A method for preparing 5-methylfurfural by utilizing 5-hydroxymethylfurfural
By loading metal nickel on niobium pentoxide to prepare Ni-TT-Nb2O5 catalyst, the problems of high cost, low yield and poor selectivity in the preparation process of 5-hydroxymethylfurfural to 5-methylfurfural are solved, and high efficiency is achieved , economical preparation of 5-methylfurfural.
Patent Information
- Application Number
- CN202311081809.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-25
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-08-25
AI Technical Summary
In the prior art, there are problems such as high cost, complex preparation method, low yield, poor selectivity and harsh reaction conditions in the direct hydrogenation process of 5-hydroxymethylfurfural to 5-methylfurfural, which limits the application of catalysts. .
Niobium pentoxide (Ni-TT-Nb2O5) catalyst supported by metal nickel to the hexagonal crystal system was prepared by hydrothermal calcining method to achieve selective hydrogenation of 5-hydroxymethylfurfural to form a high yield of 5-methyl Basic furfural.
The advantages of mild reaction conditions, high substrate conversion rate, strong catalyst selectivity and high product yield are achieved, filling the gap in non-precious metal catalysts in this reaction system.
Smart Images

Figure CN117065758B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of 5-methylfurfural preparation, and particularly relates to a method for preparing 5-methylfurfural by selectively hydrogenating 5-hydroxymethylfurfural. Background Art
[0002] 5-Methylfurfural (MF), as a direct hydrogenation product of 5-hydroxymethylfurfural, is a very useful chemical and can be used as a food additive and an intermediate in the synthesis of other chemicals.
[0003] At present, the system for preparing 5-methylfurfural by catalytic direct hydrogenation of 5-hydroxymethylfurfural is extremely difficult. This is mainly because in the process of hydrogenation of 5-hydroxymethylfurfural, compared with the C-OH structure, the C=O structure is easier to hydrogenate from both a kinetic and a thermodynamic point of view (ACS Catalysis, 2013, 2655–2668, Journal of Catalysis, 2016, 248-260), which undoubtedly causes great difficulties for the preparation of 5-methylfurfural. At present, only precious metal catalysts (Pt, Au, etc.) can achieve the preparation of 5-hydroxymethylfurfural to 5-methylfurfural, but the high cost and complex preparation method limit the application of catalysts (Nature Communications, 2021, 12 (1); Applied Catalysis B: Environmental, 2023, 122893). In addition, in the process of preparing 5-methylfurfural from 5-hydroxymethylfurfural, the low product yield, poor selectivity and harsh reaction conditions also pose great challenges to the preparation of 5-methylfurfural (Applied Catalysis B: Environmental, 2023, 122893). Therefore, it is urgent to develop and research a non-precious metal with mild reaction conditions, simple preparation method, low cost and high activity for this reaction system. Summary of the invention
[0004] The purpose of the present invention is to realize the one-step preparation of 5-methylfurfural from 5-hydroxymethylfurfural. The present invention loads nickel into pseudo-hexagonal niobium pentoxide (TT-Nb 2 O 5 ) 2 O 5A catalyst is provided, which can selectively hydrogenate the C-OH structure of 5-hydroxymethylfurfural in a single manner, so that 5-hydroxymethylfurfural is completely converted into 5-methylfurfural with high yield. The catalyst used in the present invention can be obtained by a hydrothermal calcination method, and the preparation method is simple. In addition, during the reaction process, the catalyst has the advantages of mild reaction conditions, high substrate conversion rate, strong catalyst selectivity, high product yield, etc. In addition, the catalyst is a non-precious metal catalyst, which fills the industry gap for preparing 5-methylfurfural from 5-hydroxymethylfurfural in a one-step method.
[0005] The technical problem to be solved by the present invention is achieved by adopting the following technical solutions:
[0006] The present invention provides a nickel / niobium pentoxide catalyst (Ni-TT-Nb 2 O 5 ), which comprises the following steps:
[0007] S1 First, dissolve urea in a beaker containing deionized water, then add Ni(NO 3 ) 2 6H 2 O into the mixed solution; then, the pseudo-hexagonal niobium pentoxide carrier was poured into the mixed solution and ultrasonicated, and finally, the beaker was placed in an oil bath at 95°C and stirred for 12 hours until the mixed solution was completely dry, and a light green solid powder was collected;
[0008] S2 The solid powder is then calcined in a tube furnace at N 2 / H 2 calcined in an atmosphere, and after the tube furnace cooled to room temperature, the black solid was collected, which was the nickel / niobium pentoxide catalyst;
[0009] Wherein, the pseudo-hexagonal niobium pentoxide (TT-Nb 2 O 5 ) The preparation method of the carrier is as follows:
[0010] a. Add ammonium niobium oxalate to a mixed solution containing deionized water and hydrogen peroxide, stir magnetically for 30 minutes, pour the mixed solution into a polytetrafluoroethylene liner, and react at 175°C;
[0011] b. After the reaction is completed, the reactor is cooled to room temperature, the product is collected, and repeatedly washed with deionized water and anhydrous ethanol;
[0012] c. The niobium pentoxide precursor was then placed in a vacuum drying oven at 60°C and dried overnight;
[0013] d. The dried niobium pentoxide precursor was then placed in a muffle furnace and calcined at 380° C. for 2 h to obtain a pseudo-hexagonal niobium pentoxide carrier.
[0014] Preferably, in step S1, Ni(NO 3 ) 2 6H 2 O and pseudo-hexagonal niobium pentoxide carrier are used in a mass ratio of 1:20 to 1:5, preferably Ni(NO 3 ) 2 6H 2 The mass ratio of O and pseudo-hexagonal niobium pentoxide carrier is 1:10.
[0015] In step S2, the solid powder is calcined in a tube furnace, specifically at N 2 / H 2 (10%) atmosphere, the temperature was raised to 300-600°C at 2-5°C / min and kept at this temperature for 2h.
[0016] In addition, preferably, in step a, the hydrogen peroxide is 30% by mass, the volumes of deionized water and hydrogen peroxide are 65 mL to 100 mL and 15 mL to 20 mL, respectively, and the volume ratio of the two is 4:1 to 5:1; the amount of ammonium niobium oxalate added is 5.2 g to 6.9 g, and the molar ratio of hydrogen peroxide to niobium is 10:1; in step b, the reaction is carried out at 175° C. for 12-18 hours; the mixture is washed alternately with deionized water and ethanol for 3-8 times; in step c, the residual material is placed in a vacuum drying oven and dried at 60-80° C. for 12-24 hours; in step d, the specific operation of calcination is to heat the mixture to 300-400° C. at 4-6° C. / min in a muffle furnace and then keep the temperature for 1-3 hours;
[0017] The present invention provides Ni-TT-Nb obtained by the preparation method 2 O 5 catalyst.
[0018] The present invention further provides a method for preparing 5-methylfurfural by selectively hydrogenating the C-OH structure of 5-hydroxymethylfurfural, which comprises the following steps: reacting 5-hydroxymethylfurfural, the Ni-TT-Nb as claimed in claim 5, 2 O 5 The catalyst and tetrahydrofuran are added into a closed reactor, the hydrogen replaces the air, and a catalytic reaction occurs to generate 5-methylfurfural.
[0019] Preferably, the conditions of the catalytic reaction are: reaction temperature 100-160° C., hydrogen pressure 0.1-4 MPa, preferably 1-3 MPa, stirring speed 400-1000 rpm, preferably 500-800 rpm, reaction time 1 h-8 h, preferably 3-6 h.
[0020] More preferably, the conditions of the catalytic reaction are: reaction temperature 160° C., hydrogen pressure 2 MPa, stirring speed 600 rpm, and reaction time 4 h.
[0021] In a specific embodiment, the 5-hydroxymethylfurfural, Ni-TT-Nb 2 O 5 The ratio of catalyst to tetrahydrofuran is 0.06-0.25 g: 0.025-0.075: 10 mL; preferably, the 5-hydroxymethylfurfural, Ni-TT-Nb 2 O 5 The ratio of catalyst to tetrahydrofuran was 0.126 g:0.05 g:10 mL.
[0022] Preferably, the closed reactor is a stainless steel closed reactor.
[0023] The beneficial effects of the present invention are as follows: the present invention constructs a non-precious metal catalyst Ni-TT-Nb 2 O 5 , selectively hydrogenate the C-OH structure of 5-hydroxymethylfurfural to prepare 5-methylfurfural. 2 O 5 As a catalyst, not only is the preparation method simple and the preparation cost low, but it also has a strong adsorption capacity for the C-OH structure of 5-hydroxymethylfurfural, so that 5-hydroxymethylfurfural can be completely converted to obtain a high yield of 5-methylfurfural. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 The gas chromatograms of 5-hydroxymethylfurfural and 5-methylfurfural prepared in Example 2 of the present invention when there is no catalyst.
[0025] Figure 2 The catalyst of Example 2 of the present invention is TT-Nb 2 O 5 Gas chromatogram of 5-hydroxymethylfurfural and 5-methylfurfural prepared.
[0026] Figure 3 The catalyst of Example 2 of the present invention is Ni-TT-Nb 2 O 5 Gas chromatograms of 5-hydroxymethylfurfural and 5-methylfurfural prepared at 500 °C.
[0027] Figure 4 This is the gas chromatogram of 5-hydroxymethylfurfural and 5-methylfurfural obtained when the dosage of 5-hydroxymethylfurfural is 0.126 g in Example 7 of the present invention. DETAILED DESCRIPTION
[0028] The technical solution of the present invention is clearly and completely described in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] Example 1: Preparation of different catalysts
[0030] The specific operations of the preparation experiments of different catalysts are as follows:
[0031] First, urea was dissolved in a beaker containing deionized water, and then Ni(NO 3 ) 2 6H 2 O into the mixed solution; then the pseudo-hexagonal niobium pentoxide carrier was poured into the mixed solution and ultrasonicated, and finally the beaker was placed in a 95°C oil bath and stirred for 12 hours to completely dry the mixed solution, and the light green solid powder was collected; then N 2 / H 2 The calcinations were carried out in a calcination atmosphere at 400, 500, and 600 °C, respectively. After the tube furnace was cooled to room temperature, black solid powders were collected and named Ni-TT-Nb 2 O 5 400, Ni-TT-Nb 2 O 5 500, Ni-TT-Nb 2 O 5 600.
[0032] Example 2: Effect of different catalysts on 5-methylfurfural yield
[0033] The specific operation steps of the comparative experiment of different catalysts are as follows:
[0034] 0.126 g 5-hydroxymethylfurfural, different catalysts and 10 mL tetrahydrofuran were added into a stainless steel closed reactor and filled with 2 MPa H 2 , reacted at 130°C for 4h at a stirring speed of 600rpm. After the reaction was completed, it was cooled to room temperature. A centrifuge was used for solid-liquid separation (8000r / min, 5min), and a gas chromatograph (GC, Agilent 7890A) was used for quantitative analysis. The conversion rate of 5-hydroxymethylfurfural, the molar yield and selectivity of 5-methylfurfural were calculated by gas chromatography analysis, and the effect of the catalyst on the yield and selectivity of 5-methylfurfural was further explored.
[0035] It can be seen from Table 1 that without adding catalyst and adding TT-Nb 2 O 5There is no effect on the conversion rate of 5-hydroxymethylfurfural, and no corresponding 5-methylfurfural is generated. The gas chromatogram is as follows: Figure 1 , 2 Shown; Ni-TT-Nb 2 O 5 Although the catalysts calcined at different temperatures can convert 5-hydroxymethylfurfural into 5-methylfurfural, the calcination temperature is 500℃, the 5-hydroxymethylfurfural conversion rate is the highest and the selectivity of 5-methylfurfural is the best. The gas chromatogram is as follows: Figure 3 shown.
[0036] Table 1 Effect of different catalysts on 5-methylfurfural yield
[0037]
[0038] Example 3: Effect of different reaction temperatures on 5-methylfurfural yield
[0039] The specific operation steps of the comparative experiment of different reaction temperatures are as follows:
[0040] Referring to Example 2, 0.05 g of Ni-TT-Nb 2 O 5 500 was used as a catalyst, and the reaction was carried out under different temperature conditions. The conversion rate of 5-hydroxymethylfurfural, the molar yield and selectivity of 5-methylfurfural were calculated by gas chromatography analysis, and the effect of the catalyst on the yield and selectivity of 5-methylfurfural was further explored.
[0041] As can be seen from Table 2, with the increase of reaction temperature, the conversion rate of 5-hydroxymethylfurfural gradually increases and finally reaches complete conversion; the yield and selectivity of 5-methylfurfural first increase and then decrease with the increase of reaction temperature. When the reaction temperature is 160°C, the yield (98%) and selectivity (98%) are the highest.
[0042] Table 2 Effect of different reaction temperatures on 5-methylfurfural yield
[0043]
[0044]
[0045] Example 4: Effect of different hydrogen pressures on 5-methylfurfural yield
[0046] The specific operation steps of the comparative experiment of different hydrogen pressures are as follows:
[0047] Referring to Example 3, the reaction was carried out under different hydrogen pressure atmosphere conditions and at 160° C. for 4 h at a stirring speed of 600 rpm. The conversion rate of 5-hydroxymethylfurfural, the molar yield and selectivity of 5-methylfurfural were calculated by gas chromatography analysis to further explore the effect of the catalyst on the yield and selectivity of 5-methylfurfural.
[0048] As can be seen from Table 3, with the increase of hydrogen pressure, the conversion rate of 5-hydroxymethylfurfural gradually increased and finally reached complete conversion; the yield of 5-methylfurfural increased with the increase of hydrogen pressure and reached the best at 2MPa, while the selectivity of 5-methylfurfural did not change with the change of hydrogen pressure.
[0049] Table 3 Effect of different hydrogen pressures on 5-methylfurfural yield
[0050]
[0051] Example 5: Effect of different stirring speeds on 5-methylfurfural yield
[0052] The specific operation steps of the comparative experiment of different stirring speeds are as follows:
[0053] Referring to Example 4, the hydrogen pressure was selected to be 2 MPa, and the reaction was carried out under different stirring speeds. The conversion rate of 5-hydroxymethylfurfural, the molar yield and selectivity of 5-methylfurfural were calculated by gas chromatography analysis, and the effect of the catalyst on the yield and selectivity of 5-methylfurfural was further explored.
[0054] As shown in Table 4, with the increase of stirring speed, the conversion rate of 5-hydroxymethylfurfural gradually increased and finally reached complete conversion; the yield and selectivity of 5-methylfurfural increased with the increase of stirring speed and reached the best at 600 rpm.
[0055] Table 4 Effect of different stirring speeds on 5-methylfurfural yield
[0056]
[0057] Example 6: Different Ni-TT-Nb 2 O 5 Effect of 500 dosage on the yield of 5-methylfurfural
[0058] The specific operation steps of the comparative experiment of different catalyst dosages are as follows:
[0059] Referring to Example 5, the stirring speed was selected to be 600 rpm, and the reaction was carried out under different Ni-TT-Nb 2 O 5The reaction was carried out under the condition of 500 dosage. The conversion rate of 5-hydroxymethylfurfural, the molar yield and selectivity of 5-methylfurfural were calculated by gas chromatography analysis, and the effect of catalyst on the yield and selectivity of 5-methylfurfural was further explored.
[0060] As shown in Table 5, the reaction 2 O 5 With the increase of the dosage of Ni-TT-Nb 2 O 5 500 showed an increasing trend with the increase of dosage, and reached the best under the condition of 0.05g; in addition, with the increase of Ni-TT-Nb 2 O 5 With the increase of 500% dosage, the selectivity of 5-methylfurfural remained unchanged.
[0061] Table 5 Different Ni-TT-Nb 2 O 5 Effect of 500 dosage on the yield of 5-methylfurfural
[0062]
[0063]
[0064] Example 7: Effect of different 5-hydroxymethylfurfural dosages on 5-methylfurfural yield
[0065] The specific operation steps of the comparative experiment of different 5-hydroxymethylfurfural dosages are as follows:
[0066] Referring to Example 4, Ni-TT-Nb 2 O 5 The dosage of 500 was 0.05 g, and the reaction was carried out under different 5-hydroxymethylfurfural dosage conditions. The conversion rate of 5-hydroxymethylfurfural, the molar yield and selectivity of 5-methylfurfural were calculated by gas chromatography analysis, and the effect of the catalyst on the yield and selectivity of 5-methylfurfural was further explored.
[0067] As shown in Table 6, the conversion rate of 5-hydroxymethylfurfural decreases with the increase of 5-hydroxymethylfurfural dosage; the yield of 5-methylfurfural decreases with the increase of 5-hydroxymethylfurfural dosage, but has no effect on the selectivity of 5-methylfurfural. In view of the conversion of the substrate, the yield of the product and the cost, the dosage of 5-hydroxymethylfurfural is selected as 0.126g. The results are as follows: Figure 4 shown.
[0068] Table 6 Effect of different 5-hydroxymethylfurfural dosage on 5-methylfurfural yield
[0069]
[0070] Through further optimization and screening of the examples, the reaction temperature was 160 °C, the reaction time was 4 h, and the pressure was 2 MPa. 2 and 600rpm, 0.05gNi-TT-Nb 2 O 5 The 500 catalyst can completely hydrogenate 0.126 g of 5-hydroxymethylfurfural to form 5-methylfurfural with a yield of up to 98%. Under the reaction conditions, the selectivity of generating 5-methylfurfural is 98%.
[0071] The specific embodiments of the present invention are only for illustrative purposes and do not limit the protection scope of the present invention in any way. Those skilled in the art may modify or change them according to the above description, and these improvements and changes should fall within the protection scope of the claims attached to the present invention.
Claims
1. A method for preparing 5-methylfurfural by selectively hydrogenating the C-OH structure of 5-hydroxymethylfurfural, characterized in that: The method comprises the following steps: adding 5-hydroxymethylfurfural, Ni-TT-Nb2O5 catalyst and tetrahydrofuran into a closed reactor, replacing air with hydrogen, and causing a catalytic reaction to generate 5-methylfurfural; The preparation method of the nickel / niobium pentoxide Ni-TT-Nb2O5 catalyst comprises the following steps: S1: First, urea is dissolved in a beaker containing a deionized water solution, and then Ni(NO3)2·6H2O is added to the mixed solution; then, a pseudo-hexagonal niobium pentoxide carrier is poured into the mixed solution and ultrasonicated, and finally, the beaker is placed in an oil bath at 90-100°C and stirred for 8-16 hours until the mixed solution is completely dry, and a light green solid powder is collected; In step S1, the mass ratio of Ni(NO3)2·6H2O and pseudo-hexagonal niobium pentoxide carrier is 1:20 to 1:5; S2 then calcined the solid powder in a tube furnace in a N2 / H2 atmosphere, and after the tube furnace cooled to room temperature, collected the black solid, which was the nickel / niobium pentoxide catalyst; In step S2, the solid powder is calcined in a tube furnace, specifically by heating to 500°C at 2-5°C / min in a N2 / H2 atmosphere, and keeping the temperature for 2 hours; wherein the N2 / H2 is 10%; Wherein, the preparation method of the pseudo-hexagonal niobium pentoxide TT-Nb2O5 carrier is as follows: a. Add ammonium niobium oxalate to a mixed solution containing deionized water and hydrogen peroxide, stir magnetically and pour the mixed solution into a polytetrafluoroethylene liner, and react at 160-190°C; b. After the reaction is completed, the reactor is cooled to room temperature, the product is collected, and repeatedly washed with deionized water and anhydrous ethanol; c. The niobium pentoxide precursor is then placed in a vacuum drying oven at 40-80°C and dried overnight; d. Then the dried niobium pentoxide precursor is placed in a muffle furnace and calcined to obtain a pseudo-hexagonal niobium pentoxide carrier at 350-400° C. for 2 h.
2. The preparation method according to claim 1, characterized in that In step S1 of the preparation of nickel / niobium pentoxide Ni-TT-Nb2O5 catalyst, the temperature in the oil bath is 95°C and the stirring time is 10-14h.
3. The preparation method according to claim 1, characterized in that: In step S1 of the preparation of nickel / niobium pentoxide Ni-TT-Nb2O5 catalyst, the stirring time in the oil bath is 12 h.
4. The preparation method according to claim 1, characterized in that: In the preparation of the pseudo-hexagonal niobium pentoxide carrier, the reaction temperature in step a is 170-180°C.
5. The preparation method according to claim 1, characterized in that: In the preparation of the pseudo-hexagonal niobium pentoxide carrier, the reaction temperature in step a is 175°C.
6. The preparation method according to claim 1, characterized in that: In the preparation of the pseudo-hexagonal niobium pentoxide carrier, in step c, the drying temperature is 50-70°C.
7. The preparation method according to claim 1, characterized in that: In the preparation of the pseudo-hexagonal niobium pentoxide carrier, in step c, the drying temperature is 60°C.
8. The preparation method according to claim 1, characterized in that: In the preparation of the pseudo-hexagonal niobium pentoxide carrier, in step d, the calcination temperature is 370-390.
9. The preparation method according to claim 1, characterized in that: In the preparation of the pseudo-hexagonal niobium pentoxide carrier, in step d, the calcination temperature is 380°C.
10. The preparation method according to claim 1, characterized in that: In step S1 of the preparation of the nickel / niobium pentoxide Ni-TT-Nb2O5 catalyst, the mass ratio of Ni(NO3)2·6H2O and the pseudo-hexagonal niobium pentoxide carrier is 1:
10.
11. The preparation method according to claim 1, characterized in that: In the preparation of pseudo-hexagonal niobium pentoxide TT-Nb2O5 carrier, In step a, the hydrogen peroxide is 30% by mass, the volumes of deionized water and hydrogen peroxide are 65 mL to 100 mL and 15 mL to 20 mL, respectively, and the volume ratio of the two is 4:1 to 5:1; the amount of ammonium niobium oxalate added is 5.2 g to 6.9 g, and the molar ratio of hydrogen peroxide to niobium is 10:1; In step b, the reaction is carried out at 175° C. for 12-18 hours; and washing is performed alternately with deionized water and ethanol for 3-8 times; In step c, the residual material is placed in a vacuum drying oven and dried for 12-24 hours; In step d, the specific operation of calcination is in a muffle furnace with a heating rate of 4-6°C / min.
12. The method according to claim 1, characterized in that The conditions of the catalytic reaction are: reaction temperature 100-160° C., hydrogen pressure 0.1-4 MPa, stirring speed 400-1000 rpm, and reaction time 1 h-8 h.
13. The method according to claim 1, characterized in that The conditions of the catalytic reaction are: reaction temperature of 100-160° C., hydrogen pressure of 1-2 MPa, stirring speed of 500-800 rpm, and reaction time of 3-6 h.
14. The method according to claim 1, wherein: The conditions of the catalytic reaction are: reaction temperature 160° C., hydrogen pressure 2 MPa, stirring speed 600 rpm, and reaction time 4 h.
15. The method according to claim 1, wherein: The ratio of the 5-hydroxymethylfurfural, Ni-TT-Nb2O5 catalyst and tetrahydrofuran is 0.06-0.25g:0.025-0.075:10mL.
16. The method according to claim 1, wherein: The ratio of the 5-hydroxymethylfurfural, Ni-TT-Nb2O5 catalyst and tetrahydrofuran is 0.126 g:0.05 g:10 mL.