Hydroxymethylurea-PTGE-carboxymethyl cellulose antifreeze and water-resistant sand-fixing material and preparation method thereof

Through the free radical polymerization reaction of hydroxymethylurea and glycerol triglycidyl ether and carboxymethyl cellulose, HDM-PTGE-CMC sand fixing material is formed, which solves the problem of low consolidation strength and insufficient water resistance of carboxymethyl cellulose. Problem, it has achieved anti-freeze, water and sand fixing effect suitable for high-altitude sandy land, and replaced toxic enhancers.

CN116854955BActive Publication Date: 2024-11-26NORTHWEST INST OF ECO ENVIRONMENT & RESOURCES CAS +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310752327.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-25
Publication Date
2024-11-26
Estimated Expiration
2043-06-25

AI Technical Summary

Technical Problem

In the prior art, carboxymethyl cellulose has low consolidation strength, insufficient thermal stability and water resistance, and the commonly used enhancer acrylamide is toxic, affecting human health and ecological environment.

Method used

The free radical polymerization reaction of hydroxymethylurea and glycerol triglycidyl ether with carboxymethyl cellulose is carried out to form hydroxymethylurea-PTGE-carboxymethyl cellulose (HDM-PTGE-CMC) sand fixing material, which improves its Consolidation strength and cold resistance.

Benefits of technology

This material has good low temperature resistance, strong bonding strength and water resistance. It is suitable for anti-freezing, water-resistant sand fixing in the high-cold sands of the Qinghai-Tibet Plateau, replacing traditional toxic enhancers and improving the sand fixing effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116854955B_ABST
    Figure CN116854955B_ABST
Patent Text Reader

Abstract

The present invention discloses a hydroxymethylurea-PTGE-carboxymethyl cellulose antifreeze and water-resistant sand-fixing material and a preparation method thereof. The preparation method comprises: subjecting a mixed reaction system comprising carboxymethyl cellulose salt, hydroxymethyl urea and PTGE to a free radical polymerization reaction under the action of an initiator to obtain a hydroxymethyl urea-PTGE-carboxymethyl cellulose antifreeze and water-resistant sand-fixing material. The present invention utilizes hydroxymethyl urea to improve its consolidation strength, and uses glycerol triglycidyl ether to improve its cold resistance and water resistance, to prepare a hydroxymethyl urea-PTGE-carboxymethyl cellulose (HDM-PTGE-CMC) sand-fixing material suitable for the low-temperature high-altitude sandy land of the Qinghai-Tibet Plateau that is moist after rain, so that it has low-temperature resistance, strong bonding strength and water resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a sand-fixing agent, in particular to a hydroxymethylurea-PTGE-carboxymethyl cellulose (HDM-PTGE-CMC) antifreeze and water-resistant sand-fixing material and a preparation method and application thereof, belonging to the technical field of biopolymers and sand-fixing. Background Art

[0002] Desertification seriously threatens global ecological security and the sustainable development of human economy and society, affects 25% of the world's total land area, and threatens the lives of more than 1 billion people in more than 100 countries. It is a major environmental problem and development bottleneck facing the world. Wind and sand activities are typical surface processes in desert areas. Therefore, it is of great significance to take necessary measures to prevent wind and sand.

[0003] In the semi-humid climate areas of the Qinghai-Tibet Plateau, such as the Riganqiao Ecological Protection Area on the southeastern edge of the Qinghai-Tibet Plateau, the annual average temperature is about 2.55℃, the annual minimum temperature is about -23℃, and the annual precipitation is about 801.76mm, which is more than the semi-arid climate areas of the Qinghai-Tibet Plateau, such as the annual precipitation of 440.86mm in the Qinghai Lake East Ecological Protection Area on the northeastern edge of the Qinghai-Tibet Plateau. Therefore, the environmental temperature after rain in the high-cold sandy land in the semi-humid climate areas of the Qinghai-Tibet Plateau is low and the humidity is high. The sand fixation agent suitable for this area needs to have good antifreeze and water resistance.

[0004] The long chain structure of carboxymethyl cellulose (CMC) gives it good adhesion and film-forming properties, but it is very easy to decompose, has low consolidation strength, and its antifreeze and water resistance properties need to be improved. Acrylamide is commonly used in the prior art to enhance the interaction between cellulose and its derivatives, but acrylamide is toxic and poses uncertain risks to human health and the ecological environment. Therefore, it is of great significance to find a new non-toxic substance to replace acrylamide to enhance carboxymethyl cellulose. Summary of the invention

[0005] The purpose of the present invention is to improve the consolidation strength of the material by using hydroxymethyl urea and improve the cold resistance and water resistance of the material by using glycerol triglycidyl ether, and to provide a hydroxymethyl urea-PTGE-carboxymethyl cellulose (HDM-PTGE-CMC) sand-fixing material suitable for the low-temperature high-cold sandy land of the Qinghai-Tibet Plateau that is moist after rain and a preparation method thereof, so as to improve the shortcomings of the prior art that the carboxymethyl fiber is very easy to decompose, has low consolidation strength and low thermal stability.

[0006] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:

[0007] The embodiment of the present invention provides a method for preparing a hydroxymethyl urea-PTGE-carboxymethyl cellulose antifreeze and water-resistant sand-fixing material, which comprises: subjecting a mixed reaction system comprising carboxymethyl cellulose salt, hydroxymethyl urea and PTGE to a free radical polymerization reaction under the action of an initiator to obtain the hydroxymethyl urea-PTGE-carboxymethyl cellulose antifreeze and water-resistant sand-fixing material.

[0008] In some embodiments, the preparation method includes: introducing a protective gas into the mixed reaction system at a temperature between 65 and 100° C., then adding an initiator, and reacting for 3 to 6 hours to obtain a hydroxymethyl urea-PTGE-carboxymethyl cellulose antifreeze and water-resistant sand-fixing material.

[0009] The embodiment of the present invention also provides a hydroxymethylurea-PTGE-carboxymethyl cellulose antifreeze and water-resistant sand-fixing material prepared by the above-mentioned preparation method.

[0010] Furthermore, the embodiments of the present invention also provide the use of the aforementioned hydroxymethyl urea-PTGE-carboxymethyl cellulose antifreeze and water-resistant sand-fixing material in the field of sand fixation.

[0011] Compared with the prior art, the beneficial effects of the present invention are:

[0012] The present invention utilizes hydroxymethyl urea to improve its consolidation strength, and utilizes glycerol triglycidyl ether to improve its cold resistance and water resistance, so as to prepare a hydroxymethyl urea-PTGE-carboxymethyl cellulose (HDM-PTGE-CMC) sand-fixing material suitable for the low-temperature high-altitude sandy land of the Qinghai-Tibet Plateau that is moist after rain, so that the material has low-temperature resistance, strong bonding strength and water resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0014] Figure 1 It is a schematic diagram of the preparation of hydroxymethyl urea-PTGE-carboxymethyl cellulose (HDM-PTGE-CMC) antifreeze and water-resistant sand-fixing material in a typical embodiment of the present invention. DETAILED DESCRIPTION

[0015] In view of the deficiencies in the prior art, the inventors have proposed the technical solution of the present invention after long-term research and extensive practice, which mainly utilizes hydroxymethyl urea to enhance the mechanical strength of carboxymethyl cellulose, and uses PTGE to enhance the antifreeze performance and water resistance of the HDM-CMC sand-fixing agent, so as to prepare an antifreeze and water-resistant hydroxymethyl urea-PTGE-carboxymethyl cellulose (HDM-PTGE-CMC) sand-fixing material that can be used in the high-cold sandy land of the Qinghai-Tibet Plateau that is moist after rain. The technical solution, its implementation process and principles will be further explained as follows. However, it should be understood that within the scope of the present invention, the above-mentioned technical features of the present invention and the technical features specifically described in the following (embodiments) can be combined with each other to form a new or preferred technical solution. Due to space limitations, they will not be described one by one here.

[0016] As another aspect of the technical solution of the present invention, a method for preparing a hydroxymethyl urea-glycerol triglycidyl ether-carboxymethyl cellulose (HDM-PTGE-CMC) antifreeze and water-resistant sand-fixing material is provided, comprising: subjecting a mixed reaction system comprising carboxymethyl cellulose salt, hydroxymethyl urea, and PTGE to a free radical polymerization reaction under the action of an initiator to obtain a hydroxymethyl urea-PTGE-carboxymethyl cellulose antifreeze and water-resistant sand-fixing material.

[0017] In some embodiments, the preparation method comprises: mixing carboxymethyl cellulose salt with water to form a carboxymethyl cellulose salt aqueous solution, adjusting the pH value of the carboxymethyl cellulose salt aqueous solution to 6-9 with an alkaline substance, and then adding hydroxymethyl urea and PTGE to form the mixed reaction system.

[0018] Furthermore, the initial pH value can be 6, 7, 8, 9, etc., but is not limited thereto.

[0019] Furthermore, in the mixed reaction system, the molar ratio of carboxymethyl cellulose salt, hydroxymethyl urea and PTGE is 1:1:1 to 1:2:2.

[0020] The hydroxymethyl urea (HDM) used in the present invention is a nitrogen-containing organic compound with a molecular formula of C 2 H 6 N 2 O 2, containing amide, amino, hydroxyl and carboxyl groups, and is mainly produced using non-protein nitrogen (NPN) as the main raw material. NPN refers to nitrogen-containing compounds in a non-protein state, including amino acids, peptides, ammonia and its derivatives, urea and its derivatives, amines, phthalamides, hey yin, cyanamides, nitrates and alkaloids, etc., which are widely present in the bodies of animals and plants. It is a non-toxic and naturally degradable material. Its amino, hydroxyl and amide groups can replace the hydrogen bonds between acrylamide and cellulose and its derivatives to form a stable cross-linked network, enhancing the mechanical properties of cellulose and its derivatives.

[0021] Furthermore, the carboxymethyl cellulose salt includes any one or a combination of two or more of sodium carboxymethyl cellulose, lithium carboxymethyl cellulose, potassium carboxymethyl cellulose, calcium carboxymethyl cellulose, ammonium carboxymethyl cellulose, etc., but is not limited thereto.

[0022] Glycerol triglycidyl ether (PTGE) not only has good water resistance, but also is often used to improve the low-temperature toughness of rigid structures due to its large number of ether bonds. The introduction of PTGE flexible segments into the cross-linked network can improve the flexibility of the network chain molecules, reduce internal stress, and achieve a balance between low-temperature toughness and bonding strength by adjusting the cross-linking density. In addition, the epoxy groups in PTGE can be tightly combined with the flexible long chains through hydrophilic groups to form a dense cross-linked network, thereby enhancing the low-temperature resistance, strong bonding strength and water resistance of carboxymethyl cellulose.

[0023] In some embodiments, the preparation method may specifically include: introducing a protective gas into the mixed reaction system at a temperature between 65 and 100° C., then adding an initiator, and reacting for 3 to 6 hours to obtain a hydroxymethyl urea-propylene triglycidyl ether-carboxymethyl cellulose (HDM-PTGE-CMC) antifreeze and water-resistant sand-fixing material.

[0024] Further, the reaction temperature may be 65° C., 70° C., 80° C., 90° C., 100° C., etc., but is not limited thereto.

[0025] Furthermore, the reaction time can be 3 h, 4 h, 5 h, 6 h, etc., but is not limited thereto.

[0026] The mechanism of action of the sand-fixing material with antifreeze and water-resistant performance prepared by the present invention is that when the HDM-PTGE-CMC sand-fixing agent is sprayed in the sand tray, the carbonyl group on the hydroxymethylurea chain can react with the inorganic ions in the sand, and at the same time, the calcium carbonate and other substances in the gravel will react with the carboxymethyl cellulose to replace the sodium ions, so that two carboxyl anions and an inorganic cation (such as calcium ions, magnesium ions, etc.) are combined to form a stable network structure, thereby playing a role in fixing sand. In addition, the epoxy group in glycerol triglycidyl ether (PTGE) can be tightly combined with the flexible long chain through the hydrophilic group, and the epoxy group will react with the phenolic hydroxyl group on the benzene ring under alkaline conditions to form an ether bond, forming a dense cross-linked network, thereby enhancing the low temperature resistance, strong bonding strength and water resistance of the carboxymethyl cellulose.

[0027] Furthermore, the initiator may be potassium persulfate (K 2 S 2 O 8 ), but are not limited to them.

[0028] Furthermore, the concentration of the initiator added to the mixed reaction system is 0.05 to 0.25 g / mL, for example, 0.05 g / mL, 0.1 g / mL, 0.15 g / mL, 0.2 g / mL and 0.25 g / mL, but not limited thereto.

[0029] Further, the inert gas may be nitrogen, but is not limited thereto.

[0030] Another aspect of the embodiments of the present invention further provides a hydroxymethyl urea-glycerol triglycidyl ether-carboxymethyl cellulose (HDM-PTGE-CMC) antifreeze and water-resistant sand-fixing material prepared by the aforementioned preparation method.

[0031] Furthermore, the water permeability coefficient of the hydroxymethylurea-PTGE-carboxymethyl cellulose antifreeze and water-resistant sand-fixing material is 5×10 -4 cm / s~1.5x10 -3 cm / s, the compressive strength of the sand-fixed samples is between 4 and 6 MPa. After curing for 8 hours, the bonding strength at liquid nitrogen temperature (-210 to -196°C) is between 3 and 7 MPa.

[0032] Correspondingly, another aspect of the embodiments of the present invention further provides the use of any of the aforementioned hydroxymethyl urea-PTGE-carboxymethyl cellulose antifreeze and water-resistant sand-fixing materials in the field of sand fixation, such as the preparation of sand-fixing materials or sand-fixing devices.

[0033] Through the above technical scheme, the present invention uses hydroxymethyl urea to improve its consolidation strength, and uses propylene glycol triglycidyl ether to improve its cold resistance and water resistance, so as to prepare a hydroxymethyl urea-PTGE-carboxymethyl cellulose (HDM-PTGE-CMC) sand-fixing material suitable for the low-temperature high-altitude sandy land of the Qinghai-Tibet Plateau that is moist after rain, so that the material has low-temperature resistance, strong bonding strength and water resistance, and can be used in the field of sand fixation.

[0034] In order to make the purpose, technical scheme and application of the present invention clearer, the technical scheme of the present invention is further described in detail below in conjunction with several preferred embodiments and drawings. The described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work belong to the scope of protection of the present invention. The implementation conditions used in the following embodiments can be further adjusted according to actual needs, and the unspecified implementation conditions are usually the conditions in conventional experiments.

[0035] Example 1

[0036] Deionized water was added to 10 g of sodium carboxymethyl cellulose (CMC) and stirred thoroughly to obtain a CMC aqueous solution, which was adjusted to a pH of 8 using an aqueous NaOH solution (analytical grade), and monomers hydroxymethyl urea (HDM, analytical grade) and PTGE were added to adjust the molar ratio of carboxymethyl cellulose salt, hydroxymethyl urea, and PTGE to 1:1:1.

[0037] Then, nitrogen was introduced for protection and stirred for 30 min. After the solution was fully dissolved, the initiator potassium persulfate solution (K 2 S 2 O 8 After the addition was completed, the reaction system was placed in a 90°C constant temperature water bath and stirred for 4 hours with a stirrer at 500 rpm to allow CMC and HDM to undergo free radical polymerization under the action of potassium persulfate as an initiator. The reaction process is as follows: Figure 1 After 4 h of constant temperature reaction at 90 °C, the product was washed with ethanol (CH 3 CH 2 OH, analytical grade) was precipitated and centrifuged (speed 3500r / min) to separate. The product was washed with ethanol and then with acetone (CH 3 COCH 3 , analytical grade) and dried at 65°C to obtain the HDM-PTGE-CMC sand-fixing sample.

[0038] Example 2

[0039] Deionized water was added to 10 g of sodium carboxymethyl cellulose (CMC) and stirred thoroughly to obtain a CMC aqueous solution, which was adjusted to a pH of 8 using an aqueous NaOH solution (analytical grade), and monomers hydroxymethyl urea (HDM, analytical grade) and PTGE were added to adjust the molar ratio of carboxymethyl cellulose salt, hydroxymethyl urea, and PTGE to 1:2:1.

[0040] Then, nitrogen was introduced for protection and stirred for 30 min. After the mixture was fully dissolved, 0.05 g of initiator potassium persulfate solution (K 2 S 2 O 8 After the addition was completed, the reaction system was placed in a 90°C constant temperature water bath and stirred for 4 hours with a stirrer at 500 rpm to allow CMC and HDM to undergo free radical polymerization under the action of the initiator potassium persulfate. The reaction process is as follows: Figure 1 After 4 h of constant temperature reaction at 90 °C, the product was washed with ethanol (CH 3 CH 2 OH, analytical grade) was precipitated and centrifuged (speed 3500r / min) to separate. The product was washed with ethanol and then with acetone (CH 3 COCH 3 , analytical grade) and dried at 65°C to obtain the HDM-PTGE-CMC sand-fixing sample.

[0041] Example 3

[0042] Deionized water was added to 10 g of sodium carboxymethyl cellulose (CMC) and stirred thoroughly to obtain a CMC aqueous solution, which was adjusted to a pH of 8 using an aqueous NaOH solution (analytical grade), and monomers hydroxymethyl urea (HDM, analytical grade) and PTGE were added to adjust the molar ratio of carboxymethyl cellulose salt, hydroxymethyl urea, and PTGE to 1:2:2.

[0043] Then, nitrogen was introduced for protection and stirred for 30 min. After the solution was fully dissolved, the initiator potassium persulfate solution (K 2 S 2 O 8 After the addition was completed, the reaction system was placed in a 90°C constant temperature water bath and stirred for 4 hours with a stirrer at 500 rpm to allow CMC and HDM to undergo free radical polymerization under the action of the initiator potassium persulfate. The reaction process is as follows: Figure 1 After 4 h of constant temperature reaction at 90 °C, the product was washed with ethanol (CH 3 CH 2 OH, analytical grade) was precipitated and centrifuged (speed 3500r / min) to separate. The product was washed with ethanol and then with acetone (CH 3 COCH3 , analytical grade) and dried at 65°C to obtain the HDM-PTGE-CMC sand-fixing sample.

[0044] The inventors of this case also tested the antifreeze performance, mechanical strength, water resistance, etc. of the sand-fixing materials obtained in the above embodiments, and the results are as follows:

[0045] In Example 1, the water permeability coefficient of the obtained HDM-PTGE-CMC is 1x10 -3 cm / s, the compressive strength of the sand-fixed sample is 4MPa. After curing for 8h, the bonding strength at liquid nitrogen temperature (-210~-196℃) is 4MPa.

[0046] In Example 2, the water permeability coefficient of the obtained HDM-PTGE-CMC is 0.5x10 -3 cm / s, the compressive strength of the sand-fixed sample is 5MPa. After curing for 8h, the bonding strength at liquid nitrogen temperature (-210~-196℃) is 6MPa.

[0047] In Example 3, the water permeability coefficient of the obtained HDM-PTGE-CMC is 5x10 -4 cm / s, the compressive strength of the sand-fixed sample is 6MPa. After curing for 8h, the bonding strength at liquid nitrogen temperature (-210~-196℃) is 7MPa.

[0048] Example 4

[0049] Deionized water was added to 10 g of sodium carboxymethyl cellulose (CMC) and stirred thoroughly to obtain a CMC aqueous solution, which was adjusted to a pH of 8 using an aqueous NaOH solution (analytical grade), and monomers hydroxymethyl urea (HDM, analytical grade) and PTGE were added to adjust the molar ratio of carboxymethyl cellulose salt, hydroxymethyl urea, and PTGE to 1:2:2.

[0050] Then, nitrogen was introduced for protection and stirred for 30 min. After the solution was fully dissolved, the initiator potassium persulfate solution (K 2 S 2 O 8 After the addition was completed, the reaction system was placed in a 90°C constant temperature water bath and stirred for 4 hours with a stirrer at 500 rpm to allow CMC and HDM to undergo free radical polymerization under the action of the initiator potassium persulfate. The reaction process is as follows: Figure 1 After 4 h of constant temperature reaction at 90 °C, the product was washed with ethanol (CH 3 CH 2 OH, analytical grade) was precipitated and centrifuged (speed 3500r / min) to separate. The product was washed with ethanol and then with acetone (CH 3 COCH3 , analytical grade) and dried at 65°C to obtain the HDM-PTGE-CMC sand-fixing sample.

[0051] Example 5

[0052] Deionized water was added to 10 g of sodium carboxymethyl cellulose (CMC) and stirred thoroughly to obtain a CMC aqueous solution, which was adjusted to a pH of 8 using an aqueous NaOH solution (analytical grade), and monomers hydroxymethyl urea (HDM, analytical grade) and PTGE were added to adjust the molar ratio of carboxymethyl cellulose salt, hydroxymethyl urea, and PTGE to 1:2:2.

[0053] Then, nitrogen was introduced for protection and stirred for 30 min. After the solution was fully dissolved, the initiator potassium persulfate solution (K 2 S 2 O 8 After the addition was completed, the reaction system was placed in a 90°C constant temperature water bath and stirred for 5 hours with a stirrer at 500 rpm to allow CMC and HDM to undergo free radical polymerization under the action of the initiator potassium persulfate. The reaction process is as follows: Figure 1 After the reaction was continued at 90°C for 5 h, the product was washed with ethanol (CH 3 CH 2 OH, analytical grade) was precipitated and centrifuged (speed 3500r / min) to separate. The product was washed with ethanol and then with acetone (CH 3 COCH 3 , analytical grade) and dried at 65°C to obtain the HDM-PTGE-CMC sand-fixing sample.

[0054] Example 6

[0055] Deionized water was added to 10 g of ammonium carboxymethyl cellulose and stirred thoroughly to obtain a CMC aqueous solution, which was adjusted to a pH of 9 with an aqueous NaOH solution (analytical grade), and monomers of hydroxymethyl urea (HDM, analytical grade) and PTGE were added to adjust the molar ratio of carboxymethyl cellulose salt, hydroxymethyl urea, and PTGE to 1:2:2.

[0056] Then, nitrogen was introduced for protection and stirred for 30 min. After the solution was fully dissolved, the initiator potassium persulfate solution (K 2 S 2 O 8 After the addition was completed, the reaction system was placed in a constant temperature water bath at 80°C and stirred for 4 hours with a stirrer at 500 rpm to allow CMC and HDM to undergo free radical polymerization under the action of the initiator potassium persulfate. The reaction process is as follows: Figure 1 After 4 h of constant temperature reaction at 80 °C, the product was washed with ethanol (CH 3CH 2 OH, analytical grade) was precipitated and centrifuged (speed 3500r / min) to separate. The product was washed with ethanol and then with acetone (CH 3 COCH 3 , analytical grade) and dried at 65°C to obtain the HDM-PTGE-CMC sand-fixing sample.

[0057] The inventors of this case also tested the antifreeze performance, mechanical strength, water resistance, etc. of the sand-fixing materials obtained in the above embodiments, and the results are as follows:

[0058] In Example 4, the water permeability coefficient of the obtained HDM-PTGE-CMC is 1x10 -3 cm / s, the compressive strength of the sand-fixed sample is 4.5MPa. After curing for 8h, the bonding strength at liquid nitrogen temperature (-210~-196℃) is 5MPa.

[0059] In Example 5, the water permeability coefficient of the obtained HDM-PTGE-CMC is 0.5x10 -3 cm / s, the compressive strength of the sand-fixed sample is 5.5MPa. After curing for 8h, the bonding strength at liquid nitrogen temperature (-210~-196℃) is 6MPa.

[0060] In Example 6, the water permeability coefficient of the obtained HDM-PTGE-CMC is 5.5x10 -4 cm / s, the compressive strength of the sand-fixed sample is 6MPa. After curing for 8h, the bonding strength at liquid nitrogen temperature (-210~-196℃) is 7MPa.

[0061] Example 7

[0062] Deionized water was added to 10 g of calcium carboxymethyl cellulose and stirred thoroughly to obtain a CMC aqueous solution, which was adjusted to a pH of 6 with an aqueous NaOH solution (analytical grade), and monomers hydroxymethyl urea (HDM, analytical grade) and PTGE were added to adjust the molar ratio of carboxymethyl cellulose salt, hydroxymethyl urea, and PTGE to 1:2:2.

[0063] Then, nitrogen was introduced for protection and stirred for 30 min. After the solution was fully dissolved, the initiator potassium persulfate solution (K 2 S 2 O 8 After the addition was completed, the reaction system was placed in a 70°C constant temperature water bath and stirred for 6 hours with a stirrer at 500 rpm to allow CMC and HDM to undergo free radical polymerization under the action of the initiator potassium persulfate. The reaction process is as follows: Figure 1 After 6 h of constant temperature reaction at 70 °C, the product was washed with ethanol (CH 3 CH2 OH, analytical grade) was precipitated and centrifuged (speed 3500r / min) to separate. The product was washed with ethanol and then with acetone (CH 3 COCH 3 , analytical grade) and dried at 65°C to obtain the HDM-PTGE-CMC sand-fixing sample.

[0064] Example 8

[0065] Deionized water was added to 10 g of potassium carboxymethyl cellulose and stirred thoroughly to obtain a CMC aqueous solution, which was adjusted to a pH of 7 with an aqueous NaOH solution (analytical grade), and monomers of hydroxymethyl urea (HDM, analytical grade) and PTGE were added to adjust the molar ratio of carboxymethyl cellulose salt, hydroxymethyl urea, and PTGE to 1:2:2.

[0066] Then, nitrogen was introduced for protection and stirred for 30 min. After the solution was fully dissolved, the initiator potassium persulfate solution (K 2 S 2 O 8 After the addition was completed, the reaction system was placed in a 100°C constant temperature water bath and stirred for 3 hours with a stirrer at 500 rpm to allow CMC and HDM to undergo free radical polymerization under the action of the initiator potassium persulfate. The reaction process is as follows: Figure 1 After the reaction was continued at 100°C for 3 h, the product was washed with ethanol (CH 3 CH 2 OH, analytical grade) was precipitated and centrifuged (speed 3500r / min) to separate. The product was washed with ethanol and then with acetone (CH 3 COCH 3 , analytical grade) and dried at 65°C to obtain the HDM-PTGE-CMC sand-fixing sample.

[0067] Example 9

[0068] Deionized water was added to 10 g of lithium carboxymethyl cellulose and stirred thoroughly to obtain a CMC aqueous solution, which was adjusted to a pH of 8 using an aqueous NaOH solution (analytical grade), and monomers hydroxymethyl urea (HDM, analytical grade) and PTGE were added to adjust the molar ratio of carboxymethyl cellulose salt, hydroxymethyl urea, and PTGE to 1:2:2.

[0069] Then, nitrogen was introduced for protection and stirred for 30 min. After the solution was fully dissolved, the initiator potassium persulfate solution (K 2 S 2 O 8After the addition was completed, the reaction system was placed in a 65°C constant temperature water bath and stirred for 6 hours with a stirrer at 500 rpm to allow CMC and HDM to undergo free radical polymerization under the action of the initiator potassium persulfate. The reaction process is as follows: Figure 1 After the reaction was continued at 65°C for 6 h, the product was washed with ethanol (CH 3 CH 2 OH, analytical grade) was precipitated and centrifuged (speed 3500r / min) to separate. The product was washed with ethanol and then with acetone (CH 3 COCH 3 , analytical grade) and dried at 65°C to obtain the HDM-PTGE-CMC sand-fixing sample.

[0070] The inventors of this case also tested the antifreeze performance, mechanical strength, water resistance, etc. of the sand-fixing materials obtained in the above embodiments, and the results are as follows:

[0071] In Example 7, the water permeability coefficient of the obtained HDM-PTGE-CMC is 1.5x10 -3 cm / s, the compressive strength of the sand-fixed sample is 6MPa. After curing for 8h, the bonding strength at liquid nitrogen temperature (-210~-196℃) is 5MPa.

[0072] In Example 8, the water permeability coefficient of the obtained HDM-PTGE-CMC is 7x10 -4 cm / s cm / s, the compressive strength of the sand-fixed sample is 5.6MPa. After curing for 8 hours, the bonding strength at liquid nitrogen temperature (-210~-196℃) is 7MPa.

[0073] In Example 9, the water permeability coefficient of the obtained HDM-PTGE-CMC is 0.5x10 -3 cm / s, the compressive strength of the sand-fixed sample is 6.0MPa. After curing for 8h, the bonding strength at liquid nitrogen temperature (-210~-196℃) is 6MPa.

[0074] Comparative Example 1

[0075] Compared with Example 1, this comparative example differs in that no hydroxymethyl urea is added. The water permeability coefficient of the obtained sand-fixing material is 2x10 -3 cm / s, the compressive strength of the sand-fixed sample is 4MPa. After curing for 8h, the bonding strength at liquid nitrogen temperature (-210~-196℃) is 4MPa.

[0076] Comparative Example 2

[0077] The difference between this comparative example and Example 1 is that PTGE is not added. The water permeability coefficient of the obtained sand-fixing material is 1.5x10-3 cm / s, the compressive strength of the sand-fixed sample is 5MPa. After curing for 8h, the bonding strength at liquid nitrogen temperature (-210~-196℃) is 3MPa.

[0078] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.

[0079] It should be understood that the above examples are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a hydroxymethylurea-PTGE-carboxymethyl cellulose antifreeze and water-resistant sand-fixing material, characterized in that: include: Mixing carboxymethyl cellulose salt with water to form a carboxymethyl cellulose salt aqueous solution, adjusting the pH value of the carboxymethyl cellulose salt aqueous solution to 6-9 with an alkaline substance, and then adding hydroxymethyl urea and glycerol triglycidyl ether (PTGE) to form the mixed reaction system; the molar ratio of carboxymethyl cellulose salt, hydroxymethyl urea and glycerol triglycidyl ether in the mixed reaction system is 1:1:1-1:2:2; At a temperature between 65 and 100° C., a protective gas is introduced into the mixed reaction system, and then an initiator is added. After sufficient free radical polymerization reaction for 3 to 6 hours, the hydroxymethyl urea-PTGE-carboxymethyl cellulose antifreeze and water-resistant sand-fixing material is obtained.

2. The preparation method according to claim 1, characterized in that: The carboxymethyl cellulose salt includes any one of sodium carboxymethyl cellulose, lithium carboxymethyl cellulose, potassium carboxymethyl cellulose, calcium carboxymethyl cellulose and ammonium carboxymethyl cellulose, or a combination of two or more thereof.

3. The preparation method according to claim 1, characterized in that: The concentration of the initiator added to the mixed reaction system is 0.05-0.25 g / mL.

4. The preparation method according to claim 1, characterized in that: The initiator includes potassium persulfate.

5. The preparation method according to claim 1, characterized in that: The protective gas includes nitrogen.

6. The hydroxymethylurea-PTGE-carboxymethyl cellulose antifreeze and water-resistant sand-fixing material prepared by the preparation method according to any one of claims 1 to 5.

7. The hydroxymethylurea-PTGE-carboxymethyl cellulose antifreeze and water-resistant sand-fixing material according to claim 6, characterized in that: The water permeability coefficient of the hydroxymethylurea-PTGE-carboxymethyl cellulose antifreeze and water-resistant sand-fixing material is 5 × 10 -4 cm / s~ 1.5 × 10 -3 cm / s, the compressive strength of the sand-fixing samples is between 4 and 6 MPa, and after 8 hours of curing, the bonding strength at liquid nitrogen temperatures of -210 to -196 °C is between 3 and 7 MPa.