Organic small molecule near-infrared absorber and its application in UV curable film
By designing the nitrogen pyrrolithiophene structure and the organic small molecule near-infrared absorber that introduces side chain groups, the problems of narrow absorption range and poor solubility in the prior art are solved, and a wider near-infrared absorption coverage and good solubility are achieved. In near-infrared barrier applications.
Patent Information
- Application Number
- CN202310885627.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-17
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-07-17
AI Technical Summary
In the prior art, the absorption range of the near-infrared absorber is relatively narrow and has poor solubility, making it difficult to disperse in a non-solution system, and cannot effectively cover a wider near-infrared band.
Using nitrogen pyrrolethiophene structure as the nucleus, through the structural design of electron-pull-π bridge-electron-drawn electrons, combined with the non-covalent bonding in the molecule, the spectral absorption range is expanded, and different groups are introduced in the side chains. , improve the solubility of molecules, and prepare an organic small molecule near-infrared absorber with a wide near-infrared absorption coverage range.
The absorption range of near-infrared absorber has been expanded to above 1200nm and maintained good solubility in a solvent-free system. It is suitable for near-infrared barrier tape and film, and is suitable for glass, wall curtains and other scenarios where infrared radiation is required.
Smart Images

Figure CN116891482B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of new material preparation, and specifically relates to an organic small molecule near-infrared absorber used in a near-infrared blocking tape or film, a preparation method and application thereof in a UV curing coating and a curing film. Background Art
[0002] Near infrared light (NIR) is an electromagnetic wave between visible light and mid-infrared light. According to the definition of ASTM (American Society for Testing and Materials), it refers to electromagnetic waves with a wavelength range of 780 to 2526 nm. It is customary to divide the near infrared region into two regions: near infrared short wave (780 to 1100 nm) and near infrared long wave (1100 to 2526 nm).
[0003] In the existing reports on infrared absorption, the commonly used infrared absorbers are mostly non-metallic oxides, metal ions, metal oxides, phthalocyanines, organic small molecules, etc. Known application number, 201710571460.3, reported a transparent heat-insulating film, the infrared absorber used is metal oxide, and its infrared coverage range can reach 2500nm, but the light transmittance effect is poor, and the metal inorganic absorber is difficult to disperse in the non-solution system. Known application number, 201910477227.8, reported a near-infrared absorption film, which uses metal-organic complex near-infrared absorbers. The absorber can withstand high temperatures, but its effective absorption area only covers up to 900nm, and the band is relatively short. Known application number, 202210603284.8, reported an organic small molecule near-infrared absorber, which has good stability, but its near-infrared absorption range only covers up to 900nm.
[0004] Combining the above information, we see that it is imperative to develop a near-infrared absorber with a wide coverage range and good solubility. Summary of the invention
[0005] In order to solve the above problems existing in the prior art, the present invention aims to provide a near-infrared absorber, a preparation method and its application in UV curing coatings and curing films, which has a wide near-infrared absorption coverage range and good solubility properties.
[0006] The technical solution adopted by the present invention is:
[0007] An organic small molecule near-infrared absorber, the structural formula of which is:
[0008]
[0009] Where R1 is C8-C 16 The alkyl chain of R2 is C 10 -C18 An alkyl chain, R1 and R2 are the same or different.
[0010] Furthermore, the R1=C 12 ,R2=C 16 .
[0011] Further, its structural formula is:
[0012]
[0013] Furthermore, the present invention also relates to a method for preparing the above-mentioned organic small molecule near-infrared absorber, comprising the following steps:
[0014] Taking the nitrogen pyrrolothiophene structure as the core, the electron-withdrawing-π bridge-electron-donating-π bridge-electron-withdrawing structure is adopted. Through the action of non-covalent bonds within the molecule, the spectral absorption range is moved to the near-infrared light region; different side chain groups are introduced into the side chain, and an organic small molecule near-infrared absorber is constructed through molecular engineering.
[0015] Further, the general formula of the synthetic route is:
[0016]
[0017] Furthermore, the present invention also relates to a UV curable film, which uses the above-mentioned organic small molecule near-infrared absorber and comprises the following components in parts by weight:
[0018] 40-50 parts of polyurethane resin, 10-25 parts of acrylic acid diluent monomer, 0.3-1 parts of photoinitiator, and 10-25 parts of organic small molecule near-infrared absorber.
[0019] Furthermore, the molecular weight of the polyurethane resin is 8000-15000.
[0020] Furthermore, the acrylic acid diluent monomer includes one or more of acrylic acid, isobornyl acrylate, hydroxyethyl acrylate, hydroxypropyl acrylate, N-vinyl pyrrolidone, acryloylmorpholine, tetrahydrofuran acrylate, glycidyl methacrylate, 1,6-hexanediol diacrylate, neopentyl glycol diacrylate, and trimethylolpropane triacrylate.
[0021] Furthermore, the photoinitiator includes one or more of 2-hydroxy-2-methyl-1-phenyl-1-propanone, 1-hydroxycyclohexyl phenyl ketone, diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide, and ethyl 2,4,6-trimethylbenzoylphenylphosphonate.
[0022] Finally, the present invention also relates to a method for preparing a UV curable film, which is used to prepare the above-mentioned UV curable film, comprising the following steps:
[0023] First, a solvent-free near-infrared UV curing hardening liquid is prepared: an organic small molecule near-infrared absorber and an acrylic acid diluent monomer are evenly mixed, and then a polyurethane resin and a photoinitiator are added, and the mixture is stirred for 1 to 2 hours;
[0024] Secondly, a solvent-free near-infrared UV curing liquid is applied to the substrate and cured by a UV curing lamp to form a UV coating.
[0025] The beneficial effects of the present invention are:
[0026] An organic small molecule near-infrared absorber, a preparation method and its application in UV hardening coatings and hardening films, with a nitrogen pyrrolothiophene structure as the core, adopting the structural concept of electron-pulling-π bridge-electron-donating-π bridge-electron-pulling, increasing the planarity through the action of intramolecular non-covalent bonds, making the molecular absorption range further red-shifted and covering more near-infrared regions; different side chain groups can be introduced into the side chain, and through molecular engineering, the molecule has good solubility and can be suitable for dissolution in various solvent-containing or solvent-free systems. It can be used to prepare near-infrared absorbing coatings, applied in the field of near-infrared blocking tapes or films, and can also be applied to glass, wall curtains and other scenes where infrared radiation needs to be blocked. It has a wide near-infrared absorption coverage range and good solubility. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 is a spectrum absorption curve diagram of the organic small molecule INO-4F according to Example 1 of the present invention;
[0028] Figure 2 This is the structural hydrogen spectrum of the organic small molecule INO-4F according to Example 1 of the present invention. DETAILED DESCRIPTION
[0029] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. All other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] In order to provide a near-infrared absorber, a preparation method and its application in UV curing coating and curing film, the overall planning scheme of the present invention is: to conceive an organic small molecule near-infrared absorber, whose structural formula is:
[0031]
[0032] Where R1 is C8-C 16 The alkyl chain of R2 is C 10 -C 18An alkyl chain, R1 and R2 are the same or different.
[0033] Furthermore, in a preferred embodiment, the specific value is: R1 = C 12 ,,R2=C 16 , whose structural formula is:
[0034]
[0035] Furthermore, the present invention also relates to a method for preparing the above-mentioned organic small molecule near-infrared absorber, comprising the following steps:
[0036] With the nitrogen pyrrolothiophene structure as the core, the electron-withdrawing-π bridge-electron-donating-π bridge-electron-withdrawing structure is adopted. Through the action of intramolecular non-covalent bonds, the organic near-infrared molecule forms a good planar structure and the spectral absorption range is moved to the near-infrared light region. Different side chain groups are introduced into the side chain, and organic small molecule near-infrared absorbers are constructed through molecular engineering.
[0037] The specific molecular structure formula of the intramolecular non-covalent bonds is as follows:
[0038]
[0039] It can make the molecular planarity better.
[0040] The specific synthesis route is as follows:
[0041]
[0042] Furthermore, the present invention also relates to a UV curable film, which uses the above-mentioned organic small molecule near-infrared absorber and comprises the following components in parts by weight:
[0043] 40-50 parts of polyurethane resin, 10-25 parts of acrylic acid diluent monomer, 0.3-1 parts of photoinitiator, and 10-25 parts of organic small molecule near-infrared absorber.
[0044] The molecular weight of the polyurethane resin is 8000-15000.
[0045] The acrylic acid diluent monomer includes one or more of acrylic acid, isobornyl acrylate, hydroxyethyl acrylate, hydroxypropyl acrylate, N-vinyl pyrrolidone, acryloylmorpholine, tetrahydrofuran acrylate, glycidyl methacrylate, 1,6-hexanediol diacrylate, neopentyl glycol diacrylate, and trimethylolpropane triacrylate.
[0046] The photoinitiator comprises one or more of 2-hydroxy-2-methyl-1-phenyl-1-propanone, 1-hydroxycyclohexyl phenyl ketone, diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide, and ethyl 2,4,6-trimethylbenzoylphenylphosphonate.
[0047] Furthermore, the present invention also relates to a method for preparing a UV curable film, which is used to prepare the above-mentioned UV curable film, comprising the following steps:
[0048] First, a solvent-free near-infrared UV curing liquid is prepared by uniformly mixing an organic small molecule near-infrared absorber and an acrylic acid diluent monomer, then adding a polyurethane resin and a photoinitiator, and mixing and stirring for several hours to obtain a UV curing liquid.
[0049] The mixing and stirring time lasts for 1 to 2 hours. During the specific operation, the time can be adaptively selected according to the actual situation. Usually, the mixing and stirring time is about 1 hour.
[0050] Secondly, as a preferred application method, a solvent-free near-infrared UV curing hardening liquid is coated on the substrate and cured by UV curing lamp to form a UV coating.
[0051] The UV curable film can be applied to the field of near-infrared blocking tapes or films, and can be used in glass, wall curtains and other scenes where infrared radiation needs to be blocked.
[0052] Again, verify the near-infrared absorption coverage:
[0053] In the structure of organic small molecule near-infrared absorber, R1=C 12 、R2=C 16 According to the synthesis path, the structural formula is:
[0054] The organic small molecule INO-4F product has a yield of 76%.
[0055] Then, H NMR spectroscopy ( 1 H-NMR) was used to identify the structure of INO-4F product, and the results are as follows:
[0056] 1H NMR(400MHz,Chloroform-d)δ8.54(s,2H),8.39(dd,J=9.9,6.5Hz,2H),7.61 (t,J=7.5Hz,2H),7.36(s,2H),7.24(s,2H),4.20-4.07(m,4H),3.97(d,J=7.8 Hz,2H),1.99(dt,J=11.7,5.8Hz,3H),1.66(td,J=14.6,7..2Hz,4H),1.52-1 .11(m,52H),0.99(t,J=7.0Hz,6H),0.94-0.87(m,6H),0.81(q,J=6.8Hz,6H).
[0057] The scheme and effect of the present invention are verified and confirmed by comparing Examples 1 to 3 with Comparative Examples 1 to 3.
[0058] Embodiment 1:
[0059] Prepare the raw materials according to the following components and weight proportions:
[0060] 50 parts of polyurethane resin;
[0061] 25 parts of acrylic acid diluent monomer;
[0062] 1 part of photoinitiator;
[0063] Near infrared absorber INO-4F: 25 parts;
[0064] First, weigh the acrylic acid dilution monomer and INO-4F and mix them evenly, then mix them with the polyurethane resin and the photoinitiator, stir at room temperature for 1 hour, and the measured viscosity is about 6300mPa·s to obtain a near-infrared absorbing coating liquid. Among them, the acrylic acid dilution monomer includes 3 parts of acrylic acid, 10 parts of isobornyl acrylate, 3 parts of hydroxyethyl acrylate, 4 parts of N-vinyl pyrrolidone, and 5 parts of 1,6-hexanediol diacrylate; the photoinitiator is 0.5 parts of 2-hydroxy-2-methyl-1-phenyl-1-propanone and 0.5 parts of diphenyl-(2,4,6-trimethylbenzoyl) phosphine oxide. The above-mentioned near-infrared absorbing coating liquid is coated / coated on a PET substrate, and after curing by UV lamp irradiation for 20s, a near-infrared absorbing coating is obtained. The thickness of the PET substrate is 25μm, and the thickness of the coating is 25μm. Performance test: tested by UV-visible spectrophotometer, its near-infrared coverage range can cover above 1200nm, no absorption blue shift is observed, and the transmittance measured according to national standard GB / T 2410-2008 is 90.6% and the haze is 0.8%.
[0065] Example 2
[0066] Prepare the raw materials according to the following components and weight proportions:
[0067] 40 parts of polyurethane resin;
[0068] 10 parts of acrylic acid diluent monomer;
[0069] 0.3 parts of photoinitiator;
[0070] Near infrared absorber INO-4F: 10 parts;
[0071] First, weigh the acrylic acid dilution monomer and INO-4F and mix them evenly, then mix them with the polyurethane resin and the photoinitiator, stir at room temperature for 1 hour, and the measured viscosity is about 10500mPa·s to obtain a near-infrared absorbing coating liquid. Among them, the acrylic acid dilution monomer includes 1 part of acrylic acid, 3 parts of isobornyl acrylate, 3 parts of acryloyl morpholine, and 3 parts of 1,6-hexanediol diacrylate; the photoinitiator is 0.15 parts of 2-hydroxy-2-methyl-1-phenyl-1-propanone and 0.15 parts of diphenyl-(2,4,6-trimethylbenzoyl) phosphine oxide. The above-mentioned near-infrared absorbing coating liquid is coated / coated on a PET substrate, and after curing by UV lamp irradiation for 40s, a near-infrared absorbing coating is obtained. The thickness of the PET substrate is 25μm, and the thickness of the coating is 25μm. Performance test: tested by UV-visible spectrophotometer, its near-infrared coverage range can cover above 1100nm. According to the national standard GB / T 2410-2008, the transmittance is 92.8% and the haze is 0.7%.
[0072] Example 3
[0073] Prepare the raw materials according to the following components and weight proportions:
[0074] 45 parts of polyurethane resin;
[0075] 20 parts of acrylic acid diluent monomer;
[0076] 0.3 parts of photoinitiator;
[0077] Near infrared absorber INO-4F: 17 parts;
[0078] First, weigh the acrylic acid dilution monomer and INO-4F and mix them evenly, then mix them with the polyurethane resin and the photoinitiator, stir at room temperature for 1 hour, and the measured viscosity is about 7100mPa·s to obtain a near-infrared absorbing coating liquid. Among them, the acrylic acid dilution monomer includes 3 parts of acrylic acid, 5 parts of isobornyl acrylate, 5 parts of acryloyl morpholine, 4 parts of N-vinyl pyrrolidone, and 3 parts of trimethylolpropane triacrylate; the photoinitiator is 0.15 parts of 2-hydroxy-2-methyl-1-phenyl-1-propanone and 0.15 parts of diphenyl-(2,4,6-trimethylbenzoyl) phosphine oxide. The above-mentioned near-infrared absorbing coating liquid is coated / coated on a PET substrate, and after curing by UV lamp irradiation for 20s, a near-infrared absorbing coating is obtained. The thickness of the PET substrate is 25μm, and the thickness of the coating is 25μm. Performance test: tested by UV-visible spectrophotometer, its near-infrared coverage range can cover above 1200nm, no absorption blue shift is observed, and the transmittance measured according to national standard GB / T 2410-2008 is 92.1% and the haze is 0.6%.
[0079] Comparative Example 1:
[0080] Prepare the raw materials according to the following components and weight proportions:
[0081] 50 parts of polyurethane resin;
[0082] 25 parts of acrylic acid diluent monomer;
[0083] 1 part of photoinitiator;
[0084] Weigh polyurethane resin, acrylic acid diluent monomer, and photoinitiator, mix, stir at room temperature for 1 hour, and the measured viscosity is about 6100mPa·s to obtain a coating liquid. Among them, the acrylic acid diluent monomer includes 3 parts of acrylic acid, 10 parts of isobornyl acrylate, 3 parts of hydroxyethyl acrylate, 4 parts of N-vinyl pyrrolidone, and 5 parts of 1,6-hexanediol diacrylate; the photoinitiator is 0.5 parts of 2-hydroxy-2-methyl-1-phenyl-1-propanone and 0.5 parts of diphenyl-(2,4,6-trimethylbenzoyl) phosphine oxide. The above coating liquid is coated / coated on a PET substrate, and cured by UV lamp irradiation for 20s to obtain a coating. The thickness of the PET substrate is 25μm, and the thickness of the coating is 25μm. Performance test: It has no near-infrared absorption as tested by a UV-visible spectrophotometer. According to the national standard GB / T 2410-2008, the transmittance is 92.7% and the haze is 0.7%.
[0085] Comparative Example 2:
[0086] Prepare the raw materials according to the following components and weight proportions:
[0087] 40 parts of polyurethane resin;
[0088] 10 parts of acrylic acid diluent monomer;
[0089] 0.3 parts of photoinitiator;
[0090] Near infrared absorber IRG-022: 10 parts;
[0091] Near-infrared absorber IRG-022 is an organic salt near-infrared absorber. First, weigh the acrylic acid dilution monomer and the commercial near-infrared absorber IRG-022 separately and mix them. It is found that it is difficult to dissolve. Then mix them with polyurethane resin and photoinitiator, stir at room temperature for 1 hour, and the measured viscosity is about 10100mPa·s to obtain a near-infrared absorbing coating liquid. Among them, the acrylic acid dilution monomer includes 1 part of acrylic acid, 3 parts of isobornyl acrylate, 3 parts of acryloyl morpholine, and 3 parts of 1,6-hexanediol diacrylate; the photoinitiator is 0.15 parts of 2-hydroxy-2-methyl-1-phenyl-1-propanone and 0.15 parts of diphenyl-(2,4,6-trimethylbenzoyl) phosphine oxide. The above-mentioned near-infrared absorbing coating liquid is coated / coated on a PET substrate, and after curing by UV lamp irradiation for 60s, a near-infrared absorbing coating is obtained. The thickness of the PET substrate is 25μm, and the thickness of the coating is 25μm. Performance test: tested by UV-visible spectrophotometer, its near-infrared coverage range covers about 930nm. According to the national standard GB / T 2410-2008, the transmittance is 78.1% and the haze is 3.6%.
[0092] Comparative Example 3:
[0093] Prepare the raw materials according to the following components and weight proportions:
[0094] 50 parts of polyurethane resin;
[0095] 25 parts of acrylic acid diluent monomer;
[0096] 1 part of photoinitiator;
[0097] Near infrared absorber nano zinc oxide: 10 parts;
[0098] Nano zinc oxide is an inorganic near-infrared absorber. First, weigh the acrylic acid dilution monomer and commercially available zinc oxide separately, mix them, and disperse them at high speed for 2 hours. It is still found that dispersion is difficult and agglomeration occurs. Then mix them with polyurethane resin and photoinitiator, stir them at room temperature for 1 hour, and the measured viscosity is about 6800mPa·s to obtain a near-infrared absorbing coating liquid. Among them, the acrylic acid dilution monomer includes 3 parts of acrylic acid, 10 parts of isobornyl acrylate, 3 parts of hydroxyethyl acrylate, 4 parts of N-vinyl pyrrolidone, and 5 parts of 1,6-hexanediol diacrylate; the photoinitiator is 0.5 parts of 2-hydroxy-2-methyl-1-phenyl-1-propanone and 0.5 parts of diphenyl-(2,4,6-trimethylbenzoyl) phosphine oxide. The above-mentioned near-infrared absorbing coating liquid is coated / coated on a PET substrate, and after curing by UV lamp for 60s, a near-infrared absorbing coating is obtained. The thickness of the PET substrate is 25μm, and the thickness of the coating is 25μm. Performance test: Through the UV-Vis spectrophotometer test, it was found that it did not show good near-infrared absorption due to poor dispersion. According to the national standard GB / T 2410-2008, the transmittance was 77.5% and the haze was 5.8%.
[0099] The organic small molecule near-infrared absorber, preparation method and application in UV hardening coating and hardening film of the present invention take nitrogen pyrrolothiophene structure as core, adopt the structural concept of electron-pulling-π bridge-electron-donating-π bridge-electron-pulling, increase planarity through the action of intramolecular non-covalent bonds, make organic near-infrared molecules form a good planar structure, further red-shift the molecular absorption range, and cover more near-infrared regions; different side chain groups can be introduced into the side chain, and through molecular engineering, the molecule has good solubility, and can be suitable for dissolution in various solvent or solvent-free systems. It can be used to prepare near-infrared absorbing coatings, applied in the field of near-infrared blocking tapes or films, and can also be applied to glass, wall curtains and other scenes where infrared radiation needs to be blocked. It has a wide near-infrared absorption coverage and good solubility.
[0100] The present invention is not limited to the above-mentioned optional implementation modes. Anyone can derive other various forms of products under the inspiration of the present invention. However, no matter what changes are made in the shape or structure, all technical solutions that fall within the scope defined by the claims of the present invention fall within the protection scope of the present invention.
Claims
1. An organic small molecule near-infrared absorber, Features: Its structural formula is: R 1 C 12 Alkyl chain, R 2 C 16 Alkyl chain.
2. The near infrared absorber according to claim 1, Features: Its structural formula is: 。 3. A method for preparing the organic small molecule near-infrared absorber according to claim 1, Features: The following steps are involved: 。 4. A UV curing film, Features: The organic small molecule near-infrared absorber according to claim 1 comprises the following components in parts by weight: 40-50 parts of polyurethane resin, 10-25 parts of acrylic acid diluent monomer, 0.3-1 parts of photoinitiator, and 10-25 parts of organic small molecule near-infrared absorber.
5. According to the UV curing film of claim 4, Features: The molecular weight of the polyurethane resin is 8000-15000.
6. According to the UV curing film of claim 4, Features: The acrylic acid diluent monomer includes one or more of acrylic acid, isobornyl acrylate, hydroxyethyl acrylate, hydroxypropyl acrylate, N-vinyl pyrrolidone, acryloylmorpholine, tetrahydrofuran acrylate, glycidyl methacrylate, 1,6-hexanediol diacrylate, neopentyl glycol diacrylate, and trimethylolpropane triacrylate.
7. According to the UV curing film of claim 4, Features: The photoinitiator includes one or more of 2-hydroxy-2-methyl-1-phenyl-1-propanone, 1-hydroxycyclohexyl phenyl ketone, diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide, and ethyl 2,4,6-trimethylbenzoylphenylphosphonate.
8. A method for preparing a UV curable film, for preparing the UV curable film according to any one of claims 4 to 7, Features: The steps include: First, a solvent-free near-infrared UV curing hardening liquid is prepared: an organic small molecule near-infrared absorber and an acrylic acid diluent monomer are evenly mixed, and then a polyurethane resin and a photoinitiator are added, and the mixture is stirred for 1 to 2 hours; Secondly, a solvent-free near-infrared UV curing liquid is applied to the substrate and cured by a UV curing lamp to form a UV coating.