A method for recovering lithium from ternary cathode waste

By separating other metal elements from the positive electrode waste of ternary lithium battery and performing high-temperature roasting in conventional air in tunnel kiln, the safety hazards and high production costs of high-temperature roasting in lithium battery positive electrode waste are solved, and the problem of high-temperature roasting in lithium battery positive electrode waste is achieved. High lithium recovery rate and low production cost effect.

CN116995327BActive Publication Date: 2024-11-26JIANGXI JINHUI LITHUIM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310976768.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-04
Publication Date
2024-11-26
Estimated Expiration
2043-08-04

AI Technical Summary

Technical Problem

The prior art has problems such as high-temperature roasting safety hazards, high production costs, high equipment requirements and other rare metal elements that lead to difficulties in the extraction of lithium and low extraction rate in the recycling process of lithium in the positive electrode waste of ternary lithium batteries.

Method used

Using ternary positive electrode waste as raw material and fully mixed with carbon powder, conventional high-temperature roasting in the tunnel kiln is carried out in the tunnel kiln. Through crushing, leaching, purification and lithium sedimentation processes, other metal elements are separated first, reducing process costs and improving lithium recovery rate .

Benefits of technology

It has achieved high lithium recovery rate, low production costs, environmental protection and pollution-free, improved production scale and economic benefits, and reduced environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention provides a method for recovering lithium from ternary positive electrode waste, which uses waste ternary battery waste as raw materials after crushing and screening, and undergoes processes such as crushing, mixing and removing impurities, making brick-shaped blocks, roasting, leaching, and lithium precipitation to prepare lithium salts, providing a method for recovering lithium with simple process and high efficiency; the ternary positive electrode waste is roasted in a tunnel kiln, which has large production capacity; at the same time, inert gas protection is not required during the roasting process, and roasting in conventional air is safe and low in cost; no acid is required during the reaction process, the lithium recovery rate is high, the process flow is short, and the environmental protection is obvious, and the economic and technical benefits are obvious, and the lithium recovery rate is high. Reduce the environmental pollution of waste resources and achieve sustainable development.
Need to check novelty before this filing date? Find Prior Art

Description

Technical field:

[0001] The present invention relates to a method for recovering valuable metal materials from waste materials, mainly a method for extracting lithium from discarded waste battery positive electrode materials, in particular a method for recovering lithium from ternary positive electrode waste materials. Background technology:

[0002] With the continuous rise and development of lithium-ion new energy, lithium-ion new energy vehicles have been recognized by the market. As an important means of transportation, new energy vehicles have been widely popularized. As an important power source for new energy vehicles, lithium batteries have also been unprecedentedly developed and increased. However, any chemical product has service life and years requirements. If scrapped lithium batteries are not processed, they will have a serious impact on the environment and society. For example, the waste of ternary positive electrodes contains a large amount of recyclable rare metal elements. Recycling them has great social and economic benefits for both society and enterprises.

[0003] The determination of China's dual carbon goals has made green, low-carbon and efficient recycling of resources an important direction for future industry development. Driven by the rapid demand for lithium-ion batteries in the new energy vehicle and energy storage markets, a large number of waste and retired lithium-ion batteries will increase sharply in the next few years. Due to its dual attributes of environment and resources, the green and low-carbon recovery and reuse of valuable metals has become a hot topic in the current research field of waste lithium-ion battery recycling.

[0004] Waste power lithium-ion batteries are rich in heavy metals such as lithium, nickel, and cobalt, as well as organic matter such as electrolytes and binders, which pose a potential threat to the natural environment and human health. Waste lithium-ion batteries contain a large amount of valuable metal components, far exceeding the valuable metal content of ores in nature. If waste lithium-ion batteries can be safely and harmlessly treated, it will not only alleviate my country's resource shortage and promote the healthy development of the industry, but also avoid environmental pollution caused by waste batteries. At present, China's waste power lithium battery production is about 34GWh, and it is expected that the production of waste power lithium batteries will reach 134GWh in 2025, of which ternary lithium-ion batteries account for more than 50%.

[0005] At present, the waste lithium batteries that have been eliminated from the market are usually treated by reducing acid leaching, that is, the waste ternary positive electrode materials are leached with sulfuric acid and hydrogen peroxide to dissolve the metal elements nickel, cobalt, manganese and lithium. After purification, the pure Ni, Co and Mn salt solutions are obtained by solution extraction. This method is simple in process and has a low recovery rate for lithium.

[0006] In addition, the recycling methods for waste ternary lithium batteries are mainly divided into pyrometallurgy, hydrometallurgy and biometallurgy. Pyrometallurgy has strong adaptability to raw materials and rapid reaction, but it consumes a lot of energy (melting temperature > 1500°C) and produces toxic gases. The bacteria required for biometallurgy have high environmental requirements and a long metal extraction cycle, which is rarely mentioned in general industry. Hydrometallurgy is widely used due to its mild conditions, low energy consumption and high selectivity for metals, but the process requires the use of strong acids and reducing agents, which may lead to equipment corrosion, long purification process, complex process, and secondary pollution of the environment.

[0007] For example, Chinese patent CN114684872A discloses "A method for carbon reduction roasting and recovery of ternary positive electrode waste". This method combines multiple steps such as carbon reduction roasting (argon protection), water leaching, acid leaching, etc., which can effectively extract, recover and reuse ternary positive electrode waste, especially the valuable metals contained therein, and at the same time prepare high-purity, high-quality spherical ternary material precursors and LiPF6 organic solutions that can be directly used as raw materials for lithium-ion battery electrolytes.

[0008] Another Chinese patent CN114597526A discloses "A method for extracting lithium salts from waste positive electrode materials of ternary lithium batteries through reduction roasting", wherein scrapped lithium batteries are disassembled to obtain ternary positive electrode sheets, the ternary positive electrode sheets are crushed and sieved to obtain ternary positive electrode powder; the ternary positive electrode powder is placed in a reducing atmosphere roasting furnace for reduction roasting to obtain roasted ternary material; the roasted ternary material is placed in a ball mill for slurry ball milling to obtain ball-milled ternary material; the ball-milled ternary material is transferred to a reactor and leached with water, a lithium-rich solution and a residue are obtained through solid-liquid separation, the lithium-rich solution is refined and impurities are removed to obtain a refined lithium-rich solution; carbon dioxide is introduced into the refined lithium-rich solution to obtain a lithium carbonate precipitate; the lithium carbonate precipitate is subjected to slurry washing, centrifugal dehydration, and drying steps to obtain battery-grade lithium carbonate.

[0009] It can be seen from the above disclosed technical solutions that the above prior art requires high-temperature roasting in a reducing atmosphere or an argon protected atmosphere for the recovery of lithium from the positive electrode waste of ternary lithium batteries. The gas atmosphere has safety hazards and increases production costs on the one hand, and on the other hand, the high equipment requirements restrict production capacity. At the same time, since the positive electrode waste of ternary lithium batteries contains a large amount of other rare metal elements such as nickel, cobalt, manganese, etc. in addition to lithium, the presence of other rare metal elements makes it difficult to purify lithium in the subsequent separation and extraction of lithium elements, and also seriously affects the extraction rate of lithium, and further increases the extraction cost of lithium.

[0010] Based on the deficiencies in the prior art, a method for recovering lithium from ternary positive electrode waste is provided, wherein the ternary positive electrode waste is used as a raw material and fully mixed with carbon powder, and other metal elements in the ternary positive electrode waste are preliminarily separated before extraction and roasting, and then the material containing lithium elements is conventionally roasted in a tunnel kiln using pressed bricks, and is carried out under the protection of a gas-free atmosphere, thereby reducing its process calcination cost and production cost, and then the lithium carbonate product is obtained after crushing, leaching, purification, and lithium precipitation. The present invention has the advantages of large production scale, high lithium recovery rate, low equipment corrosion, low operating cost, and environmental protection and pollution-free. It also reduces environmental pollution in the process of resource development and utilization, and achieves sustainable development. Summary of the invention:

[0011] The present invention provides a method for recovering lithium from ternary positive electrode waste, which uses waste ternary battery waste as raw materials after crushing and screening, and undergoes processes such as crushing, mixing and removing impurities, making brick-shaped blocks, roasting, leaching, and lithium precipitation to prepare lithium salts, providing a method for recovering lithium with simple process and high efficiency; the ternary positive electrode waste is roasted in a tunnel kiln, which has large production capacity; at the same time, inert gas protection is not required during the roasting process, and roasting in conventional air is safe and low in cost; no acid is required during the reaction process, the lithium recovery rate is high, the process flow is short, and the environmental protection is obvious, and the economic and technical benefits are obvious, and the lithium recovery rate is high. Reduce the environmental pollution of waste resources and achieve sustainable development.

[0012] The present invention discloses a method for recovering lithium from ternary positive electrode waste, which uses waste ternary battery waste as raw materials after crushing and screening, and comprises the following steps:

[0013] (a) Crushing: The positive electrode materials recovered from the dismantling of waste ternary batteries are crushed and sieved to obtain fine powder of ternary positive electrode waste;

[0014] (b) Mixing and impurity removal: the fine powder of the ternary cathode waste and N-methylpyrrolidone are fully mixed to obtain a ternary cathode mixed slurry; after the ternary cathode mixed slurry is mixed with polyacrylamide, potassium sulfate is added, and the polyacrylamide is heated to hydrolyze the polyacrylamide. After the reaction is completed, the impurity ions are dissolved in the separation liquid, and the solid and liquid are separated to obtain a separation liquid and a solid residue;

[0015] (c) Brick making material: the solid slag is firstly mixed with the mixed binder and then mixed with the carbon powder, and then sent to a press device to be pressed into a brick shape, which is a baked mixed brick material;

[0016] (d) Calcination: The calcined mixed bricks are stacked on a tunnel kiln car and sent into a tunnel kiln device for calcination at high temperature in the tunnel kiln. After calcination, they are mechanically crushed and ball-milled to obtain calcined and crushed fine powder;

[0017] (e) leaching: adding water to the roasted and crushed fine powder and stirring and mixing to perform leaching, and performing solid-liquid separation using a belt filter device to obtain a lithium-containing solution and leached residue;

[0018] (f) Purification and lithium precipitation: The lithium-containing solution is purified and impurities are removed, and then lithium is precipitated with sodium carbonate to prepare battery-grade lithium carbonate.

[0019] The method for recovering lithium from ternary cathode waste comprises:

[0020] In step (a), the lithium content in the fine powder of the ternary positive electrode waste is controlled between 2.0-6.0 wt%, and the fine powder of the ternary positive electrode waste is ≤ 60 mesh.

[0021] In the method for recovering lithium from ternary positive electrode waste, in step (b), the mass ratio of the ternary positive electrode waste fine powder to carbon powder is 1.0:(0.1-3.0), and the carbon powder is ≤60 mesh.

[0022] The method for recovering lithium from ternary positive electrode waste, in which step (b) controls the mass ratio of ternary positive electrode waste fine powder and N-methylpyrrolidone to 1:2.5-2.8; controls the mass ratio of ternary positive electrode mixed slurry and polyacrylamide to 1:0.2-0.35; and controls the amount of potassium sulfate added to 0.01-0.05 of the mass of the ternary positive electrode waste fine powder.

[0023] In the method for recovering lithium from ternary positive electrode waste, the mixed binder in step (c) is sodium carbonate or sodium hydroxide solution, and the amount of sodium carbonate or sodium hydroxide solution added is to ensure that the solid slag and carbon powder can be pressed into a brick shape after being stirred and mixed evenly without falling apart.

[0024] In the method for recovering lithium from ternary cathode waste, in step (c), the high-temperature roasting temperature is 420° C.-1050° C., and the roasting time is 0.5 h-3.5 h.

[0025] In the method for recovering lithium from ternary cathode waste, in step (d), the calcined and crushed fine powder is 60-200 meshes.

[0026] In the method for recovering lithium from ternary cathode waste, in step (e), the leaching temperature is 20°C-90°C, and the leaching time is 0.5h-2.0h.

[0027] The method for recovering lithium from ternary positive electrode waste, in step (e), the lithium ion concentration in the leached residue can reach ≤0.10wt%; the lithium ion concentration of the lithium-containing solution is ≥15g / L; in step (f), the impurity removal method is first to adjust the pH to 8-9 with alkali to remove nickel, cobalt and manganese, and then to adjust the pH to 11-13 with sodium carbonate and sodium hydroxide to remove calcium and magnesium.

[0028] The present invention discloses a method for recovering lithium from ternary positive electrode waste, and its main process flow is: ternary positive electrode waste crushing → screening treatment → mixing and impurity removal treatment → including adding chemical agents → removing other rare metal elements → making brick block materials → tunnel kiln roasting → leaching → purification → lithium precipitation and making lithium salt products such as battery-grade lithium carbonate.

[0029] The present invention discloses a method for recovering lithium from ternary positive electrode waste, which uses ternary positive electrode waste crushed material as raw material and adopts the above-mentioned process method, and has the following characteristics: adopting a tunnel kiln to roast the ternary positive electrode waste, the production capacity is large; the roasting process does not need to be carried out under inert gas protection conditions, and the roasting can be carried out in conventional air, and the roasting is safe and low in cost; in the existing production of lithium extraction from ternary positive electrode waste, there is no process method and device for roasting using a tunnel kiln as the present invention, which is because on the one hand, the raw material mainly composed of ternary positive electrode waste is difficult to press into a brick shape, that is, when it is sent to the tunnel kiln device for roasting after forming, it is very easy to collapse the kiln, that is, due to the insufficient adhesion of the raw material composition, or the control of the content of other metal elements in the component composition of the raw material, it is very easy to disperse under high temperature conditions, thereby seriously affecting the production output and the roasting process, and greatly increasing the production cost. Second, in the existing process of extracting lithium from ternary positive electrode waste as raw material, it is generally necessary to produce under protective gas conditions, and the tunnel kiln has a higher production cost due to its strong fluidity. The reaction process of the present invention does not require acid or chemical reducing agent, has high lithium recovery rate, short process flow and is environmentally friendly.

[0030] Second, the present invention adopts a mixed impurity removal process by adding N-methylpyrrolidone and the like to the fine powder of the ternary positive electrode waste and mixing them fully to obtain a ternary positive electrode mixed slurry; after the ternary positive electrode mixed slurry is mixed with polyacrylamide, potassium sulfate is added and heated to hydrolyze the polyacrylamide; through the above-mentioned reaction process, other rare metal ions in the fine powder of the ternary positive electrode waste such as nickel, Co, Mn metals, etc. can be removed and dissolved in the filtered solution, that is, the separation liquid, and then the separation liquid is used to recover nickel, Co, Mn and other metals using existing processes. The solid slag obtained after separation in this step mainly contains lithium elements, which facilitates the subsequent recovery of lithium, thereby greatly improving the leaching rate of lithium, and further increasing the recovery rate of lithium to more than 97%;

[0031] Third, the present invention adds sodium carbonate or sodium hydroxide solution as a binder in the process of making bricks, which greatly increases the adhesiveness of the solid slag when it is mixed with carbon powder and pressed into bricks, so that the fine powder of the ternary positive electrode waste is sticky and does not fall apart when making bricks. Therefore, when it is sent to the tunnel kiln for roasting, it can greatly prevent the occurrence of kiln collapse through practical use, thereby improving its production efficiency. Its production cost is reduced; the lithium leaching rate is generally above 90%, and the highest is above 97.6%. It realizes the transformation of solid waste into treasure, with great economic and social benefits. Specific implementation method:

[0032] The present invention is further described in detail below in conjunction with specific implementation methods. The implementation method of the present invention uses the crushed powder of a company's ternary positive electrode waste as raw material, that is, the ternary positive electrode waste fine powder or ternary positive electrode waste has the same meaning; the devices and methods used in the following methods that are not described are all prior art methods and devices. The following description refers to mass parts or mass ratios unless otherwise specified.

[0033] The present invention provides a method for recovering lithium from ternary positive electrode waste, wherein the ternary positive electrode waste is used as raw material and is fully mixed with carbon powder, etc., pressed into bricks, conventionally roasted in a tunnel kiln, roasted under the protection of a non-protective gas atmosphere, and then crushed, leached, purified, and lithium precipitated to obtain a lithium carbonate product. Compared with the prior art, the present invention has the advantages of large production scale, high lithium recovery rate up to 97%, low equipment corrosion, low operating cost, environmental protection, no pollution, easy operation, high efficiency and reliability.

[0034] The specific scheme is that the method for recovering lithium from ternary positive electrode waste disclosed in the present invention uses waste ternary battery waste as raw material after crushing and screening, and comprises the following steps:

[0035] (a) Crushing: The positive electrode materials recovered from the dismantling of waste ternary batteries are crushed and then sieved to control the lithium content in the ternary positive electrode waste to be between 2.0-6.0Wt%, and the fine powder of the ternary positive electrode waste is controlled to be ≤60 mesh; thus obtaining the fine powder of the ternary positive electrode waste;

[0036] (b) Mixing and removing impurities: First, the fine powder of the ternary positive electrode waste and N-methylpyrrolidone are fully mixed to obtain a ternary positive electrode mixed slurry; then, after the ternary positive electrode mixed slurry is mixed with polyacrylamide, potassium sulfate or sodium sulfate is added, and the polyacrylamide is heated to undergo a hydrolysis reaction. After the reaction is completed, solid-liquid separation is performed to obtain a separated liquid and solid residue; the mass ratio of the ternary positive electrode waste fine powder and N-methylpyrrolidone is controlled to be 1:2.5-2.8; the mass ratio of the ternary positive electrode mixed slurry and polyacrylamide is controlled to be 1:0.2-0.35; and the amount of potassium sulfate added is controlled to be 0.01-0.05 of the mass of the ternary positive electrode waste fine powder;

[0037] (c) Brick making material, the solid slag is first fully mixed with the mixed binder, then mixed with the carbon powder, and sent to a press device to be pressed into a brick shape, which is a roasted mixed brick material; the mixed binder is sodium carbonate or sodium hydroxide solution, and the amount of sodium carbonate or sodium hydroxide solution added is to ensure that the solid slag and the carbon powder can be pressed into a brick shape after being stirred and mixed evenly without falling apart; the mass ratio of the ternary positive electrode waste fine powder to the carbon powder is 1.0: (0.1-3.0), and the carbon powder is ≤ 60 mesh; the high temperature roasting temperature is 420°C-1050°C, and the roasting time is 0.5h-3.5h;

[0038] (d) calcination: stacking the calcined mixed bricks on a tunnel kiln car, sending them into a tunnel kiln device, calcining them at high temperature in the tunnel kiln, and then mechanically crushing and ball milling them. The calcined and crushed fine powder is 60-200 meshes. The calcined and crushed fine powder is obtained.

[0039] (e) Leaching: adding water to the roasted and crushed fine powder and stirring and mixing to leach, and separating the solid and liquid by a belt filter device, the leaching temperature is 30°C-90°C, and the leaching time is 0.5h-2.0h. The lithium ion concentration in the leached residue can reach ≤0.10wt%; the lithium ion concentration of the lithium-containing solution is controlled to be ≥15g / L; obtaining the lithium-containing solution and leached residue;

[0040] (f) Purification and lithium precipitation: The lithium-containing solution is purified and impurities are removed by first adjusting the pH to 8-9 with alkali to remove the remaining small amount of nickel, cobalt and manganese, and then adjusting the pH to 11-13 with sodium carbonate and sodium hydroxide to remove calcium and magnesium; and then using sodium carbonate to precipitate lithium to prepare battery-grade lithium carbonate.

[0041] The following unexplained parts are the same as the technical solutions disclosed above. At the same time, the technologies involved that are not explained are all carried out according to the existing technical solutions, such as ball milling can be dry or wet ball milling. All other raw materials used in the present invention are obtained commercially. The test data of battery-grade lithium carbonate prepared by specific embodiments 1-3 of the method of the present invention are shown in Table 1 below.

[0042] Example 1

[0043] The positive electrode materials recovered from the dismantling of the waste ternary positive battery are crushed and passed through a 60-mesh sieve, and the material under the sieve is taken to obtain a ternary positive electrode waste fine powder of ≤60 mesh, and then the ternary positive electrode waste fine powder and N-methylpyrrolidone are fully mixed to obtain a ternary positive electrode mixed slurry; then the ternary positive electrode mixed slurry is mixed with polyacrylamide, and potassium sulfate or sodium sulfate is added, and the polyacrylamide is heated to hydrolyze. This step is processed according to the prior art scheme. After the reaction is completed, metal ions such as Co and Mn in the ternary positive electrode waste fine powder, that is, impurity ions relative to the lithium ions of the present invention, enter the separation liquid in this step. Therefore, it is convenient to remove impurities, extract and separate lithium ions in the subsequent process; impurity ions enter the separation liquid after solid-liquid separation to obtain separation liquid and solid slag; the metal ions mainly contained in the obtained solid slag are solid slag materials mainly composed of lithium, and other metal ions enter the separation solution; the filtration is carried out by suction filtration or pressure filtration. In the impurity removal process of this step, the mass ratio of the fine powder of the ternary positive electrode waste and N-methylpyrrolidone is controlled to be 1:2.5-2.8; the mass ratio of the ternary positive electrode mixed slurry and polyacrylamide is controlled to be 1:0.2-0.35; and the amount of potassium sulfate added is controlled to be 0.01-0.05 of the mass of the fine powder of the ternary positive electrode waste;

[0044] Then, a sodium hydroxide solution as a binder is added to the solid slag. The sodium hydroxide solution and the like are all commercially available. For example, the concentration of the sodium hydroxide solution is below 5%. The solid slag is first mixed with the sodium hydroxide solution until the mixture is held tightly by hand without falling apart, so as to obtain a mixture of the solid slag and the sodium hydroxide solution. Finally, the mixture is mixed with 100-mesh carbon powder in a mixer at a mass ratio of 1:1 and then pressed into a brick in a pressing device to obtain a baked mixture brick. The brick-shaped baked material is placed on a tunnel kiln car device, sent into a tunnel kiln device, and baked in the tunnel kiln. The baked mixture brick is heated in the tunnel kiln for 8 hours. The mixture was roasted at 50°C for 3.0h, mechanically crushed and ball-milled to 60-200 mesh after roasting and cooling, and water was added to the roasted and crushed fine powder clinker, stirred and leached at 60°C for 1.0h, and solid-liquid separation was performed to obtain a lithium-containing solution and leached slag; the lithium leaching rate was 95.8% after testing, and the lithium ion concentration in the leached slag was 0.15wt%; the lithium ion concentration of the lithium-containing solution was 24.7g / L, and the pH was adjusted to 9.0 with caustic soda flakes, and then the solid-liquid separation was performed, and then the pH was adjusted to 11-13 with sodium carbonate and sodium hydroxide, and then the calcium and magnesium ions were removed, and lithium was precipitated with sodium carbonate to prepare battery-grade lithium carbonate. The recovery rate of lithium is shown in Table 2.

[0045] In the technical solutions disclosed in the following Examples 2 and 3, except for the parameters disclosed below, the remaining undisclosed ones are the same as the solutions and data disclosed in Example 1 and the specific implementation methods.

[0046] Example 2

[0047] The positive electrode materials recovered from the dismantling of waste ternary positive electrode batteries are crushed and passed through a 60-mesh sieve, and the sieved materials are taken to obtain ≤60-mesh ternary positive electrode waste fine powder, and then the ternary positive electrode waste fine powder and 100-mesh carbon powder are placed in a mixer at a mass ratio of 1:0.66, fully mixed and evenly pressed into bricks to obtain baked mixed bricks; the baked mixed bricks are baked at 900°C in a tunnel kiln for 3.0h, and after baking and cooling, they are mechanically crushed and ball-milled to 60-200 meshes. Then, the roasted crushed fine powder clinker was added with water and stirred at 60°C for 1.0h, and then solid-liquid separation was performed to obtain a lithium-containing solution and leached slag; the lithium leaching rate was tested to be 97.6%, and the lithium ion concentration in the leached slag was 0.10wt%; the lithium ion concentration of the lithium-containing solution was 26.2g / L, and the pH was adjusted to 9.0 with caustic soda flakes, and then solid-liquid separation was performed, and then the pH was adjusted to 11-13 with sodium carbonate and sodium hydroxide, and then calcium and magnesium ions were removed, and lithium was precipitated with sodium carbonate to prepare battery-grade lithium carbonate. The recovery rate of lithium in the fine powder of the raw material ternary positive electrode waste was tested, as shown in Table 2.

[0048] Example 3

[0049] The positive electrode materials recovered from the dismantling of waste ternary positive electrode batteries are crushed and passed through a 60-mesh sieve, and the sieved materials are taken to obtain ≤60-mesh ternary positive electrode waste fine powder, and then the ternary positive electrode waste fine powder and 100-mesh carbon powder are placed in a mixer at a mass ratio of 1:2 and fully mixed and evenly pressed to obtain baked mixed bricks; the baked mixed bricks are baked at 500°C in a tunnel kiln for 2.0h, and after baking and cooling, they are mechanically crushed and ball-milled to 60-200 mesh, and then The calcined, crushed, finely powdered clinker was added with water and stirred for leaching at 30°C for 2.0h, followed by solid-liquid separation to obtain a lithium-containing solution and leached slag; the lithium leaching rate was detected to be 94.5%, and the lithium ion concentration in the leached slag was 0.18wt%; the lithium ion concentration of the lithium-containing solution was 22.8g / L, and the pH was adjusted to 9.0 with caustic soda flakes, followed by solid-liquid separation, and then the pH was adjusted to 11-13 with sodium carbonate and sodium hydroxide, and then lithium was precipitated with sodium carbonate to prepare battery-grade lithium carbonate.

[0050] Table 1 Test results of main indicators of battery-grade lithium carbonate prepared by the method of the present invention,

[0051]

[0052]

[0053] It is noted that the data disclosed in Table 1 above are the test data of the battery-grade lithium carbonate products prepared in Examples 1-3. The test data of each embodiment are somewhat different, and the data in Table 1 above are the average data; it can be seen from Table 1 above that the battery lithium carbonate extracted by the method of the present invention using the crushed powder of the ternary positive electrode waste as the raw material has various indicators that are better than the quality index requirements of battery-grade lithium carbonate, and the recovery rate of lithium in the raw material is as high as 97.6%, as shown in Table 2 below, etc.

[0054] Table 2: The leaching rate and recovery rate of the specific embodiments of the present invention and the comparative embodiments are shown in Table 2.

[0055]

[0056] Note: The lithium content (%) of the ternary positive electrode waste described in Table 2 refers to the lithium extraction raw material used in the present invention; and the mass (kg) of the ternary positive electrode waste is for the convenience of comparison and explanation with 10 kg of raw material for comparison. From the data in Table 2 above, it can be seen that compared with the prior art method of the comparative example, the lithium recovery rate of the present invention is nearly 6% higher than that of the prior art, and the method of the present invention has a large processing capacity for raw materials, which can be industrialized and mass-produced, and has high efficiency, with great economic and social benefits. However, it is difficult to achieve industrialization and scale-up using the existing technical solutions. The following comparative examples are all carried out using the existing technical methods, and the raw materials used are the same as those of the present invention.

[0057] Comparative Example 1

[0058] The raw materials used in the following comparative examples 1-3 are the same as those used in examples 1-3, but the mixed impurity removal process is not adopted, that is, the ternary positive electrode waste fine powder obtained in step (a) is not subjected to other metal ion removal treatments such as Co and Mn; at the same time, the roasting method thereof is also different from the roasting method of the tunnel kiln of the present invention, that is, the roasting is carried out under reducing atmosphere conditions; at the same time, brick pressing is not carried out; therefore, the processing amount of the raw materials of this method is small, which is not conducive to industrial and large-scale production;

[0059] The positive electrode materials recovered from the dismantling of waste ternary positive battery are crushed and passed through a 60-mesh sieve, and the material under the sieve is taken to obtain a 60-mesh ternary positive electrode waste fine powder, and the ternary positive electrode waste fine powder is placed in a reducing atmosphere roasting furnace for reduction roasting. The reducing atmosphere in the reduction roasting atmosphere is a mixed gas of carbon monoxide, nitrogen, and natural gas, and the reducing atmosphere concentration is 60%. The roasting temperature is 600°C, and the roasting time of the ternary positive electrode powder in the reduction furnace is controlled at 3h to obtain a roasted ternary material. The roasted ternary material is placed in a ball mill for slurry ball milling to obtain a ball-milled ternary material with a particle size of 100 meshes. The slurry material after ball milling is transferred to a water leaching reaction tank for water leaching reaction. The liquid-to-solid ratio of the water leaching reaction liquid is controlled at 4:1, and the reaction temperature is controlled at 60°C. The slurry after leaching is filtered and separated to obtain a leaching liquid and a residue after leaching. The lithium leaching rate is 89.8%, that is, the lithium recovery rate is less than 90%; the lithium ion concentration in the leached residue is 0.53wt%. The recovery rate of lithium in the fine powder of the raw material ternary positive electrode waste is 89.2%.

[0060] Comparative Example 2

[0061] The positive electrode materials recovered from the dismantling of waste ternary positive battery are crushed and passed through a 60-mesh sieve. The material under the sieve is taken to obtain a 60-mesh ternary positive electrode waste fine powder. The ternary positive electrode waste fine powder is mixed with carbon powder at a mass ratio of 2:1 and then argon gas protection is introduced into the roasting furnace for reduction roasting. The roasting temperature is 1050°C. The roasting time of the ternary positive electrode powder in the reduction furnace is controlled at 2h to obtain the roasted ternary material. The roasted ternary material is placed in a ball mill for slurry ball milling to obtain a ball-milled ternary material with a particle size of 100 mesh. The slurry material after ball milling is transferred to a water immersion reaction tank for water immersion reaction. The liquid-solid ratio of the water immersion reaction is controlled at 4:1, and the reaction temperature is controlled at 60°C. The slurry after leaching is separated by filtration to obtain a leachate and a residue after leaching. The lithium leaching rate is 89.6%, and the lithium ion concentration in the leached residue is 0.47wt%. The recovery rate of lithium in the fine powder of the raw material ternary positive electrode waste was tested to be 90.2%.

[0062] Comparative Example 3

[0063] The positive electrode materials recovered from the dismantling of waste ternary positive battery are crushed and passed through a 60-mesh sieve. The material under the sieve is taken to obtain a ternary positive electrode waste fine powder of ≤60 mesh. The ternary positive electrode waste fine powder is mixed with carbon powder at a mass ratio of 1:2 and then argon gas protection is introduced into the roasting furnace for reduction roasting. The roasting temperature is 900°C. The roasting time of the ternary positive electrode powder in the reduction furnace is controlled at 4h to obtain the roasted ternary material. The roasted ternary material is placed in a ball mill for slurry ball milling to obtain a ball-milled ternary material with a particle size of 100 mesh. The slurry material after ball milling is transferred to a water immersion reaction tank for water immersion reaction. The liquid-solid ratio of the water immersion reaction is controlled at 4:1, and the reaction temperature is controlled at 60°C. The slurry after leaching is separated by filtration to obtain a leachate and a residue after leaching. The lithium leaching rate is 88.7%, and the lithium ion concentration in the leached residue is 0.51wt%. The recovery rate of lithium in the fine powder of the raw material ternary positive electrode waste was tested to be 88.4%.

[0064] It is explained that the method of the present invention improves the lithium extraction efficiency in waste ternary positive electrode battery raw materials, and the leaching rate is also relatively high, and the prepared battery-grade lithium carbonate product meets the quality requirements.

Claims

1. A method for recovering lithium from ternary positive electrode waste, using waste ternary battery waste as raw material after crushing and screening, characterized in that: The following steps are involved: (a) Crushing: The positive electrode materials recovered from the dismantling of waste ternary batteries are crushed and sieved to obtain fine powder of ternary positive electrode waste; (b) Mixing and impurity removal: the fine powder of the ternary cathode waste and N-methylpyrrolidone are fully mixed to obtain a ternary cathode mixed slurry; after the ternary cathode mixed slurry is mixed with polyacrylamide, potassium sulfate is added, and the polyacrylamide is heated to hydrolyze the polyacrylamide. After the reaction is completed, the impurity ions are dissolved in the separation liquid, and the solid and liquid are separated to obtain a separation liquid and a solid residue; (c) Making brick material: the solid slag is firstly mixed with the mixed binder and then mixed with the carbon powder to be uniformly mixed, and then sent to a press device to be pressed into a brick shape, which is a baked mixed brick material; (d) Calcination: The calcined mixed bricks are stacked on a tunnel kiln car and sent into a tunnel kiln device. They are calcined at high temperature in an air atmosphere in the tunnel kiln. After calcination, they are mechanically crushed and ball-milled to obtain calcined and crushed fine powder; (e) Leaching: adding water to the roasted and crushed fine powder and fully stirring and mixing to carry out leaching, and separating the solid and liquid by a belt filter device to obtain a lithium-containing solution and leached residue; (f) Purifying and precipitating lithium: purifying and removing impurities from the lithium-containing solution, and then using sodium carbonate to precipitate lithium to prepare battery-grade lithium carbonate; In step (a), the lithium content in the ternary positive electrode waste fine powder is controlled to be between 2.0-6.0 wt%, and the ternary positive electrode waste fine powder is ≤ 60 mesh; In step (b), the mass ratio of the ternary cathode waste fine powder to the carbon powder is 1.0: (0.1-3.0), and the carbon powder is ≤ 60 mesh; Step (b) controlling the mass ratio of the ternary positive electrode waste fine powder to N-methylpyrrolidone to be 1:2.5-2.8; controlling the mass ratio of the ternary positive electrode mixed slurry to polyacrylamide to be 1:0.2-0.35; and controlling the amount of potassium sulfate added to be 0.01-0.05 of the mass of the ternary positive electrode waste fine powder; In step (c), the high temperature calcination temperature is 420°C-1050°C, and the calcination time is 0.5h-3.5h; In step (e), the leaching temperature is 20°C-90°C, and the leaching time is 0.5h-2.0h; In step (e), the lithium ion concentration in the leached residue can reach ≤0.10wt%; the lithium ion concentration of the lithium-containing solution is ≥15g / L; in step (f), the impurity removal method is to first adjust the pH to 8-9 with alkali to remove nickel, cobalt and manganese, and then adjust the pH to 11-13 with sodium carbonate and sodium hydroxide to remove calcium and magnesium.

2. The method for recovering lithium from ternary cathode waste according to claim 1, characterized in that: The mixed binder in step (c) is sodium carbonate or sodium hydroxide solution, and the amount of sodium carbonate or sodium hydroxide solution added is to ensure that the solid slag and carbon powder can be pressed into bricks after being stirred and mixed evenly without falling apart.

3. The method for recovering lithium from ternary cathode waste according to claim 1, characterized in that: In step (d), the roasted and crushed fine powder is 60 mesh-200 mesh.