A ceramic green body gel and preparation method thereof

Through a specific method of preparing ceramic blank gel, the porosity problem during firing of ceramic blanks is solved, the high strength and high yield of the ceramic blank are achieved, and its thermal stability and heat resistance are enhanced.

CN116969768BActive Publication Date: 2024-11-08HUNAN NEW CENTURY ELECTRIC PORCELAIN CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310962725.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-02
Publication Date
2024-11-08
Estimated Expiration
2043-08-02

AI Technical Summary

Technical Problem

Pores are easily generated when the ceramic blank gel is fired, resulting in a decrease in the strength of ceramic products, and traditional methods are difficult to effectively solve this problem.

Method used

A ceramic blank gel preparation method is adopted, by grinding powders such as lanthanum oxide powder, yttrium oxide powder, cerium oxide powder, zirconium dioxide powder, etc., and mixing them with deionized water and zirconium oxide milling balls, and then at specific temperatures and frequency Ultrasonic stirring is carried out to form a gel precursor and sintered in a vacuum sintering furnace. Finally, rare earth admixtures, potassium feldspar and other materials are added to adjust the pH value and solid content to form a ceramic blank gel.

Benefits of technology

This method can effectively avoid cracks and pore defects in the ceramic body during firing, improve the yield and strength of the ceramic body, and enhance its thermal stability and heat resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004372166690000072
    Figure BDA0004372166690000072
Patent Text Reader

Abstract

The invention discloses a ceramic blank gel and a preparation method thereof, belonging to the technical field of ceramic blanks. Rare earth powder, boric acid, melamine and deionized water are prepared into a gel precursor, sintered, crushed and sieved to obtain rare earth composite powder, the rare earth composite powder, isopropanol and deionized water are stirred and mixed and ultrasonically dispersed, ammonia water and tetraethyl orthosilicate are added to react to obtain a rare earth admixture, potassium feldspar, sodium feldspar, quartz, aluminum powder, magnesium powder, lithium fluoride powder and deionized water are added into a ball mill for ball milling and mixing, rare earth admixture, acrylamide monomer, crosslinking agent and ammonium citrate are added, solid content and pH value are adjusted after stirring and mixing, and a catalyst is added for crosslinking to obtain the ceramic blank gel; the rare earth admixture helps to improve the viscosity of the ceramic blank gel, prevents defects such as cracks from being generated, helps to improve the yield of the ceramic blank, and the fired ceramic has no microscopic defects such as pores and has high strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ceramic blanks, and in particular relates to a ceramic blank gel and a preparation method thereof. Background Art

[0002] Ceramics is a general term for pottery and porcelain, which is made by firing ceramic blanks. Traditional ceramic blanks are usually made by mixing natural clay, quartz, feldspar and other raw materials and preparing them through processes such as drying and molding. This blank has low strength and shape retention before sintering, and needs to be densified and strengthened through a high-temperature sintering process.

[0003] With the advancement of technology, ceramic technology is constantly improving, and the preparation method of green body is also being innovated. Ceramic green body gel is a ceramic green body that has undergone a hydrolysis reaction to form a gel system, generally composed of inorganic powder and organic substances (such as polyacrylic acid or polyvinyl ester, etc.). The formation of the gel system is to suspend the powder in water through the sol-gel method, and add certain additives and wetting agents to control the interaction between the powder particles, so that it forms a unique gel network structure.

[0004] Ceramic green body gel has high shape retention and processability, and can also provide a certain strength, and can be used to prepare various ceramic products. During the sintering process, the gel will undergo changes such as sublimation and sintering shrinkage, and finally form a dense ceramic green body. The formation and sintering process of the gel have an important influence on the performance and microstructure of the final ceramic product. However, the addition of gel material can easily cause microscopic defects such as pores in the fired ceramic, resulting in a decrease in its strength. Summary of the invention

[0005] One of the purposes of the present invention is to provide a ceramic green body gel to solve the problem that gas generated during firing of gel material easily leads to pores in ceramics; the second purpose is to provide a method for preparing the ceramic green body gel.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A method for preparing a ceramic green body gel comprises the following steps:

[0008] Step 1: Add lanthanum oxide powder, yttrium oxide powder, cerium oxide powder, zirconium dioxide powder and titanium dioxide powder into a ball mill, then add deionized water and zirconium oxide grinding balls with a diameter of 5 mm, ball mill and mix for 10-15 hours, filter the material, remove the zirconium oxide grinding balls, dry the remaining slurry, and crush it to obtain rare earth powder;

[0009] Step 2: Mix rare earth powder, boric acid, melamine and deionized water, stir at 90-95° C. for 20-30 minutes to dissolve boric acid and melamine in deionized water, and stably disperse the mixed powder in deionized water, then heat to 120-150° C., stir at a frequency of 40-50 kHz with ultrasonic assistance and a stirring speed of 800-1200 r / min for 2-4 hours, then stop stirring, and continue ultrasonic treatment at the same frequency for 2-3 hours to obtain a gel precursor;

[0010] Step 3: Transfer the gel precursor to a crucible, and then place it in a vacuum sintering furnace, keep it warm for 2-4 hours under nitrogen protection and 1850-1900°C, and after cooling, crush the sintered block and pass it through a 150-200 mesh sieve to obtain a rare earth composite powder;

[0011] Step 4: Add rare earth composite powder, isopropanol and deionized water into a stirring tank, stir and mix, then ultrasonically disperse for 30-60 minutes, add 20% ammonia water and ethyl orthosilicate by mass fraction, stir for 10-12 hours at 25-30°C, centrifuge, wash the precipitate with deionized water 3-5 times, and dry to obtain a rare earth admixture.

[0012] Step 5: Add potassium feldspar, sodium feldspar, quartz, aluminum powder, magnesium powder, lithium fluoride powder and deionized water into a ball mill and mix for 4-6 hours, then add rare earth admixture, acrylamide monomer, crosslinking agent and ammonium citrate and stir for 2-3 hours, wherein ammonium citrate is a dispersant, and the solid content is adjusted to 60±5%, and then the pH value is adjusted to 8.5-9 with ammonia water, and then the catalyst is added and the temperature is raised to 75±5°C and stirring is continued for 15-30 minutes to obtain a ceramic green body gel.

[0013] Furthermore, the dosage ratio of lanthanum oxide powder, yttrium oxide powder, cerium oxide powder, zirconium dioxide powder, titanium dioxide powder, deionized water and zirconium oxide grinding balls is 10-12g: 6-8g: 20-24g: 5-6g: 4-8g: 180-230mL: 40-45g.

[0014] Furthermore, the usage ratio of rare earth powder, boric acid, melamine and deionized water is 0.5-0.8 g: 1.5-1.6 g: 1 g: 80 mL.

[0015] Furthermore, the usage ratio of the rare earth composite powder, isopropanol, deionized water, ammonia water and tetraethyl orthosilicate is 15-20 g: 250-300 mL: 80-100 mL: 60-80 mL: 25-30 mL.

[0016] Furthermore, the usage ratio of potassium feldspar, sodium feldspar, quartz, aluminum powder, magnesium powder, lithium fluoride powder, rare earth admixture, acrylamide monomer, crosslinking agent, ammonium citrate and catalyst is 15-20g: 14-18g: 45-55g: 15-20g: 1-2g: 1-2g: 15-20g: 10-15g: 0.75-1g: 0.3-0.4g: 1-2g.

[0017] Furthermore, the acrylamide monomer is one or a mixture of dimethylacrylamide and methacrylamide in any ratio.

[0018] Furthermore, the cross-linking agent is N,N'-methylenebisacrylamide.

[0019] Furthermore, the catalyst is a mixture of ammonium persulfate and N,N,N',N'-tetramethylethylenediamine in a mass ratio of 3:2.

[0020] Beneficial effects of the present invention:

[0021] The ceramic green body gel of the present invention has no defects such as cracks after drying, which helps to improve the yield of the ceramic green body. The fired ceramic has no microscopic defects such as pores and has high strength.

[0022] Rare earth admixtures are added to the ceramic green body gel. The compounded rare earth powder helps to improve the thermal stability and sintering performance of the ceramic, plays a role in adjusting the grain size, and helps to improve the strength and quality of the ceramic. After the rare earth powder is mixed with boric acid and melamine, the boric acid and melamine generate melamine diboric acid gel, in which the system powder is evenly dispersed. After firing, melamine diboric acid forms boron nitride fibers. The rare earth powder is sintered and bonded to the overlap of the boron nitride fibers. After crushing, a branched rare earth admixture with a high surface area is formed, which helps to improve the viscosity of the ceramic green body gel, prevent defects such as cracks, and help to improve the heat resistance and strength of the fired ceramic. Potassium feldspar, sodium feldspar and quartz are the main materials of the ceramic green body gel, and aluminum powder and magnesium powder help to improve the strength, thermal stability and density of the fired ceramic. Lithium fluoride powder plays a fluxing role, which helps to improve the hardness and corrosion resistance of the fired ceramic. DETAILED DESCRIPTION

[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] Example 1

[0025] This embodiment provides a ceramic green body gel, comprising the following implementation steps:

[0026] Step 1: Add 20kg of lanthanum oxide powder, 12kg of yttrium oxide powder, 40kg of cerium oxide powder, 10kg of zirconium dioxide powder and 8kg of titanium dioxide powder into a ball mill, then add 360L of deionized water and 80kg of zirconium oxide grinding balls with a diameter of 5mm, ball mill and mix for 10 hours, filter the material, remove the zirconium oxide grinding balls, dry the remaining slurry, and crush it to obtain rare earth powder.

[0027] Step 2: 50 kg of rare earth powder, 150 kg of boric acid, 100 kg of melamine and 8000 L of deionized water are mixed, stirred at 90 ° C for 20 min to dissolve the boric acid and melamine in the deionized water, and the mixed powder is stably dispersed in the deionized water, then heated to 120 ° C, stirred for 2 h at a frequency of 40 kHz and a stirring speed of 800 r / min with ultrasonic assistance, then stopped stirring, and continued ultrasonic treatment at the same frequency for 2 h to obtain a gel precursor; the gel precursor is transferred to a crucible, and then placed in a vacuum sintering furnace, kept warm for 2 h under nitrogen protection and 1850 ° C, and after cooling, the sintered block is crushed and passed through a 150 mesh sieve to obtain a rare earth composite powder.

[0028] Step 3: Add 45 kg of rare earth composite powder, 750 L of isopropanol and 240 L of deionized water into a stirring tank, stir and mix, then ultrasonically disperse for 30 minutes, add 180 L of 20% ammonia water and 75 L of tetraethyl orthosilicate, stir at 25°C for 10 hours, centrifuge, wash the precipitate with deionized water three times, and dry to obtain a rare earth admixture.

[0029] Step 4: Add 15kg of potassium feldspar, 14kg of sodium feldspar, 45kg of quartz, 15kg of aluminum powder, 1kg of magnesium powder, 1kg of lithium fluoride powder and deionized water into a ball mill and mix for 4 hours, then add 15kg of rare earth admixture, 10kg of dimethylacrylamide, 0.75kg of N,N'-methylenebisacrylamide and 0.3kg of ammonium citrate and stir for 2 hours, wherein ammonium citrate is a dispersant, and the solid content is adjusted to 60±5%, and then the pH value is adjusted to 8.5 with ammonia water, and then 1kg of ammonium persulfate and N,N,N',N'-tetramethylethylenediamine mixed in a mass ratio of 3:2 are added as a catalyst, and the temperature is raised to 75±5°C and stirring is continued for 15 minutes to obtain a ceramic green body gel.

[0030] Example 2

[0031] This embodiment provides a ceramic green body gel, comprising the following implementation steps:

[0032] Step 1: Add 22kg of lanthanum oxide powder, 14kg of yttrium oxide powder, 44kg of cerium oxide powder, 11kg of zirconium dioxide powder and 12kg of titanium dioxide powder into a ball mill, then add 410L of deionized water and 85kg of zirconium oxide grinding balls with a diameter of 5mm, ball mill and mix for 12.5h, filter the material, remove the zirconium oxide grinding balls, dry the remaining slurry, and crush it to obtain rare earth powder.

[0033] Step 2: 65kg of rare earth powder, 155kg of boric acid, 100kg of melamine and 8000L of deionized water are mixed, stirred at 92°C for 25min to dissolve the boric acid and melamine in the deionized water, and the mixed powder is stably dispersed in the deionized water, then heated to 135°C, stirred for 3h at a frequency of 45kHz and a stirring speed of 1000r / min with ultrasonic assistance, then stopped stirring, and continued ultrasonic treatment at the same frequency for 2.5h to obtain a gel precursor; the gel precursor is transferred to a crucible, and then placed in a vacuum sintering furnace, kept warm for 3h under nitrogen protection and 1875°C, and after cooling, the sintered block is crushed and passed through a 180-mesh sieve to obtain a rare earth composite powder.

[0034] Step 3: Add 52.5 kg of rare earth composite powder, 825 L of isopropanol and 270 L of deionized water into a stirring tank and stir to mix, then ultrasonically disperse for 45 minutes, add 210 L of 20% ammonia water and 82.5 L of tetraethyl orthosilicate, stir at 27°C for 11 hours, centrifuge, wash the precipitate with deionized water 4 times, and dry to obtain a rare earth admixture.

[0035] Step 4: Add 17.5kg of potassium feldspar, 16kg of sodium feldspar, 50kg of quartz, 18kg of aluminum powder, 1.5kg of magnesium powder, 1.5kg of lithium fluoride powder and deionized water into a ball mill and mix for 5 hours, then add 18kg of rare earth admixture, 12.5kg of dimethylacrylamide and methacrylamide mixed in a mass ratio of 1:1, 0.8kg of N,N'-methylenebisacrylamide and 0.35kg of ammonium citrate and stir for 2.5 hours, wherein ammonium citrate is a dispersant, and the solid content is adjusted to 60±5%, and then the pH value is adjusted to 8.5 with ammonia water, and then 1.5kg of ammonium persulfate and N,N,N',N'-tetramethylethylenediamine mixed in a mass ratio of 3:2 are added as a catalyst, and the temperature is raised to 75±5°C and stirring is continued for 20 minutes to obtain a ceramic green body gel.

[0036] Example 3

[0037] This embodiment provides a ceramic green body gel, comprising the following implementation steps:

[0038] Step 1: Add 24kg of lanthanum oxide powder, 16kg of yttrium oxide powder, 48kg of cerium oxide powder, 12kg of zirconium dioxide powder and 16kg of titanium dioxide powder into a ball mill, then add 460L of deionized water and 90kg of zirconium oxide grinding balls with a diameter of 5mm, ball mill and mix for 15h, filter the material, remove the zirconium oxide grinding balls, dry the remaining slurry, and crush it to obtain rare earth powder.

[0039] Step 2: 80 kg of rare earth powder, 160 kg of boric acid, 100 kg of melamine, and 8000 L of deionized water are mixed, stirred at 95 ° C for 30 minutes to dissolve the boric acid and melamine in the deionized water, and the mixed powder is stably dispersed in the deionized water, then heated to 150 ° C, stirred for 4 hours at a frequency of 50 kHz and a stirring speed of 1200 r / min with ultrasonic assistance, and then stopped stirring, and continued ultrasonic treatment at the same frequency for 3 hours to obtain a gel precursor; the gel precursor is transferred to a crucible, and then placed in a vacuum sintering furnace, and kept warm for 4 hours under nitrogen protection and 1900 ° C. After cooling, the sintered block is crushed and passed through a 200 mesh sieve to obtain a rare earth composite powder.

[0040] Step 3: Add 60 kg of rare earth composite powder, 900 L of isopropanol and 300 L of deionized water into a stirring tank, stir and mix, then ultrasonically disperse for 60 minutes, add 240 L of 20% ammonia water and 90 L of tetraethyl orthosilicate, stir at 30°C for 12 hours, centrifuge, wash the precipitate with deionized water 5 times, and dry to obtain a rare earth admixture.

[0041] Step 4: Add 20kg of potassium feldspar, 18kg of sodium feldspar, 55kg of quartz, 20kg of aluminum powder, 2kg of magnesium powder, 2kg of lithium fluoride powder and deionized water into a ball mill and mix for 6 hours, then add 20kg of rare earth admixture, 15kg of methacrylamide, 1kg of N,N'-methylenebisacrylamide and 0.4kg of ammonium citrate and stir for 3 hours, wherein ammonium citrate is a dispersant, and the solid content is adjusted to 60±5%, and then the pH value is adjusted to 9 with ammonia water, and then 2kg of ammonium persulfate and N,N,N',N'-tetramethylethylenediamine mixed in a mass ratio of 3:2 are added as a catalyst, and the temperature is raised to 75±5°C and stirring is continued for 30 minutes to obtain a ceramic green body gel.

[0042] Comparative Example 1: Based on Example 3, the rare earth powder in step 1 is used in the same proportion to replace the rare earth admixture in step 4, and the other steps remain unchanged to prepare a ceramic green body gel.

[0043] Comparative Example 2: Based on Example 3, no rare earth admixture is added, and the other steps remain unchanged to prepare a ceramic green body gel.

[0044] Comparative Example 3: Based on Example 3, the amount of methacrylamide was increased to 30 kg, the amount of the cross-linking agent and the catalyst was doubled, and the other steps remained unchanged to prepare a ceramic green body gel.

[0045] Performance tests were performed on Examples 1 to 3 and Comparative Examples 1 to 3. According to GB / T4740-1999, different ceramic green body gels were prepared into green bodies with a diameter of 20 mm × 20 mm × 20 mm. The green bodies were air-dried for 8 hours and the surface conditions were observed. Then, the green bodies were kept warm and fired at 1450 ± 25 ° C for 3 hours to obtain different ceramic samples. The surface conditions were observed and the compressive strength was tested. The results are shown in Table 1:

[0046] Table 1

[0047]

[0048]

[0049] It can be seen from Table 1 that the green bodies in Examples 1 to 3 are defect-free and have high compressive strength after firing. The green bodies in Comparative Examples 1 and 2 have cracks because too little gel material is used without adding rare earth admixtures. The samples in Comparative Example 3 have cracks and pores because too much gel material is used, resulting in a large amount of gas generated during the firing process.

[0050] It should be noted that, in this article, terms such as "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.

[0051] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a ceramic green body gel, characterized in that: The steps include: Step 1: Mix rare earth powder, boric acid, melamine and deionized water, stir at 90-95°C for 20-30min, heat to 120-150°C, stir at 40-50kHz ultrasonic assistance and 800-1200r / min stirring speed for 2-4h, stop stirring and continue ultrasonic treatment for 2-3h to obtain a gel precursor; Step 2: keeping the gel precursor under nitrogen protection at 1850-1900° C. for 2-4 hours, cooling, crushing, and passing through a 150-200 mesh sieve to obtain a rare earth composite powder; Step 3: Mix the rare earth composite powder, isopropanol and deionized water and disperse them by ultrasonication, add 20wt% ammonia water and ethyl orthosilicate, stir at 25-30°C for 10-12h, centrifuge, wash and dry to obtain a rare earth admixture; Step 4: Add potassium feldspar, sodium feldspar, quartz, aluminum powder, magnesium powder, lithium fluoride powder and deionized water into a ball mill and mix for 4-6 hours, then add rare earth additives, acrylamide monomer, crosslinking agent and ammonium citrate and stir for 2-3 hours, adjust the solid content to 60±5%, and then adjust the pH value to 8.5-9 with ammonia water, add a catalyst and heat to 75±5°C and continue stirring for 15-30 minutes to obtain a ceramic green body gel; The dosage ratio of potassium feldspar, sodium feldspar, quartz, aluminum powder, magnesium powder, lithium fluoride powder, rare earth admixture, acrylamide monomer, crosslinking agent, ammonium citrate and catalyst in step 4 is 15-20g: 14-18g: 45-55g: 15-20g: 1-2g: 1-2g: 15-20g: 10-15g: 0.75-1g: 0.3-0.4g: 1-2g.

2. The method for preparing a ceramic green body gel according to claim 1, characterized in that: The rare earth powder is prepared by the following steps: Lanthanum oxide powder, yttrium oxide powder, cerium oxide powder, zirconium dioxide powder, titanium dioxide powder, deionized water and zirconium oxide grinding balls with a diameter of 5 mm are added into a ball mill, ball-milled and mixed for 10-15 hours, the material is filtered, dried, and crushed to obtain rare earth powder.

3. The method for preparing a ceramic green body gel according to claim 2, characterized in that: The dosage ratio of the lanthanum oxide powder, yttrium oxide powder, cerium oxide powder, zirconium dioxide powder, titanium dioxide powder, deionized water and zirconium oxide grinding balls is 10-12g: 6-8g: 20-24g: 5-6g: 4-8g: 180-230mL: 40-45g.

4. The method for preparing a ceramic green body gel according to claim 1, characterized in that: The dosage ratio of the rare earth powder, boric acid, melamine and deionized water in step 1 is 0.5-0.8 g: 1.5-1.6 g: 1 g: 80 mL.

5. The method for preparing a ceramic green body gel according to claim 1, characterized in that: The usage ratio of the rare earth composite powder, isopropanol, deionized water, ammonia water and tetraethyl orthosilicate in step 3 is 15-20 g: 250-300 mL: 80-100 mL: 60-80 mL: 25-30 mL.

6. The method for preparing a ceramic green body gel according to claim 1, characterized in that: The acrylamide monomer is one of dimethyl acrylamide and methacrylamide or a mixture of the two in any ratio.

7. The method for preparing a ceramic green body gel according to claim 1, characterized in that: The cross-linking agent is N,N'-methylenebisacrylamide.

8. The method for preparing a ceramic green body gel according to claim 1, characterized in that: The catalyst is prepared by mixing ammonium persulfate and N,N,N',N'-tetramethylethylenediamine in a mass ratio of 3:

2.

9. A ceramic green body gel, characterized in that: Prepared by the preparation method according to any one of claims 1 to 8.