off the surface moisture, immediately according to JIS K5600-5-6 (1990), 100 checkerboards of 2 mm × 2 mm were made on the coating film. A tape was pasted on this surface and rapidly peeled off. Then, the number of checkerboard coating films remaining on the coating surface was evaluated. ◎ and 〇 are considered qualified. The evaluation results are shown in Table 2.
[0338] ◎: Number of remaining / Total number = 100 / 100, no edge defect.
[0339] 〇: Number of remaining / Total number = 100 / 100, with edge defect.
[0340] Δ: Number of remaining / Total number = 99 - 90 / 100.
[0341] ×: Number of remaining / Total number = 89 or less / 100.
[0342] Hardness after water resistance: The test boards obtained in the above Examples and Comparative Examples were immersed in warm water at 40°C for 240 hours and dried at 20°C for 12 hours. Then, according to JIS K 5600-5-4 (1999) "Scratch hardness (pencil method)", the pencil hardness of the coating surface of each test board was measured. If the pencil hardness is B or higher, it is considered qualified. The evaluation results are shown in Table 2.
[0343] Resistance to stone chipping: The test plate obtained in the above-mentioned embodiment and comparative example was set on the test piece holding table of the flying stone tester "JA-400" (trade name, manufactured by Suga Test Instruments, a stone chipping resistance tester). At 0°C, 50 g of granite crushed stone with a particle size of No. 7 was made to collide with the test plate at an angle of 45 degrees from 30 cm away from the test plate using 0.39 MPa (4 kgf / cm2) compressed air. Then, the obtained test plate was washed with water and dried, and a cloth tape (manufactured by Nichiban Co., Ltd.) was attached to the coating surface. After the cloth tape was peeled off, the degree of damage to the coating film was visually observed, and the evaluation was performed according to the following criteria. ◎ and ○ are qualified. The evaluation results are shown in Table 2.
[0344] ◎: The damage is extremely small, and the electrodeposited surface and the base steel sheet are not exposed.
[0345] ○: The damage is small, and the electrodeposited surface and the base steel sheet are not exposed.
[0346] Δ: The damage is small, but the electrodeposited surface and the underlying steel sheet are exposed.
[0347] ×: The damage is quite large, and the underlying steel plate is also largely exposed.
[0348] Glass adhesion: A urethane adhesive (trade name "3740", manufactured by Sunstar Co., Ltd., automotive windshield agent) was further applied to each test coated plate obtained in the above-mentioned embodiments and comparative examples in a coating shape having a width of 20 mm, a thickness of 3 mm, and a length of 100 mm or more, and after covering with release paper, it was evenly pressed with a flat plate. After removing the flat plate, it was placed at a temperature of 23±2°C and a humidity of 50±5% for 72 hours to cure. Then, the release paper was peeled off. Next, each test coated plate was immersed in a constant temperature water bath set at 50°C for 240 hours, and then immersed in water at 23°C for 1 hour. After cooling, the following peeling test was performed.
[0349] While manually stretching the cured adhesive layer in a direction of 90 degrees or more relative to the coating film, the cured adhesive layer was cut with a cutter at intervals of 2 to 3 mm and at an angle of about 60 degrees relative to the coating film to the surface of the coating film. The peeling state after peeling off the adhesive layer was evaluated according to the following criteria. ◎, 0+ and 0 were qualified.
[0350] ⊚: No peeling of the adhesive layer was observed, and no exposure of the coating film was observed.
[0351] 0+: The coating film was not destroyed, and only the adhesive layer was peeled off due to cohesive failure, but the adhesion between the coating film and the adhesive layer was almost maintained.
[0352] ○: The coating film was peeled off due to cohesive failure, and the width of the peeled off film was less than 1 mm from the portion cut by the cutter.
[0353] Δ: The coating film was peeled off due to cohesive failure, and the width of the peeled off film from the portion cut by the cutter was 1 mm or more.
[0354] ×: Peeling was observed at the interface between the coating film and the adhesive layer.
[0355] [Table 2]
[0356]
[0357] As mentioned above, although embodiment and Example of this invention were specifically described, this invention is not limited to the said embodiment, Various deformation|transformation based on the technical idea of this invention is possible.
[0358] For example, the structures, methods, processes, shapes, materials, and numerical values listed in the above-mentioned embodiments and examples are merely examples, and different structures, methods, processes, shapes, materials, and numerical values may be used as needed.
[0359] Furthermore, the configurations, methods, steps, shapes, materials, numerical values, and the like of the above-described embodiments can be combined with each other as long as they do not depart from the gist of the present invention.
Claims
1. A water-based coating composition comprising: (A) Resins containing hydroxyl and carboxyl groups, (B) blocked polyisocyanate compounds, (C) polycarbodiimide compounds, and (D) basic compounds, The alkaline compound (D) contains an alkaline compound (D1) having an acid dissociation constant PKa in the range of 7.0 to 8.5 and a boiling point in the range of 100 to 200° C., and the content ratio of the alkaline compound (D1) is in the range of 30 to 100% by mass based on the mass of the alkaline compound (D). The basic compound (D1) having an acid dissociation constant PKa in the range of 7.0 to 8.5 and a boiling point in the range of 100 to 200° C. is N-methylmorpholine and / or N-ethylmorpholine, Furthermore, the pH of the aqueous coating composition is within the range of 8.0 to 11.
5.
2. The aqueous coating composition according to claim 1, wherein At least a part of the blocking agent of the blocked polyisocyanate compound (B) is an active methylene-based blocking agent. 3 . The aqueous coating composition according to claim 1 , further comprising a melamine resin (E).
4. A method for forming a multilayer coating film, comprising sequentially performing the following steps: Step (1): a step of applying the aqueous coating composition according to any one of claims 1 to 3 to a coated object to form a mid-coat coating film; Step (2): a step of applying a water-based base coating composition on the intermediate coating film formed in the step (1) to form a base coating film; Step (3): a step of applying a clear coating composition on the base coating film formed in step (2) to form a clear coating film; and Step (4): a step of simultaneously curing the intermediate coating film, the base coating film, and the clear coating film formed in the steps (1) to (3) at a temperature in the range of 60 to 110°C.
Citation Information
Patent Citations
Multi-layer coating film forming method