Polyester resin and its application, and surface decoration material
Polyester resin treated with modified silica and rare earth elements is processed using terahertz laser beam technology to release ultra-far-infrared light waves and far-infrared rays, solving the problems of poor effect and high cost of existing antibacterial and formaldehyde-removing decorative materials, and achieving highly efficient antibacterial and formaldehyde-removing effects.
Patent Information
- Application Number
- CN202310970990.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-02
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-08-02
AI Technical Summary
Existing antibacterial and formaldehyde-removing decorative materials suffer from poor performance and high cost, especially after the decorative surface is covered with dust or the surface resin layer is worn away, the performance is significantly reduced. At the same time, existing materials are not effective or are easily consumed under ultraviolet light.
Polyester resin treated with modified silica and rare earth element compounds CeO2 and Yb2O3 is processed by terahertz laser beam to absorb infrared light waves and release ultra-far-infrared light waves. Combined with nano-sized rare earth element powder, it generates far-infrared rays, achieving ultra-micro energy release and thus achieving antibacterial and formaldehyde-removing effects.
It achieves a 99% antibacterial rate against Staphylococcus aureus and Escherichia coli, a formaldehyde purification rate of 87%, and a durability rate of 70%, while reducing costs and avoiding abnormal pressing problems.
Smart Images

Figure CN116855141B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of facing and decorative materials, and in particular to a polyester resin and its application and facing and decorative materials. Background Art
[0002] The existing antibacterial technologies mainly include silver ions, copper ions, and organic quaternary ammonium salt series. These materials need to be on the surface of the decorative surface. If the decorative surface is covered with dust, the antibacterial performance of the surface will be greatly reduced. Moreover, after the surface resin is worn, the performance will also be reduced.
[0003] The existing formaldehyde removal technologies mainly use chitosan and titanium dioxide photocatalytic formaldehyde removal. These materials are either consumable or require ultraviolet light irradiation to have formaldehyde removal performance, and chitosan needs to be added to the top layer of the decorative surface to be effective. The addition amount also needs to be very high to have a certain effect. This is not only costly, but also very likely to cause various problems in the hot pressing of the top layer of triamine resin, such as incomplete curing, whitening after pressing, bright stars and other problems. Summary of the invention
[0004] The present application provides a polyester resin and its application, and a finishing decorative material to solve the technical problems of poor effect and high cost of existing antibacterial and formaldehyde-free finishing decorative materials.
[0005] In a first aspect, the present application provides a polyester resin, which comprises the following components in parts by weight:
[0006] 75-105 parts of polyester modified polyacrylic acid emulsion, 1-5 parts of 1250-3000 mesh modified silicon dioxide, 0.5-2 parts of rare earth element compound and 14-20 parts of water;
[0007] The modified silicon dioxide is obtained by processing with a terahertz laser beam.
[0008] Furthermore, the polyester resin comprises the following components in parts by weight:
[0009] 80 parts of polyester modified polyacrylic acid emulsion, 2 parts of 1250-3000 mesh modified silicon dioxide, 1 part of rare earth element compound and 14-16 parts of water.
[0010] Furthermore, the polyester-modified polyacrylic acid emulsion is a high-temperature reactive polyester-modified polyacrylic acid emulsion, and the rare earth element compound includes at least one of CeO2 and Yb2O3.
[0011] Furthermore, the polyester resin further comprises, by weight: 0.5 to 2 parts of a penetrant and 0.5 to 2 parts of an anti-settling agent.
[0012] Furthermore, the preparation method of the polyester modified polyacrylic acid emulsion comprises the following steps:
[0013] Mixing polyester resin, hydrophobic monomer, emulsifier and water to obtain a pre-emulsion;
[0014] Add deionized water into the reactor and heat it to 80°C to 95°C to obtain a bottom solution;
[0015] Add the initiator solution to the base liquid, react for 40-60 minutes, then simultaneously drop the pre-emulsion for 5-6 hours, add the neutralizer and external crosslinking agent in sequence after cooling, mix well, and obtain a polyester modified polyacrylic acid emulsion with a solid content of 30wt%-35wt%.
[0016] In a second aspect, the embodiments of the present application provide a use of the polyester resin described in any one of the first aspects in the preparation of a finishing decorative material.
[0017] In a third aspect, an embodiment of the present application provides a finishing decorative material, the finishing decorative material comprising a substrate layer and an ultra-fine energy-releasing resin layer coated on the surface of the substrate layer, wherein both sides of the ultra-fine energy-releasing resin layer are coated with a top coating and a back coating respectively;
[0018] Wherein, the ultra-fine energy releasing resin layer is made of the polyester resin described in any one of the first aspects.
[0019] Furthermore, the substrate layer includes adhesive film paper;
[0020] The top coating comprises the following components in parts by weight:
[0021] 35-45 parts of melamine, 35-45 parts of 35-40wt% formaldehyde solution, 15-30 parts of water, 1-5 parts of diethylene glycol, 1-3 parts of caprolactam, 0.2-1 part of curing agent, 0.2-1 part of dust remover and 0.1-0.5 part of release agent;
[0022] The back coating layer comprises the following components in parts by weight:
[0023] 75-105 parts of polyester modified polyacrylic acid emulsion, 2-10 parts of adhesion monomer, 0.05-0.3 parts of defoaming agent and 0.05-0.3 parts of wetting agent.
[0024] Furthermore, the top coating layer comprises the following components in parts by weight:
[0025] 100 parts of melamine, 115 parts of 37% formaldehyde solution, 50 parts of water, 5 parts of diethylene glycol, 2.5 parts of caprolactam, 0.8 parts of curing agent, 0.5 parts of dust remover and 0.25 parts of release agent;
[0026] The back coating layer comprises the following components in parts by weight:
[0027] 100 parts of polyester modified polyacrylic acid emulsion, 5 parts of adhesion monomer, 0.1 parts of defoaming agent and 0.1 parts of wetting agent.
[0028] In a fourth aspect, an embodiment of the present application provides a method for preparing the facing decorative material according to any one of the third aspects, the preparation method comprising the following steps:
[0029] Impregnating a substrate with the polyester resin described in any one of the first aspects to obtain a substrate impregnated with the polyester resin;
[0030] The substrate impregnated with the polyester resin is first dried, and then a top coating and a back coating are coated on both sides to obtain a semi-finished decorative material;
[0031] performing a second drying on the semi-finished surface decoration material to obtain the surface decoration material;
[0032] Among them, the working parameters of the first drying include: adopting a four-stage drying method, and the temperatures of the four stages of drying are 115-125°C, 125-135°C, 125-135°C and 115-125°C respectively; the working parameters of the second drying include: adopting a five-stage drying method, and the temperatures of the five stages of drying are 125-135°C, 135-145°C, 145-155°C, 135-145°C and 115-125°C respectively.
[0033] The above technical solution provided by the embodiment of the present application has at least the following advantages compared with the prior art:
[0034] The embodiment of the present application provides a polyester resin, which uses 1250-3000 mesh modified silica as a modified matrix, which is low in cost. The 1250-3000 mesh silica is processed by a terahertz laser beam in a terahertz laser beam device, so that it has the ability to release ultra-far infrared, i.e., terahertz, after absorbing infrared light waves, and this ultra-far infrared light wave provides a microenvironment that is not suitable for bacterial growth, thereby inhibiting its growth and killing it. In addition, the released ultra-far infrared light waves and formaldehyde molecules have a resonance effect, so that they can resonate at the same frequency, so that the formaldehyde molecules are decomposed into carbon dioxide and water; trace amounts of rare earth elements such as CeO2 and Yb2O3 are added, and the rare earth elements undergo outer electron transitions after reaching nano-level powders, and also absorb infrared light to generate far infrared rays. The two cooperate with each other and work together to produce a polyester resin with ultra-micro energy release. When applied to finishing materials, the antibacterial rate against Staphylococcus aureus and Escherichia coli reaches 99%, the formaldehyde purification rate is 87%, and the durability rate is 70%, effectively solving the technical problems of poor effect and high cost of existing antibacterial and formaldehyde-free finishing materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.
[0036] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0037] Figure 1 A schematic diagram of the structure of a surface decoration material provided in an embodiment of the present application;
[0038] in, Figure 1 Middle: 1-substrate layer; 2-ultra-fine energy-releasing resin layer; 3-back coating layer; 4-top coating layer. DETAILED DESCRIPTION
[0039] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0040] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.
[0041] In a first aspect, the present application provides a polyester resin, which comprises the following components in parts by weight:
[0042] 75-105 parts of polyester modified polyacrylic acid emulsion, 1-5 parts of 1250-3000 mesh modified silicon dioxide, 0.5-2 parts of rare earth element compound and 14-20 parts of water;
[0043] The modified silicon dioxide is obtained by processing with a terahertz laser beam.
[0044] The embodiment of the present application provides a polyester resin, which uses 1250-3000 mesh modified silica as a modified matrix, which is low in cost. The 1250-3000 mesh silica is processed by a terahertz laser beam in a terahertz laser beam device, so that it has the ability to release ultra-far infrared, i.e., terahertz, after absorbing infrared light waves, and this ultra-far infrared light wave provides a microenvironment that is not suitable for bacterial growth, thereby inhibiting its growth and killing it. In addition, the released ultra-far infrared light waves and formaldehyde molecules have a resonance effect, so that they can resonate at the same frequency, so that the formaldehyde molecules are decomposed into carbon dioxide and water; trace amounts of rare earth elements such as CeO2 and Yb2O3 are added, and the rare earth elements undergo outer electron transitions after reaching nano-level powders, and also absorb infrared light to generate far infrared rays. The two cooperate with each other and work together to produce a polyester resin with ultra-micro energy release. When applied to finishing materials, the antibacterial rate against Staphylococcus aureus and Escherichia coli reaches 99%, the formaldehyde purification rate is 87%, and the durability rate is 70%, effectively solving the technical problems of poor effect and high cost of existing antibacterial and formaldehyde-free finishing materials.
[0045] Preferably, the polyester resin comprises the following components in parts by weight:
[0046] 80 parts of polyester modified polyacrylic acid emulsion, 2 parts of 1250-3000 mesh modified silicon dioxide, 1 part of rare earth element compound and 14-16 parts of water.
[0047] As an implementation of an example of the present application, the polyester-modified polyacrylic acid emulsion is a high-temperature reactive polyester-modified polyacrylic acid emulsion, and the rare earth element compound includes at least one of CeO2 and Yb2O3.
[0048] In some specific embodiments, the preparation method of the modified silicon dioxide comprises: processing 1250-3000 mesh silicon dioxide in a terahertz laser beam device, adjusting the device temperature to 40 degrees for 48 hours to obtain modified silicon dioxide.
[0049] As an implementation of an embodiment of the present application, the polyester resin further includes, by weight: 0.5 to 2 parts of a penetrant and 0.5 to 2 parts of an anti-settling agent.
[0050] The present application adds a penetrant when preparing the polyester resin, thereby improving the permeability of the subsequent primer glue solution to the paper, solving the problem of uneven glue penetration into the paper, causing the paper to break easily; at the same time, it also solves the problem of poor water resistance caused by the subsequent migration of small molecules caused by the externally added penetrant.
[0051] In the present application, an anti-settling agent is added during the preparation of the polyester resin, so that the system has thixotropy and the viscosity is greatly improved, which is beneficial for storage and coating.
[0052] As an implementation method of the present application, the preparation method of the polyester modified polyacrylic acid emulsion comprises the following steps:
[0053] Mixing a polyester resin, a hydrophobic monomer (such as styrene, butadiene, vinyl ester, (meth)acrylate or a combination thereof), an emulsifier and water to obtain a pre-emulsion;
[0054] Add deionized water into the reactor and heat it to 80°C to 95°C to obtain a bottom solution;
[0055] Add the initiator solution to the base liquid, react for 40-60 minutes, then simultaneously drop the pre-emulsion for 5-6 hours, add the neutralizer and external crosslinking agent in sequence after cooling, mix well, and obtain a polyester modified polyacrylic acid emulsion with a solid content of 30wt%-35wt%.
[0056] The preparation method of the polyester modified polyacrylic acid emulsion provided in the present application is simple to operate, does not require additional specific production equipment, and is suitable for industrial production.
[0057] In a second aspect, the embodiments of the present application provide a use of the polyester resin described in any one of the first aspects in the preparation of a finishing decorative material.
[0058] The decorative surface material prepared by the polyester resin provided in the embodiment of the present application has low cost and excellent antibacterial effect and formaldehyde removal effect. At the same time, the decorative surface material is realized based on the polyester resin described in any one of the first aspects above, and therefore has at least all the beneficial effects brought by the technical solutions of the above embodiments, which will not be described one by one here.
[0059] In a third aspect, the present application provides a finishing material, such as Figure 1 As shown, the surface decoration material comprises a substrate layer 1 and an ultra-fine energy-releasing resin layer 2 coated on the surface of the substrate layer 1, and both sides of the ultra-fine energy-releasing resin layer 1 are coated with a top coating layer 4 and a back coating layer 3 respectively;
[0060] Wherein, the ultra-fine energy releasing resin layer 2 is made of the polyester resin described in any one of the first aspects.
[0061] The "ultrafine energy release" mentioned in the present application can be understood as ultrafine energy release performed by modified silica and ultra-far infrared waves of rare earth elements.
[0062] The polyester resin material with ultra-micro energy in the decorative surface material provided by the present application does not act on the decorative surface coating, because the ultra-far infrared released by it can easily penetrate the decorative surface layer to play a role, so there will be no abnormal pressing problem. At the same time, the decorative surface material is realized based on the polyester resin described in any one of the first aspects above, so it has at least all the beneficial effects brought by the technical solutions of the above embodiments, which will not be repeated here one by one.
[0063] As an implementation method of the present application, the substrate layer includes adhesive film paper;
[0064] The top coating comprises the following components in parts by weight:
[0065] 35-45 parts of melamine, 35-45 parts of 35-40wt% formaldehyde solution, 15-30 parts of water, 1-5 parts of diethylene glycol, 1-3 parts of caprolactam, 0.2-1 part of curing agent, 0.2-1 part of dust remover and 0.1-0.5 part of release agent;
[0066] The back coating layer comprises the following components in parts by weight:
[0067] 75-105 parts of polyester modified polyacrylic acid emulsion, 2-10 parts of adhesion monomer, 0.05-0.3 parts of defoaming agent and 0.05-0.3 parts of wetting agent.
[0068] The surface coating in the finishing and decorative material provided in the embodiment of the present application needs to have good physical properties after film formation, such as wear resistance, scratch resistance, stain resistance, water vapor resistance, crack resistance, etc.
[0069] The back coating layer of the facing decorative material provided in the embodiment of the present application adopts a formaldehyde-free polyester resin formula and contains adhesion monomers and high-temperature reactive polyester modified polyacrylic acid emulsion. The formaldehyde-free impregnated back coating adhesive is prepared by introducing adhesion-enhancing monomers into the resin structure to increase the functional groups of the hydroxyl group bonding reaction on the paper and board, thereby improving the bonding strength of the paper and the board when pressed, and solving the problem of poor adhesion of the impregnated paper pressed onto the board.
[0070] Therefore, in addition to the antibacterial and formaldehyde-free effects, the finishing and decorative material provided in the embodiment of the present application uses a formaldehyde-containing triamine resin only in the top coating, while neither the first dipping nor the back glue uses a formaldehyde-containing resin. Therefore, the formaldehyde emission of the adhesive paper made from this product is directly lower than 0.1%, and after pressing and film formation, the formaldehyde emission reaches a nearly formaldehyde-free effect.
[0071] Preferably, the top coating comprises the following components in parts by weight:
[0072] 100 parts of melamine, 115 parts of 37% formaldehyde solution, 50 parts of water, 5 parts of diethylene glycol, 2.5 parts of caprolactam, 0.8 parts of curing agent, 0.5 parts of dust remover and 0.25 parts of release agent;
[0073] The back coating layer comprises the following components in parts by weight:
[0074] 100 parts of polyester modified polyacrylic acid emulsion, 5 parts of adhesion monomer, 0.1 parts of defoaming agent and 0.1 parts of wetting agent.
[0075] In a fourth aspect, an embodiment of the present application provides a method for preparing the facing decorative material according to any one of the third aspects, the preparation method comprising the following steps:
[0076] Impregnating a substrate with the polyester resin described in any one of the first aspects to obtain a substrate impregnated with the polyester resin;
[0077] The substrate impregnated with the polyester resin is first dried, and then a top coating and a back coating are coated on both sides to obtain a semi-finished decorative material;
[0078] performing a second drying on the semi-finished surface decoration material to obtain the surface decoration material;
[0079] Among them, the working parameters of the first drying include: adopting a four-stage drying method, and the temperatures of the four stages of drying are 115-125°C, 125-135°C, 125-135°C and 115-125°C respectively; the working parameters of the second drying include: adopting a five-stage drying method, and the temperatures of the five stages of drying are 125-135°C, 135-145°C, 145-155°C, 135-145°C and 115-125°C respectively.
[0080] In some specific embodiments, the preparation method of the above-mentioned surface decoration material is tested according to the steps of dipping in formaldehyde-free glue, back coating with formaldehyde-free glue, and surface coating with triamine glue. The specific steps are as follows:
[0081] S1: Preparation of high temperature reactive polyester modified polyacrylic acid emulsion:
[0082] (1) First, disperse the polyester resin, hydrophobic monomer, emulsifier and deionized water at 1000 r / min to form a pre-emulsion.
[0083] (2) adding deionized water into the reactor and heating it to 80°C to 95°C;
[0084] (3) Add the initiator solution to the base liquid, react for 40-60 minutes, and then simultaneously add the pre-emulsion dropwise for 5-6 hours, and then cool;
[0085] (4) adding a neutralizing agent and an external crosslinking agent in sequence and mixing them uniformly to obtain a high temperature reactive polyester modified polyacrylic acid emulsion with a solid content of 30-35%.
[0086] S2: Preparation of one-dip formaldehyde-free glue: add high-temperature reactive polyester modified polyacrylic acid emulsion into a reactor, add distilled water to reduce the solid content of the temperature reactive polyester modified polyacrylic acid emulsion to 25-30%, add penetrant and anti-settling agent, and perform shear dispersion at 400r / min for 20-30min, then add modified 1250-3000 mesh silica and rare earth elements CeO2 / Yb2O3, and perform shear dispersion at 500r / min for 30-40min to obtain one-dip formaldehyde-free resin glue.
[0087] S3: Prepare the back-coated formaldehyde-free adhesive, add the high-temperature reactive polyester modified polyacrylic acid emulsion into the reactor, add the adhesion monomer, defoamer and wetting agent at one time, and perform shear dispersion at 400r / min for 20-30min.
[0088] Get back-coated formaldehyde-free glue.
[0089] S4: Prepare the top-coated triamine glue for standby use, add 37% formaldehyde solution into the reactor, adjust the pH to 7-8 with 40% sodium hydroxide, add melamine, start stirring and heating, stirring speed 200r / min, heating from 40℃ to 90℃, time is 40-50min, add diethylene glycol and caprolactam, keep warm at 90-95℃ for 80-100min, test the water solubility ratio of the resin, and finally end when the water solubility ratio is 2.0, start cooling to room temperature, and obtain the top-coated triamine glue. Add curing agent, release agent, and dust remover to obtain the triamine resin glue that can be put on the machine.
[0090] S5: Inject the first dip formaldehyde-free resin, the back-coated formaldehyde-free glue, and the surface-coated triamine resin glue into the dipping machine, select a certain amount of paper for dipping production, and perform the dipping process in sequence. Use the first dip formaldehyde-free resin to impregnate the substrate paper; after a first oven drying (120℃, 130℃, 130℃, 120℃); perform the second dip, apply the back-coated formaldehyde-free glue, the surface-coated triamine resin glue, perform the second drying and winding: two (130℃, 140℃, 150℃, 140℃, 120℃), and wind up after the cooling section.
[0091] S6: Cut the paper into the required size of the board, place the substrate, put it into the hot press, press it for 20-30s at a temperature of 180-190°C and a pressure of 10-15MPa to obtain an ultra-fine energy space antibacterial formaldehyde-free decorative board (i.e., decorative material).
[0092] S7: Test the physical properties of ultra-fine energy space antibacterial and formaldehyde-free decorative panels.
[0093] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.
[0094] Embodiments 1 to 5 and comparative example 1 provide a kind of facing decoration material, specifically a kind of ultra-fine energy space antibacterial formaldehyde-free facing decoration material, measured in parts by weight (unit is g), and the specific dosage of each example is shown in Table 1; wherein, the rare earth elements in embodiments 1 to 3 and comparative example 1 are all CeO2, the rare earth elements in embodiments 4 to 5 are all Yb2O3, the penetrant is specifically fatty alcohol polyoxyethylene ether, the anti-settling agent is specifically polyamide wax anti-settling agent, the adhesion monomer is specifically methacryloyloxyethyl phosphate, the defoaming agent is specifically polydimethylsiloxane, the curing agent is specifically p-toluenesulfonic acid + morpholine + water mixed in a weight ratio of 1:1:1, the dust remover is specifically polyether polyol, and the release agent is specifically methyl silicone oil + polymethyl silicone resin silicone resin mixed in a weight ratio of 1:1:1.
[0095] Table 1
[0096]
[0097] Examples 1-5 and Comparative Example 1 were tested by weighing a certain amount of components according to Table 1, and the test was carried out according to the glue making steps of dipping in formaldehyde-free glue, back coating with formaldehyde-free glue, and surface coating with triamine glue. The specific steps are as follows:
[0098] S1: A high temperature reactive polyester modified polyacrylic acid emulsion was obtained, which was purchased directly from Hunan Linte Technology Co., Ltd., and the product model is 1118N.
[0099] S2: Preparation of one-dip formaldehyde-free glue: add high-temperature reactive polyester modified polyacrylic acid emulsion into a reactor, add distilled water to reduce the solid content of the temperature reactive polyester modified polyacrylic acid emulsion to 25-30%, add penetrant and anti-settling agent, and perform shear dispersion at 400r / min for 20-30min, then add modified 1250-3000 mesh silica and rare earth elements CeO2 / Yb2O3, and perform shear dispersion at 500r / min for 30-40min to obtain one-dip formaldehyde-free resin glue.
[0100] S3: Prepare the back-coated formaldehyde-free adhesive, add the high-temperature reactive polyester modified polyacrylic acid emulsion into the reactor, add the adhesion monomer, defoamer and wetting agent at one time, and perform shear dispersion at 400r / min for 20-30min.
[0101] Get back-coated formaldehyde-free glue.
[0102] S4: Prepare the top-coated triamine glue for standby use, add 37% formaldehyde solution into the reactor, adjust the pH to 7-8 with 40% sodium hydroxide, add melamine, start stirring and heating, stirring speed 200r / min, heating from 40℃ to 90℃, time is 40-50min, add diethylene glycol and caprolactam, keep warm at 90-95℃ for 80-100min, test the water solubility ratio of the resin, and finally end when the water solubility ratio is 2.0, start cooling to room temperature, and obtain the top-coated triamine glue. Add curing agent, release agent, and dust remover to obtain the triamine resin glue that can be put on the machine.
[0103] S5: Inject the first dip formaldehyde-free resin, the back-coated formaldehyde-free glue, and the surface-coated triamine resin glue into the dipping machine, select a certain amount of paper for dipping production, and perform the dipping process in sequence. Use the first dip formaldehyde-free resin to impregnate the substrate paper; after a first oven drying (120℃, 130℃, 130℃, 120℃); perform the second dip, apply the back-coated formaldehyde-free glue, the surface-coated triamine resin glue, perform the second drying and winding: two (130℃, 140℃, 150℃, 140℃, 120℃), and wind up after the cooling section.
[0104] S6: Cut the paper into the required size of the board, place the substrate, put it into the hot press, press it for 20-30s at a temperature of 180-190℃ and a pressure of 10-15MPa to obtain an ultra-fine energy space antibacterial and formaldehyde-free decorative board.
[0105] S7: Test the physical properties of ultra-fine energy space antibacterial and formaldehyde-free decorative panels.
[0106] The physical properties of the veneered artificial board obtained were tested according to the testing standards (GB 18580-2017 "Limits of formaldehyde emission from artificial boards and their products for interior decoration and renovation materials"; GB / T 34722-2017 "Impregnated film paper veneer plywood and blockboard" GB / T 15102-2017 "Impregnated film paper veneer fiberboard and particleboard"; JIS A 1460-2001 "Test method for formaldehyde emission of building boards"; GB / T 17657-2013 "Test method for physical and chemical properties of artificial boards and veneered artificial boards"). The results are shown in Table 2.
[0107] Table 2
[0108]
[0109]
[0110] As shown in Table 2, the formaldehyde release of the ultra-micro energy space antibacterial formaldehyde-free decorative panels prepared in Examples 1 to 5 is 0.1 mg / L, while the formaldehyde release of Comparative 1 is 0.3 mg / L.
[0111] It can be seen from Table 2 that the ultra-micro energy space antibacterial formaldehyde-free decorative panels prepared using Examples 1-5 of the present invention and Comparative Example 1 exhibit excellent wear resistance, scratch resistance, pollution resistance and corrosion resistance, light fastness and dry heat resistance, and the peel strength reaches 45 N / m or above.
[0112] It can be seen from Table 2 that the ultra-fine energy space antibacterial and formaldehyde-free decorative panels have excellent antibacterial, mildew-proof and formaldehyde-free functions. Compared with Example 1, the antibacterial, mildew-proof and formaldehyde-free effects are not ideal.
[0113] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0114] In the present application, in the absence of any contrary description, the directional words used, such as "upper" and "lower", are specifically the directions of the drawings in the accompanying drawings. In addition, in the description of the present specification, the terms "including", "comprising", etc. refer to "including but not limited to". In this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of the associated objects, indicating that there may be three relationships, for example, A and / or B, which can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A, B can be singular or plural. In this article, "at least one" refers to one or more, and "plural" refers to two or more. "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of singular or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c", can both mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or plural, respectively.
[0115] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
Claims
1. A surface decoration material, characterized in that: The surface decoration material comprises a substrate layer and an ultra-fine energy-releasing resin layer coated on the surface of the substrate layer, and both sides of the ultra-fine energy-releasing resin layer are coated with a top coating and a back coating respectively; Wherein, the ultra-fine energy release resin layer is made of polyester resin; The polyester resin comprises the following components in parts by weight: 80 parts of polyester modified polyacrylic acid emulsion, 2 parts of modified silica of 1250-3000 mesh, 1 part of rare earth element compound, 14-16 parts of water, 0.5-2 parts of penetrant and 0.5-2 parts of anti-settling agent; The modified silicon dioxide is obtained by processing with a terahertz laser beam; The polyester-modified polyacrylic acid emulsion is a high-temperature reactive polyester-modified polyacrylic acid emulsion, and the rare earth element compound includes at least one of CeO2 and Yb2O3; The preparation method of the polyester modified polyacrylic acid emulsion comprises the following steps: Mixing polyester resin, hydrophobic monomer, emulsifier and water to obtain a pre-emulsion; Add deionized water into the reactor and heat it to 80°C to 95°C to obtain a bottom solution; Adding the initiator solution to the base liquid, reacting for 40-60 minutes, and then simultaneously dropping the pre-emulsion for 5-6 hours, and adding the neutralizer and the external crosslinking agent in sequence after cooling, and mixing evenly to obtain a polyester-modified polyacrylic acid emulsion with a solid content of 30wt%-35wt%; The substrate layer includes film paper; The top coating comprises the following components in parts by weight: 35-45 parts of melamine, 35-45 parts of 35-40wt% formaldehyde solution, 15-30 parts of water, 1-5 parts of diethylene glycol, 1-3 parts of caprolactam, 0.2-1 part of curing agent, 0.2-1 part of dust remover and 0.1-0.5 part of release agent; The back coating layer comprises the following components in parts by weight: 75-105 parts of polyester modified polyacrylic acid emulsion, 2-10 parts of adhesion monomer, 0.05-0.3 parts of defoaming agent and 0.05-0.3 parts of wetting agent; The preparation method comprises the following steps: impregnating the substrate with a polyester resin to obtain a substrate impregnated with the polyester resin; The substrate impregnated with the polyester resin is first dried, and then a top coating and a back coating are coated on both sides to obtain a semi-finished decorative material; performing a second drying on the semi-finished surface decoration material to obtain the surface decoration material; The working parameters of the first drying include: a four-stage drying method, wherein the temperatures of the four stages are 115-125°C, 125-135°C, 125-135°C and 115-125°C respectively; the working parameters of the second drying method include: a five-stage drying method, wherein the temperatures of the five stages are 125-135°C, 135-145°C, 145-155°C, 135-145°C and 115-125°C respectively; The curing agent is a mixture of p-toluenesulfonic acid, morpholine and water in a weight ratio of 1:1:1; The release agent is a mixture of methyl silicone oil, polymethyl silicone resin and silicone resin in a weight ratio of 1:1:
1.
2. The surface decoration material according to claim 1, characterized in that: The top coating comprises the following components in parts by weight: 100 parts of melamine, 115 parts of 37% formaldehyde solution, 50 parts of water, 5 parts of diethylene glycol, 2.5 parts of caprolactam, 0.8 parts of curing agent, 0.5 parts of dust remover and 0.25 parts of release agent; The back coating layer comprises the following components in parts by weight: 100 parts of polyester modified polyacrylic acid emulsion, 5 parts of adhesion monomer, 0.1 parts of defoaming agent and 0.1 parts of wetting agent.