Preparation method of battery connector, battery connector and battery

By mixing cobalt nitrate, nickel and magnesium powder with fluoride electrolyte for electrodeposition, forming a protective layer of the SOFC battery connector, solving the problems of high cost and complex steps in traditional methods, and achieving efficient preparation of the battery connector.

CN116856023BActive Publication Date: 2024-11-26PETROCHINA SHENZHEN NEW ENERGY RESEARCH INSTITUTE CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311131906.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-04
Publication Date
2024-11-26
Estimated Expiration
2043-09-04

AI Technical Summary

Technical Problem

The preparation method of traditional SOFC battery connectors is costly and complicated, and requires a sintering process, resulting in low preparation efficiency.

Method used

Cobalt nitrate powder, nickel nitrate powder and magnesium nitrate powder are mixed with electrolytes of sodium fluoride, potassium fluoride and lithium chloride for electrodeposition to form a protective layer to simplify the preparation process.

Benefits of technology

The preparation cost of battery connectors is greatly reduced, the steps are simplified, and the preparation efficiency is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116856023B_ABST
    Figure CN116856023B_ABST
Patent Text Reader

Abstract

The present invention relates to a preparation method of a battery connector, a battery connector and a battery. The preparation method of the battery connector comprises: preparing a powder mixture, the powder mixture is a mixture containing cobalt nitrate powder, nickel nitrate powder and magnesium nitrate powder; preparing a first electrolyte, the first electrolyte is an electrolyte containing sodium fluoride, potassium fluoride and lithium chloride; mixing the powder mixture with the first electrolyte to obtain a second electrolyte; placing a connector substrate in the second electrolyte for an electrodeposition process, forming a protective layer on the surface of the connector substrate to obtain a battery connector.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of batteries, and in particular to a method for preparing a battery connector, a battery connector and a battery. Background Art

[0002] The connectors of traditional SOFC cells (Solid oxide fuel cell) generally use metal sheets such as silver, platinum, and gold, or current collecting materials such as silver paste, platinum paste, and gold paste, and the preparation process requires the use of a sintering process. As a result, conventional battery connector preparation methods have problems such as high preparation costs and complex preparation steps. Summary of the invention

[0003] In view of this, the present invention provides a method for preparing a battery connector, a battery connector and a battery.

[0004] Specifically, the present invention is achieved through the following technical solutions:

[0005] According to a first aspect of the present invention, a method for preparing a battery connector is provided, the method comprising: preparing a powder mixture, the powder mixture being a mixture containing cobalt nitrate powder, nickel nitrate powder and magnesium nitrate powder; preparing a first electrolyte, the first electrolyte being an electrolyte containing sodium fluoride, potassium fluoride and lithium chloride; mixing the powder mixture with the first electrolyte to obtain a second electrolyte; placing a connector substrate in the second electrolyte for an electrodeposition process to form a protective layer on the surface of the connector substrate to obtain a battery connector.

[0006] The preparation method of the battery connector in the present technical solution is to mix cobalt nitrate powder, nickel nitrate powder and magnesium nitrate powder to obtain a powder mixture, prepare a first electrolyte, and then add the powder mixture to the first electrolyte for mixing to obtain a second electrolyte, place a connector substrate in the second electrolyte, and perform an electrodeposition process on the connector substrate to form a protective layer on the surface of the connector substrate to obtain a battery connector, which greatly reduces the preparation cost of the battery connector, simplifies the preparation steps of the battery connector, and improves the preparation efficiency of the battery connector.

[0007] According to a second aspect of the present invention, there is provided a battery connector, which is manufactured by the method for manufacturing a battery connector in any possible implementation of the first aspect.

[0008] According to a third aspect of the present invention, there is provided a battery, the battery comprising the battery connector in any possible implementation manner of the second aspect.

[0009] The technical solution provided by the present invention brings at least the following beneficial effects:

[0010] The preparation cost of the battery connector is greatly reduced, the preparation steps of the battery connector are simplified, and the preparation efficiency of the battery connector is improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.

[0012] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or related technical descriptions are briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0013] Figure 1 One of the flow diagrams of a method for preparing a battery connector provided by an embodiment of the present invention;

[0014] Figure 2 A second schematic flow chart of a method for preparing a battery connector provided by an embodiment of the present invention;

[0015] Figure 3 A third flow chart of a method for preparing a battery connector provided by an embodiment of the present invention;

[0016] Figure 4 A fourth flow chart of a method for preparing a battery connector provided by an embodiment of the present invention;

[0017] Figure 5 A fifth flow chart of a method for preparing a battery connector provided by an embodiment of the present invention;

[0018] Figure 6 The sixth flow chart of a method for preparing a battery connector provided in an embodiment of the present invention. DETAILED DESCRIPTION

[0019] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0020] See also Figure 1 The present invention provides a method for preparing a battery connector, which may include the following steps:

[0021] S101, preparing a powder mixture, wherein the powder mixture is a mixture containing cobalt nitrate powder, nickel nitrate powder and magnesium nitrate powder;

[0022] S102, preparing a first electrolyte, wherein the first electrolyte is an electrolyte containing sodium fluoride, potassium fluoride and lithium chloride;

[0023] S103, mixing the powder mixture with the first electrolyte to obtain a second electrolyte;

[0024] S104, placing the interconnect substrate in a second electrolyte to perform an electrodeposition process, forming a protective layer on the surface of the interconnect substrate to obtain a battery interconnect.

[0025] In this embodiment, a method for preparing a battery connector is provided, wherein the connector is a component of a battery.

[0026] In some embodiments, the interconnect may specifically be an interconnect of a SOFC cell.

[0027] Cobalt nitrate powder, nickel nitrate powder and magnesium nitrate powder are mixed to obtain a powder mixture, wherein the powder mixture is a mixture of cobalt nitrate powder, nickel nitrate powder and magnesium nitrate powder.

[0028] In some embodiments, the mass ratio of cobalt nitrate powder, nickel nitrate powder and magnesium nitrate powder in the powder mixture may be 1:1:3.

[0029] A first electrolyte is prepared, wherein the first electrolyte is an electrolyte containing sodium fluoride, potassium fluoride and lithium chloride.

[0030] In some embodiments, the mass ratio of sodium fluoride, potassium fluoride and lithium chloride in the first electrolyte can be 1:1:1.

[0031] The powder mixture is added into the first electrolyte and mixed to obtain a second electrolyte, wherein the second electrolyte is an electrolyte containing the powder mixture.

[0032] In some embodiments, the mass ratio of the powder mixture in the second electrolyte to the first electrolyte may be 1:100.

[0033] The connector substrate is placed in a second electrolyte and subjected to an electrodeposition process to form a protective layer on the surface of the connector substrate to obtain a battery connector, wherein the connector substrate is a metal substrate for preparing the connector.

[0034] In some embodiments, a second electrolyte may be placed in an electrolytic cell, and the interconnect substrate may be placed in the second electrolyte to perform an electrodeposition process.

[0035] The preparation method of the battery connector in this embodiment mixes cobalt nitrate powder, nickel nitrate powder and magnesium nitrate powder to obtain a powder mixture, prepares a first electrolyte, and then adds the powder mixture to the first electrolyte for mixing to obtain a second electrolyte, places a connector substrate in the second electrolyte, and performs an electrodeposition process on the connector substrate to form a protective layer on the surface of the connector substrate to obtain a battery connector, which greatly reduces the preparation cost of the battery connector, simplifies the preparation steps of the battery connector, and improves the preparation efficiency of the battery connector.

[0036] See also Figure 2 The present invention provides a method for preparing a battery connector, which may include the following steps:

[0037] S201, mixing cobalt nitrate powder, nickel nitrate powder and magnesium nitrate powder to obtain a powder mixture;

[0038] S202, preparing a first electrolyte, wherein the first electrolyte is an electrolyte containing sodium fluoride, potassium fluoride and lithium chloride;

[0039] S203, mixing the powder mixture with the first electrolyte to obtain a second electrolyte;

[0040] S204, placing the interconnect substrate in a second electrolyte to perform an electrodeposition process, forming a protective layer on the surface of the interconnect substrate to obtain a battery interconnect.

[0041] In this embodiment, cobalt nitrate powder, nickel nitrate powder and magnesium nitrate powder are stirred and mixed to obtain a powder mixture.

[0042] In some embodiments, the mass ratio of cobalt nitrate powder, nickel nitrate powder and magnesium nitrate powder is set to 1:1:4, and they are mixed to obtain a powder mixture.

[0043] In the preparation method of the battery connector in this embodiment, cobalt nitrate powder, nickel nitrate powder and magnesium nitrate powder are stirred and mixed to obtain a powder mixture, thereby ensuring the accuracy of the composition of the powder mixture.

[0044] See also Figure 3 The present invention provides a method for preparing a battery connector, which may include the following steps:

[0045] S301, preparing a powder mixture, wherein the powder mixture is a mixture containing cobalt nitrate powder, nickel nitrate powder and magnesium nitrate powder;

[0046] S302, mixing sodium fluoride, potassium fluoride and lithium chloride in a solution to obtain a first electrolyte;

[0047] S303, mixing the powder mixture with the first electrolyte to obtain a second electrolyte;

[0048] S304, placing the interconnect substrate in a second electrolyte to perform an electrodeposition process, forming a protective layer on the surface of the interconnect substrate to obtain a battery interconnect.

[0049] In this embodiment, sodium fluoride, potassium fluoride and lithium chloride are added to a solution and stirred and mixed to obtain a first electrolyte.

[0050] In some embodiments, the mass ratio of sodium fluoride, potassium fluoride and lithium chloride is set to 1:1:8, and added into the solution for stirring and mixing to obtain a first electrolyte.

[0051] In the preparation method of the battery connector in this embodiment, sodium fluoride, potassium fluoride and lithium chloride are added into a solution and stirred to obtain a first electrolyte, thereby ensuring the accuracy of the composition of the first electrolyte.

[0052] See also Figure 4 The present invention provides a method for preparing a battery connector, which may include the following steps:

[0053] S401, preparing a powder mixture, wherein the powder mixture is a mixture containing cobalt nitrate powder, nickel nitrate powder and magnesium nitrate powder;

[0054] S402, preparing a first electrolyte, wherein the first electrolyte is an electrolyte containing sodium fluoride, potassium fluoride and lithium chloride;

[0055] S403, mixing the powder mixture with the first electrolyte to obtain a second electrolyte;

[0056] S404, connecting the connector substrate and the electrodeposition device;

[0057] S405, connecting the negative electrode substrate to the electrodeposition device;

[0058] S406, placing the connector matrix and the negative electrode matrix in a second electrolyte;

[0059] S407, performing an electrodeposition process on the second electrolyte by using an electrodeposition device to form a protective layer on the surface of the connector substrate to obtain a battery connector.

[0060] In this embodiment, the interconnect substrate is connected to an electrodeposition device, and then the negative electrode substrate is connected to the electrodeposition device, wherein the electrodeposition device is a device capable of performing an electrodeposition process.

[0061] In some embodiments, the electrodeposition device may include a power source, a cathode, an anode and other components, the connector substrate is connected to the anode of the electrodeposition device, and the negative electrode substrate is connected to the cathode of the electrodeposition device.

[0062] The connector substrate and the negative electrode substrate are placed in a second electrolyte, and the electrodeposition device is turned on to perform an electrodeposition process on the second electrolyte to form a protective layer on the surface of the connector substrate to obtain a battery connector.

[0063] In some embodiments, the electrodeposition device may include an electrolytic cell, a power source, a cathode, an anode and other components. The connector substrate is connected to the anode of the electrodeposition device, and the negative electrode substrate is connected to the cathode of the electrodeposition device. A second electrolyte is added to the electrolytic cell, and the connector substrate and the negative electrode substrate are placed in the second electrolyte respectively. The power source of the electrodeposition device is turned on, and the second electrolyte is subjected to an electrodeposition process to form a protective layer on the surface of the connector substrate to obtain a battery connector.

[0064] The preparation method of the battery connector in this embodiment connects the connector substrate and the electrodeposition device, then connects the negative electrode substrate and the electrodeposition device, and places the connector substrate and the negative electrode substrate in a second electrolyte, starts the electrodeposition device, and performs an electrodeposition process on the second electrolyte to form a protective layer on the surface of the connector substrate to obtain a battery connector. The electrodeposition process simplifies the preparation steps of the battery connector and improves the preparation efficiency of the battery connector.

[0065] See also Figure 5 The present invention provides a method for preparing a battery connector, which may include the following steps:

[0066] S501, preparing a powder mixture, wherein the powder mixture is a mixture containing cobalt nitrate powder, nickel nitrate powder and magnesium nitrate powder;

[0067] S502, preparing a first electrolyte, wherein the first electrolyte is an electrolyte containing sodium fluoride, potassium fluoride and lithium chloride;

[0068] S503, mixing the powder mixture with the first electrolyte to obtain a second electrolyte;

[0069] S504, connecting the connector substrate to the power anode of the electrodeposition device;

[0070] S505, connecting the negative electrode substrate to the electrodeposition device;

[0071] S506, placing the connector matrix and the negative electrode matrix in a second electrolyte;

[0072] S507 , performing an electrodeposition process on the second electrolyte by using an electrodeposition device to form a protective layer on the surface of the connector substrate to obtain a battery connector.

[0073] In this embodiment, the interconnect substrate is connected to a power supply anode of an electrodeposition device, wherein the power supply anode is a component of the electrodeposition device.

[0074] The preparation method of the battery connector in this embodiment connects the connector substrate to the power anode of the electrodeposition device, ensuring the normal progress of the electrodeposition process.

[0075] See also Figure 6 The present invention provides a method for preparing a battery connector, which may include the following steps:

[0076] S601, preparing a powder mixture, wherein the powder mixture is a mixture containing cobalt nitrate powder, nickel nitrate powder and magnesium nitrate powder;

[0077] S602, preparing a first electrolyte, wherein the first electrolyte is an electrolyte containing sodium fluoride, potassium fluoride and lithium chloride;

[0078] S603, mixing the powder mixture with the first electrolyte to obtain a second electrolyte;

[0079] S604, connecting the connector substrate and the electrodeposition device;

[0080] S605, connecting the negative electrode substrate to the power cathode of the electrodeposition device;

[0081] S606, placing the connector matrix and the negative electrode matrix in a second electrolyte;

[0082] S607 , performing an electrodeposition process on the second electrolyte by using an electrodeposition device to form a protective layer on the surface of the connector substrate to obtain a battery connector.

[0083] In this embodiment, the negative electrode substrate is connected to a power supply cathode of the electrodeposition device, wherein the power supply cathode is a component of the electrodeposition device.

[0084] The method for preparing the battery connector in this embodiment connects the negative electrode substrate to the power cathode of the electrodeposition device, ensuring the normal progress of the electrodeposition process.

[0085] Based on the same inventive concept, an embodiment of the present invention provides a method for preparing a battery connector, wherein the material of the negative electrode substrate is graphite material.

[0086] In this embodiment, the material of the negative electrode substrate is limited to graphite material, which ensures the normal progress of the electrodeposition process.

[0087] Based on the same inventive concept, an embodiment of the present invention provides a method for preparing a battery connector, wherein the material of the negative electrode substrate is a silicon-oxygen material.

[0088] In this embodiment, the material of the negative electrode substrate is limited to silicon-oxygen material, which ensures the normal progress of the electrodeposition process.

[0089] Based on the same inventive concept, an embodiment of the present invention provides a method for preparing a battery connector, wherein the material of the negative electrode substrate is a silicon-oxygen material.

[0090] In this embodiment, the material of the negative electrode substrate is limited to silicon-oxygen material, which ensures the normal progress of the electrodeposition process.

[0091] Based on the same inventive concept, an embodiment of the present invention provides a method for preparing a battery connector, wherein the material of the negative electrode substrate is a metallic lithium material.

[0092] In this embodiment, the material of the negative electrode substrate is limited to metallic lithium material, which ensures the normal progress of the electrodeposition process.

[0093] Based on the same inventive concept, the embodiment of the present invention provides a method for preparing a battery connector, wherein the current density of the electrodeposition device is 0.1A / dm 2 Up to 1A / dm 2 between.

[0094] In this embodiment, the current density of the electrodeposition device is limited to 0.1A / dm 2 Up to 1A / dm 2 The normal progress of the electrodeposition process is guaranteed, thereby ensuring the yield rate of the battery connector.

[0095] Based on the same inventive concept, an embodiment of the present invention provides a method for preparing a battery connector, wherein the operating temperature of the electrodeposition device is between 700 degrees Celsius and 950 degrees Celsius.

[0096] In this embodiment, the operating temperature of the electrodeposition device is limited to a value between 700 degrees Celsius and 950 degrees Celsius, thereby ensuring the normal progress of the electrodeposition process and further ensuring the yield rate of the battery connector.

[0097] Based on the same inventive concept, an embodiment of the present invention provides a method for preparing a battery connector, wherein the precipitation time of the electrodeposition device is between 5 minutes and 50 minutes.

[0098] In this embodiment, the deposition time of the electrodeposition device is limited to a value between 5 minutes and 50 minutes, thereby ensuring the normal progress of the electrodeposition process and further ensuring the yield rate of the battery connector.

[0099] Based on the same inventive concept, an embodiment of the present invention provides a method for preparing a battery connector, wherein the mass ratio of cobalt nitrate powder, nickel nitrate powder and magnesium nitrate powder is 1:1:(3-5).

[0100] In this embodiment, the mass ratio of cobalt nitrate powder, nickel nitrate powder and magnesium nitrate powder is defined as 1:1:(3-5), and the mass ratio of 1:1:(3-5) means that the mass fraction of cobalt nitrate powder is 1 part, the mass fraction of nickel nitrate powder is 1 part, and the mass fraction of magnesium nitrate powder is 3-5 parts.

[0101] In some embodiments, cobalt nitrate powder, nickel nitrate powder and magnesium nitrate powder are mixed in a mass ratio of 1:1:3 to obtain a powder mixture.

[0102] In some embodiments, cobalt nitrate powder, nickel nitrate powder and magnesium nitrate powder are mixed in a mass ratio of 1:1:5 to obtain a powder mixture.

[0103] In some embodiments, cobalt nitrate powder, nickel nitrate powder and magnesium nitrate powder are mixed in a mass ratio of 1:1:4 to obtain a powder mixture. The preparation method of the battery connector in this embodiment ensures the accuracy of the composition of the powder mixture by limiting the mass ratio of cobalt nitrate powder, nickel nitrate powder and magnesium nitrate powder, thereby ensuring the accuracy of the composition of the second electrolyte.

[0104] Based on the same inventive concept, an embodiment of the present invention provides a method for preparing a battery connector, wherein the mass ratio of sodium fluoride, potassium fluoride and lithium chloride is (1-3): (1-3): (1-8).

[0105] In this embodiment, the mass ratio of sodium fluoride, potassium fluoride and lithium chloride is defined as (1-3):(1-3):(1-8). The mass ratio of (1-3):(1-3):(1-8) means that the mass fraction of sodium fluoride is 1 to 3 parts, the mass fraction of potassium fluoride is 1 to 3 parts, and the mass fraction of lithium chloride is 1 to 8 parts.

[0106] In some embodiments, sodium fluoride, potassium fluoride and lithium chloride are added to an organic solution in a mass ratio of 1:1:1 and mixed to obtain a first electrolyte.

[0107] In some embodiments, sodium fluoride, potassium fluoride and lithium chloride are added to an organic solution in a mass ratio of 3:3:8 and mixed to obtain a first electrolyte.

[0108] In some embodiments, sodium fluoride, potassium fluoride and lithium chloride are added to an organic solution in a mass ratio of 1:3:8 and mixed to obtain a first electrolyte.

[0109] The preparation method of the battery connector in this embodiment ensures the accuracy of the composition of the first electrolyte by limiting the mass ratio of sodium fluoride, potassium fluoride and lithium chloride, thereby ensuring the accuracy of the composition of the second electrolyte.

[0110] Based on the same inventive concept, an embodiment of the present invention provides a method for preparing a battery connector, wherein the mass ratio of the powder mixture to the first electrolyte is (1-3):100.

[0111] In this embodiment, the mass ratio of the powder mixture to the first electrolyte is defined as (1-3):100, and the mass ratio of (1-3):100 means: the mass fraction of the powder mixture is 1-3 parts, the mass fraction of the first electrolyte is 1-3 parts, and the mass fraction of lithium chloride is 100 parts.

[0112] In some embodiments, the powder mixture is mixed with the first electrolyte at a mass ratio of 1:100 to obtain a second electrolyte.

[0113] In some embodiments, the powder mixture is mixed with the first electrolyte at a mass ratio of 3:100 to obtain a second electrolyte.

[0114] In some embodiments, the powder mixture is mixed with the first electrolyte at a mass ratio of 1.5:100 to obtain a second electrolyte.

[0115] The preparation method of the battery connector in this embodiment ensures the accuracy of the composition of the second electrolyte by limiting the mass ratio of the powder mixture to the first electrolyte.

[0116] Based on the same inventive concept, an embodiment of the present invention further provides a battery connector, which is manufactured by the manufacturing method of the battery connector in any possible implementation manner described above.

[0117] Based on the same inventive concept, an embodiment of the present invention further provides a battery, the battery comprising a battery connector in any possible implementation manner described above.

[0118] Based on the same inventive concept, an embodiment of the present invention further provides a battery, which is a solid oxide electrolytic cell.

[0119] Based on the same inventive concept, an embodiment of the present invention further provides a battery, which is a solid oxide fuel cell.

[0120] Example 1

[0121] A novel method for preparing a protective coating for a flat-tube SOFC metal connector comprises:

[0122] Step S1: Powder A: Co(NO3)2: Ni(NO3)2: Mn(NO3)3 = 1:1:3;

[0123] The component of the electrodeposition electrolyte B is NaF: KF: LiCl = 1:1:1;

[0124] Step S2: Powder A: electrolyte B = 1~3 (mass ratio) are mixed and placed in a container. The sample is placed in the container and connected to the anode of the power supply. The other end of the power supply is connected to the graphite plate and placed in the container. The electrodeposition process settings are: current density 0.1A / dm2, temperature setting 700℃, and deposition time 5min.

[0125] The solid oxide battery stack metal connector coating determination method was used to test the metal connector protective coating thickness of 10.1 microns and its composition was Co 0.5 Ni 0.5 Mn2O4.

[0126] Example 2

[0127] A novel method for preparing a protective coating for a flat-tube SOFC metal connector comprises:

[0128] Step S1: Powder A: Co(NO3)2: Ni(NO3)2: Mn(NO3)3 = 1:1:5;

[0129] The component of the electrodeposition electrolyte B is NaF: KF: LiCl = 3: 3: 8;

[0130] Step S2: Powder A: electrolyte B = 1-100 (mass ratio) mixed and placed in a container. The sample is placed in the container and connected to the anode of the power supply. The other end of the power supply is connected to the graphite plate and placed in the container. Electrodeposition process settings: current density 1A / dm 2 , the temperature was set at 950°C and the deposition time was 50 min.

[0131] The solid oxide battery stack metal connector coating determination method was used to test the metal connector protective coating thickness of 11.5 microns and its composition was Co 0.4 Ni 0.4 Mn 2.2 O4.

[0132] Example 3

[0133] A novel method for preparing a protective coating for a flat-tube SOFC metal connector comprises:

[0134] Step S1: Powder A: Co(NO3)2: Ni(NO3)2: Mn(NO3)3 = 1:1:4;

[0135] The component of the electrodeposition electrolyte B is NaF: KF: LiCl = 2: 2: 5;

[0136] Step S2: Powder A: electrolyte B = 1~50 (mass ratio) is mixed and placed in a container. The sample is placed in the container and connected to the anode of the power supply. The other end of the power supply is connected to the graphite plate and placed in the container. The electrodeposition process settings are: current density 0.5A / dm2, temperature setting 800℃, and deposition time 30min.

[0137] The solid oxide battery stack metal connector coating determination method was used to test the metal connector protective coating thickness of 9.6 microns and its composition was Co 0.5 Ni 0.5 Mn2O4.

[0138] Example 4

[0139] A novel method for preparing a protective coating for a flat-tube SOFC metal connector comprises:

[0140] Step S1: Powder A: Co(NO3)2: Ni(NO3)2: Mn(NO3)3 = 1:1:5;

[0141] The component of the electrodeposition electrolyte B is NaF: KF: LiCl = 2: 2: 7;

[0142] Step S2: Powder A: electrolyte B = 1~35 (mass ratio) is mixed and placed in a container. The sample is placed in the container and connected to the anode of the power supply. The other end of the power supply is connected to the graphite plate and placed in the container. The electrodeposition process settings are: current density 1A / dm2, temperature setting 800℃, and deposition time 35min.

[0143] The solid oxide battery stack metal connector coating determination method was used to test the metal connector protective coating thickness of 11.5 microns and its composition was Co 0.4 Ni 0.4 Mn 2.2 O4.

[0144] Although this specification includes many specific implementation details, these should not be interpreted as limiting the scope of any invention or the scope of protection claimed, but are mainly used to describe the features of the specific embodiments of specific inventions. Certain features described in multiple embodiments in this specification may also be implemented in combination in a single embodiment. On the other hand, the various features described in a single embodiment may also be implemented separately in multiple embodiments or in any suitable sub-combination. In addition, although the features may work as above in certain combinations and even initially claim protection, one or more features from the claimed combination may be removed from the combination in some cases, and the claimed combination may point to a sub-combination or a variation of a sub-combination.

[0145] Similarly, although operations are depicted in a particular order in the accompanying drawings, this should not be understood as requiring that these operations be performed in the particular order shown or performed sequentially, or requiring that all illustrated operations be performed to achieve the desired results. In some cases, multitasking and parallel processing may be advantageous. In addition, the separation of various system modules and components in the above-described embodiments should not be understood as requiring such separation in all embodiments, and it should be understood that the described program components and systems can generally be integrated together in a single software product, or packaged into multiple software products.

[0146] Thus, specific embodiments of the subject matter have been described. Other embodiments are within the scope of the appended claims. In some cases, the actions recited in the claims can be performed in a different order and still achieve the desired results. In addition, the processes depicted in the drawings do not necessarily require the particular order or sequential order shown to achieve the desired results. In some implementations, multitasking and parallel processing may be advantageous.

[0147] It should be noted that, in this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.

[0148] The above is only a specific embodiment of the present invention, so that those skilled in the art can understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but should conform to the widest scope consistent with the principles and novel features applied herein.

Claims

1. A method for preparing a battery connector, characterized in that: The preparation method of the battery connector comprises: preparing a powder mixture, wherein the powder mixture is a mixture containing cobalt nitrate powder, nickel nitrate powder and manganese nitrate powder, wherein the mass ratio of the cobalt nitrate powder, the nickel nitrate powder and the manganese nitrate powder is 1:1:(3-5); preparing a first electrolyte, wherein the first electrolyte is an electrolyte containing sodium fluoride, potassium fluoride and lithium chloride, wherein the mass ratio of the sodium fluoride, the potassium fluoride and the lithium chloride is (1-3):(1-3):(1-8); Mixing the powder mixture with the first electrolyte to obtain a second electrolyte, wherein the mass ratio of the powder mixture to the first electrolyte is (1-3):100; placing the interconnect substrate in the second electrolyte to perform an electrodeposition process, forming a protective layer on the surface of the interconnect substrate to obtain the battery interconnect, The connecting body substrate is connected to the electrodeposition device; the negative electrode substrate is connected to the electrodeposition device, the connecting body substrate is connected to the anode of the power supply of the electrodeposition device, and the negative electrode substrate is connected to the cathode of the power supply of the electrodeposition device; The connector substrate and the negative electrode substrate are placed in the second electrolyte, and the second electrolyte is subjected to an electrodeposition process by an electrodeposition device to form the protective layer on the surface of the connector substrate to obtain the battery connector; wherein the current density of the electrodeposition process is 0.1A / dm 2 Up to 1A / dm 2 The temperature of the electrodeposition process is between 700 degrees Celsius and 950 degrees Celsius, and the deposition time of the electrodeposition device is between 5 minutes and 50 minutes.

2. The method for preparing a battery connector according to claim 1, characterized in that: The preparation of the powder mixture specifically comprises: The cobalt nitrate powder, the nickel nitrate powder and the manganese nitrate powder are mixed to obtain the powder mixture.

3. The method for preparing a battery connector according to claim 1, characterized in that: The preparation of the first electrolyte specifically comprises: The sodium fluoride, the potassium fluoride, and the lithium chloride are mixed in a solution to obtain the first electrolyte.

4. The method for preparing a battery connector according to claim 1, characterized in that: The material of the negative electrode substrate is graphite material.

5. The method for preparing a battery connector according to claim 1, characterized in that: The material of the negative electrode substrate is silicon-carbon material.

6. The method for preparing a battery connector according to claim 1, characterized in that: The material of the negative electrode substrate is silicon oxide material.

7. The method for preparing a battery connector according to claim 1, characterized in that: The material of the negative electrode substrate is metallic lithium material.

8. A battery connector, characterized in that: The battery connector is manufactured by the method for manufacturing the battery connector according to any one of claims 1 to 7.

9. A battery, characterized in that: The battery comprises the battery connector according to claim 8.

10. The battery according to claim 9, characterized in that The cell is of the solid oxide electrolysis cell type.

11. The battery according to claim 10, characterized in that The cell type is a solid oxide fuel cell.