Polyimide composite flakes and preparation method thereof
Through the preparation method of composite floss sheets of alternately laminated polyimide nanofibers and foam layers, the warmth and feel of polyimide fiber floss sheets are solved, efficient warmth and softness are achieved, and the process is simplified. process and reduce environmental impact.
Patent Information
- Application Number
- CN202310894410.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-20
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-07-20
AI Technical Summary
The existing polyimide fiber floss pieces have severe heat loss when there is wind or temperature difference, insufficient warmth, and have large fiber diameter, large rigidity, rough feel, poor softness and comfort. They are prepared by electrospinning technology. The nanofiber film has low thickness, poor compression and resilience, and is complex in process and harmful to the environment and the human body.
The composite flocculation preparation method of alternately laminated polyimide nanofiber layer and polyimide foam layer is used to form a composite nanofiber film through electrospinning and spraying, and then heated and foamed. , polyimide composite floccules with low density, high limit oxygen index, and good compression rate and recovery rate were obtained.
It realizes good warmth, compression and resilience of polyimide composite floss, overcomes the heat loss and rough feel of fiber floss, simplifies the process flow, reduces the dependence on environmental humidity, and improves the Industrialization prospects.
Smart Images

Figure CN117067732B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of thermal insulation materials, and in particular to a polyimide composite flake and a preparation method thereof. Background Art
[0002] Wadding refers to a sheet-like material with a fluffy structure made of plant fiber, animal fiber or chemical fiber for warmth, heat insulation or shockproof. It is the main auxiliary material of clothing and is usually soft in texture. Among many materials, polyimide is known as the organic polymer material with the highest comprehensive performance. It has the characteristics of high and low temperature resistance, flame retardancy, light weight, warmth retention, antibacterial, far infrared, etc. Its fiber is a good basic material for preparing wadding, so its fiber wadding products have broad application prospects. However, due to the large fiber diameter and large pore size between fibers, the convection in the wadding of polyimide fiber is more serious when there is wind and / or a large temperature difference between the inside and outside, resulting in heat loss, thereby reducing its warmth retention, so the warmth retention effect needs to be improved. In addition, due to the large rigidity of existing polyimide fibers and the coarse fiber diameter, the wadding produced has a rough feel and lacks softness and comfort.
[0003] Nanofibers have the characteristics of small diameter, high specific surface area, high porosity, good flexibility and three-dimensional grid-like porous structure. They can store a large amount of still air and have obvious application advantages in the field of warmth preservation. Electrospinning technology has become the main way to effectively prepare nanofiber materials due to its simple manufacturing equipment, low spinning cost, a wide variety of spinnable materials and controllable process. However, the nanofiber membranes prepared by the existing electrospinning process are usually of low thickness, poor compressibility and resilience, and poor thermal insulation performance, which greatly limits their application in actual cold protection and warmth preservation.
[0004] So far, there have been many research reports on improving the fluffiness of nanofiber membranes.
[0005] In one study, fiber flakes with both micron and nanometer sizes were obtained by electrospinning in a high humidity environment (humidity is usually greater than 80%). However, there is no effective bonding structure between the fibers, which leads to inter-fiber slippage and three-dimensional structural collapse of the material under stress, poor tensile properties and compression resilience, high dependence on environmental humidity, and the phenomenon of flying flakes during the preparation process.
[0006] In another study, a uniform water mist was applied to the receiving area of the electrospun fiber to obtain fluffy flakes, and then the flakes were placed in a vapor environment of an organic solvent for cross-linking treatment, so that the fiber surface was dissolved, and dissolution and fusion occurred at the fiber overlap to construct a bonding structure. Although this method gives the flakes compression resilience, the steam cross-linking time is long, the process is complicated, and the organic solvent vapor is difficult to recover and treat, which is harmful to the environment and human body, and is not conducive to large-scale production. At the same time, it is impossible to avoid the damage of the solvent vapor to the fiber as a whole.
[0007] In addition, polyimide foam is a porous material with gas as the filling phase and polyimide as the skeleton. It can store a lot of still air, has the characteristics of low thermal conductivity and low density, has good thermal insulation performance, and has good compressibility and resilience. However, polyimide foam has poor flexibility and feels hard when used directly as a filler, which cannot meet people's demand for soft and comfortable thermal insulation sheets.
[0008] Therefore, it is expected to develop a method for preparing a composite flake with simple process and rapid production of the composite flake having both the advantages of polyimide nanofibers and polyimide foams, so as to meet the application requirements in the field of human body cold protection and warmth preservation. Summary of the invention
[0009] Technical issues
[0010] The first object of the present invention is to provide a method for preparing a polyimide composite flake which has a simple process and can quickly obtain the composite flake with good warmth retention, compressibility and resilience.
[0011] The second object of the present invention is to provide a fluffy polyimide composite flake, which comprises alternately stacked polyimide nanofiber layers and polyimide foam layers and has good warmth retention, compressibility and resilience.
[0012] Technical Solution
[0013] According to a first aspect of the present invention, there is provided a method for preparing a polyimide composite flake, the method comprising the following steps:
[0014] (1) preparing polyamic acid spinning solution A;
[0015] (2) preparing a polyimide foam precursor solution B;
[0016] (3) electrospinning the polyamic acid spinning solution A to form a polyamic acid nanofiber layer, spraying the polyimide foam precursor solution B to form a polyimide foam precursor layer, and using a conductive receiving belt to alternately receive the polyamic acid nanofiber layer and the polyimide foam precursor layer to obtain a composite nanofiber membrane comprising the alternately stacked polyamic acid nanofiber layers and the polyimide foam precursor layers, wherein the two outermost layers of the composite nanofiber membrane are both set as polyamic acid nanofiber layers;
[0017] (4) drying the composite nanofiber membrane and then heating and foaming it to obtain a composite flake intermediate;
[0018] (5) The composite flake intermediate is subjected to thermal imidization treatment to obtain a polyimide composite flake.
[0019] In one embodiment, in step (1),
[0020] The preparation of the polyamic acid spinning solution A comprises: using a diamine monomer and a dianhydride monomer to prepare the polyamic acid spinning solution A,
[0021] The diamine monomer is one or more selected from diaminodiphenyl ether diamine (ODA), p-phenylenediamine (PPD), bisphenol A diamine (BAPP), 4,4-diaminodiphenyl sulfone (DDS), biphenyl diamine (Bz) and 4,4-diamino-2,2-dimethylbiphenyl (DMB),
[0022] The dianhydride monomer is one or more selected from biphenyl dianhydride (BPDA), terephthalic anhydride (PMDA), triphenyl diether dianhydride (HQPDA), diphenyl ether dianhydride (ODPA), benzophenone dianhydride (BTDA) and bisphenol A dianhydride (BPADA).
[0023] In one embodiment, in step (2), the preparation of the polyimide foam precursor solution B comprises:
[0024] The dianhydride monomer and the low molecular alcohol are first reacted under heating conditions to obtain a transparent solution containing an esterification product.
[0025] Then, diamine monomer is added for a second reaction to obtain a homogeneous solution.
[0026] Then the mixture is cooled to 10-30° C., and a foam stabilizer is added to obtain a polyimide foam precursor solution B.
[0027] In one embodiment, in step (2),
[0028] The dianhydride monomer is one or more selected from terephthalic anhydride (PMDA), benzophenone dianhydride (BTDA), diphenyl ether dianhydride (ODPA) and biphenyl dianhydride (BPDA);
[0029] The low molecular alcohol is one or more selected from methanol, ethanol, propanol, isopropanol and n-butanol.
[0030] The diamine monomer is one or more selected from diaminodiphenyl ether diamine (ODA), p-phenylenediamine (PPD), 4,4-diaminodiphenylmethane (MDA) and bisphenol A diamine (BAPP),
[0031] The foam stabilizer is one or more selected from polydimethylsiloxane copolyol water-soluble silicone oil, AK series silicone oil, polyethylene oxide nonionic surfactant and cationic fluorine-containing surfactant.
[0032] In one embodiment, in step (2),
[0033] Relative to 100 parts by weight of the dianhydride monomer, the amount of the low molecular alcohol is 50 to 1000 parts by weight, the amount of the foam stabilizer is 5 to 30 parts by weight, and
[0034] The ratio of the diamine monomer to the dianhydride monomer is an equimolar ratio.
[0035] In one embodiment, in step (2),
[0036] The heating allows the first reaction and the second reaction to proceed at 60 to 120°C.
[0037] In one embodiment, in step (3),
[0038] The spraying method is one selected from electrostatic spraying, air spraying and airless spraying;
[0039] The conductive receiving belt is one or more selected from a non-porous conductive metal belt, a conductive metal porous mesh belt and a fiber belt containing a conductive coating;
[0040] In the composite nanofiber membrane, the ratio of the total mass of all polyimide foam precursor layers to the total mass of all polyamic acid nanofiber layers is 10 to 50%.
[0041] In one embodiment, in step (4),
[0042] The drying temperature is 50 to 120° C. and the drying time is 0.3 to 2 hours; and
[0043] The heating and foaming temperature is 130-240° C., and the foaming time is 0.5-4 hours.
[0044] In one embodiment, in step (5),
[0045] The temperature of the thermal imidization treatment is 300-400°C.
[0046] According to a second aspect of the present invention, there is provided a polyimide composite flake prepared by the above method, wherein the polyimide composite flake comprises alternately stacked polyimide nanofiber layers and polyimide foam layers.
[0047] Wherein, the two outermost layers of the composite flakes are both polyimide nanofiber layers,
[0048] Wherein, the density of the polyimide composite flakes is less than 20 mg / cm 3 , limiting oxygen index is greater than 38%, compression rate is greater than 80%, and recovery rate is greater than 90%.
[0049] Beneficial Effects
[0050] Compared with the prior art, the present invention has the following advantages.
[0051] (1) The flake preparation method of the present invention is simple in process and is not highly dependent on environmental humidity. The present invention replaces the conventional process of preparing nanofiber flakes by electrospinning in a high humidity environment by steps (4) and (5). Therefore, a high humidity environment is not required in the entire process of the present invention.
[0052] (2) In step (3) of the method of the present invention, the present invention obtains a composite nanofiber membrane comprising alternately stacked nanofiber layers and foam precursor layers by alternately performing an electrospinning process of polyamic acid and a spraying process of a polyimide foam precursor, and using a common conductive receiving belt to alternately receive the polyamic acid nanofiber layer and the polyimide foam precursor layer.
[0053] Then, in step (4), drying is performed and a heating foaming reaction is performed to expand the volume of the foam precursor layer and increase the distance between the nanofiber layers to form a fluffy composite flake intermediate. In addition, a large number of polyimide foam layers with a partially closed-cell honeycomb structure are formed by the foam precursor layer, which is conducive to storing a large amount of static air, thereby significantly improving the thermal insulation performance.
[0054] Furthermore, in step (5), during the thermal imidization treatment, the polyimide foam can be shaped at the same time, thereby giving the composite flakes excellent compressibility and resilience.
[0055] The present invention combines a polyimide foam layer and a polyimide nanofiber layer to obtain a polyimide composite flake, which overcomes the problems of poor flexibility and easy powdering of the existing polyimide foam, while maintaining the excellent thermal insulation performance of the polyimide foam.
[0056] The two outermost layers of the composite batt may be provided as polyimide nanofiber layers, thereby providing comfortable softness.
[0057] (3) In the preparation method of the present invention, heating and foaming are directly carried out after spraying the polyimide foam precursor solution B (corresponding to steps (3) and (4)), without the need to crush the foam precursor into powder or other operations. The preparation process is simple, the process flow can be continuous, and continuous roll production is easy to achieve, which has good industrialization prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0058] The drawings of this specification show preferred embodiments of the present invention and are used together with the above-mentioned invention content to further illustrate the technical concept of the present invention, so the present invention should not be interpreted as being limited to the contents described in the drawings. At the same time, the shape, size, scale or ratio of the elements in the drawings may be exaggerated for a clearer description.
[0059] Figure 1 The figure is a schematic cross-sectional view of a partial structure of a polyimide composite flake according to one embodiment of the present invention.
[0060] Figure 2a This is a scanning electron microscope (SEM) image of the polyimide nanofiber layer of the polyimide composite flake in Example 1.
[0061] Figure 2b This is a SEM image of the polyimide foam layer of the polyimide composite flakes in Example 1.
[0062] Reference numerals
[0063] 10 Polyimide nanofiber layer
[0064] 20 Polyimide foam layer DETAILED DESCRIPTION
[0065] Hereinafter, the present invention will be described in detail with reference to the accompanying drawings. The terms or words used in this specification and claims should not be restrictively interpreted as common or dictionary definitions, and should be interpreted as meanings and concepts corresponding to the technical ideas of the present invention on the basis that the inventor can appropriately define the concepts of the terms to describe the principles of the invention in the best possible way.
[0066] When the conditions and methods for measuring a property or parameter described in this specification are not described in detail, the property or parameter is measured using the measurement conditions and methods generally used by those skilled in the art.
[0067] Unless otherwise specified, "%" used herein means % by weight.
[0068] Method for preparing polyimide composite flakes
[0069] According to a first aspect of the present invention, the present invention provides a method for preparing a polyimide composite flake, the method comprising the following steps:
[0070] (1) preparing polyamic acid spinning solution A;
[0071] (2) preparing a polyimide foam precursor solution B;
[0072] (3) electrospinning the polyamic acid spinning solution A to form a polyamic acid nanofiber layer, spraying the polyimide foam precursor solution B to form a polyimide foam precursor layer, and using a conductive receiving belt to alternately receive the polyamic acid nanofiber layer and the polyimide foam precursor layer to obtain a composite nanofiber membrane comprising the alternately stacked polyamic acid nanofiber layers and the polyimide foam precursor layers, wherein the two outermost layers of the composite nanofiber membrane are both set as polyamic acid nanofiber layers;
[0073] (4) drying the composite nanofiber membrane and then heating and foaming it to obtain a composite flake intermediate;
[0074] (5) The composite flake intermediate is subjected to thermal imidization treatment to obtain a polyimide composite flake.
[0075] In the following, each step will be described in detail.
[0076] Step (1) preparing polyamic acid spinning solution A
[0077] The polyamic acid spinning solution A can be prepared by conventional methods. For example, a diamine monomer and a dianhydride monomer can be polymerized in a polar solvent for a certain period of time to obtain the polyamic acid spinning solution A. Suitable diamine monomers and dianhydride monomers and reaction time can be determined according to conventional selection. The molar ratio of the diamine monomer to the dianhydride monomer can be 1:1.
[0078] The diamine monomer is a compound containing two amino groups and is a conventional component for preparing polyamic acid spinning solution. The diamine monomer can be one or more selected from diaminodiphenyl ether diamine (ODA), p-phenylenediamine (PPD), bisphenol A diamine (BAPP), 4,4-diaminodiphenyl sulfone (DDS), biphenyl diamine (Bz) and 4,4-diamino-2,2-dimethylbiphenyl (DMB).
[0079] The dianhydride monomer is a compound containing two carboxylic anhydride groups and is a conventional component for preparing polyamic acid spinning solution. The dianhydride monomer can be one or more selected from biphenyl dianhydride (BPDA), terephthalic anhydride (PMDA), triphenyl diether dianhydride (HQPDA), diphenyl ether dianhydride (ODPA), benzophenone dianhydride (BTDA) and bisphenol A dianhydride (BPADA).
[0080] The polar solvent may be one or more selected from N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAC), and N-methylpyrrolidone (NMP).
[0081] Relative to the total mass of the polyamic acid spinning solution A, the mass fraction of the polyamic acid (ie, the solid content) may be 5 to 50%, preferably 10 to 35%, and more preferably 12 to 25%.
[0082] The reaction time may be 5 to 24 hours, preferably 8 to 18 hours, more preferably 10 to 15 hours.
[0083] Step (2) Preparation of polyimide foam precursor solution B
[0084] The polyimide foam precursor solution B can be prepared by conventional methods, thereby preparing the polyimide foam precursor solution B. For example, the dianhydride monomer and the low molecular alcohol can be subjected to a first reaction under heating conditions, and the reaction time can be 0.5 to 3 hours to obtain a transparent solution containing an esterification product; then the diamine monomer is added for a second reaction, and the reaction time can be 0.5 to 3 hours to obtain a homogeneous solution containing a polyester ammonium salt; then the solution is cooled to 10 to 30° C., and a foam stabilizer is added to obtain the polyimide foam precursor solution B.
[0085] There is no particular limitation on the material types of the dianhydride monomer, low molecular alcohol, diamine monomer, and foam stabilizer, and they may be commonly used materials in the art.
[0086] For example, the dianhydride monomer may be one or more selected from terephthalic anhydride (PMDA), benzophenone dianhydride (BTDA), diphenyl ether dianhydride (ODPA), and biphenyl dianhydride (BPDA).
[0087] The low molecular alcohol may be one or more selected from methanol, ethanol, propanol, isopropanol and n-butanol.
[0088] The diamine monomer may be one or more selected from diaminodiphenyl ether diamine (ODA), p-phenylenediamine (PPD), 4,4-diaminodiphenylmethane (MDA), and bisphenol A type diamine (BAPP).
[0089] The foam stabilizer is used as an additive, usually a liquid, which can be miscible in the homogeneous solution. The foam stabilizer can be one or more selected from polydimethylsiloxane copolyol water-soluble silicone oil, AK series silicone oil, polyoxyethylene nonionic surfactant and cationic fluorine-containing surfactant. For example, the foam stabilizer can be one or more of DC-193, AK8805 and SF8427.
[0090] The weight ratios of the above raw material components may be as follows.
[0091] For example, relative to 100 parts by weight of the dianhydride monomer,
[0092] The amount of low molecular alcohol used can be 50 to 1000 parts by weight, preferably 100 to 800 parts by weight, more preferably 200 to 600 parts by weight;
[0093] The amount of the foam stabilizer may be 5 to 30 parts by weight, preferably 10 to 25 parts by weight, more preferably 15 to 20 parts by weight.
[0094] In addition, the ratio of the diamine monomer to the dianhydride monomer may be an equimolar ratio,
[0095] By heating, the temperature of the first reaction and the second reaction can be maintained at 60-120° C., preferably 70-110° C., and most preferably 85-100° C. If the temperature is too high, the production cost will increase; if the temperature is too low, the first reaction (esterification reaction) and the second reaction will not proceed sufficiently, affecting the performance of the subsequent polyimide foam, thereby affecting the performance of the polyimide composite flakes.
[0096] The time of the first reaction (esterification reaction) can be 0.5 to 3 hours, preferably 0.5 to 4 hours, and most preferably 1 to 2 hours. If the time of the first reaction is too short, the dianhydride monomer cannot fully react with the low molecular alcohol, making the subsequent polyimide foam easy to degrade, thereby affecting its flake performance; if the time of the first reaction is too long, the process efficiency will be reduced.
[0097] The time for the second reaction of the esterification product with the diamine monomer can be 0.5 to 3 hours, preferably 0.5 to 4 hours, and most preferably 1 to 2 hours. If the time of the second reaction is too short, the esterification product cannot fully react with the diamine monomer, and the amount of the generated polyester ammonium salt is insufficient, which affects the subsequent polyimide foam performance and thus the flake performance; if the time of the second reaction is too long, the process efficiency will be reduced.
[0098] The temperature after cooling can be 10-30° C., preferably 10-25° C., more preferably 10-20° C. If the temperature after cooling is too high, the foam stabilizer added subsequently is easily ineffective, affecting the stability of the foam cells, thereby affecting the product performance; if the temperature after cooling is too low, the solubility of the foam stabilizer added subsequently will be reduced, affecting the size and distribution uniformity of the foam cells, thereby affecting the product performance.
[0099] There is no particular limitation on the order in which steps (1) and (2) are performed. For example, step (1) may be performed first, and then step (2). Alternatively, step (2) may be performed first, and then step (1). Alternatively, steps (1) and (2) may be performed simultaneously.
[0100] Step (3) Preparation of composite nanofiber membrane
[0101] The polyamic acid spinning solution A is electrospun to form a polyamic acid nanofiber layer, and the polyimide foam precursor solution B is sprayed to form a polyimide foam precursor layer, and a conductive receiving belt is used to alternately receive the polyamic acid nanofiber layer and the polyimide foam precursor layer to obtain a composite nanofiber membrane comprising alternately stacked polyamic acid nanofiber layers and polyimide foam precursor layers, wherein the two outermost layers of the composite nanofiber membrane are both set as polyamic acid nanofiber layers.
[0102] Electrospinning is a simple and effective common technology for producing micron- to nanometer-scale fibers. It allows a polymer solution with static electricity to flow and deform in an electrostatic field, and solidify through solvent evaporation to form a fibrous substance.
[0103] Spraying refers to a coating method that uses a spray gun or a disc atomizer to disperse the solution into uniform and fine droplets with the help of pressure or centrifugal force and apply it to the surface of the object to be coated.
[0104] The spraying method can be one or more selected from electrostatic spraying, air spraying and airless spraying.
[0105] The airless spraying is also called high-pressure airless spraying, which refers to a spraying method that uses a high-pressure plunger pump to directly pressurize the paint to form a high-pressure paint, and sprays it out of the muzzle to form an atomized airflow to act on the surface of the object.
[0106] There is no particular limitation on the time, speed and material quality of each electrospinning and spraying, and they can be appropriately determined according to the specifications of the final composite flakes.
[0107] There is no particular limitation on the number of polyamic acid nanofiber layers and polyimide foam precursor layers. For example, the number of polyamic acid nanofiber layers may be 10 to 100, and the number of polyimide foam precursor layers is correspondingly one layer less than that of polyamic acid nanofiber layers.
[0108] In the composite nanofiber membrane, the ratio of the total mass of all polyimide foam precursor layers to the total mass of all polyamic acid nanofiber layers is 10 to 50%, preferably 15 to 40%, more preferably 20 to 30%.
[0109] If the spraying amount of the polyimide foam precursor solution B is too much, the volume of the foam precursor layer will expand too much in the subsequent heating and foaming reaction, affecting its flexibility, thereby affecting the softness and comfort of the final polyimide composite flakes.
[0110] If the spraying amount of polyimide foam precursor solution B is too small, then in the subsequent heating foaming reaction, the volume expansion force of the foam precursor layer will be too small to increase the distance between the nanofiber layers. At the same time, the number of local closed-cell honeycomb structures formed is small, which is not conducive to the storage of static air, thereby affecting the thermal insulation performance.
[0111] The conductive receiving belt can be one or more selected from a non-porous conductive metal belt, a conductive metal porous mesh belt and a fiber belt containing a conductive coating. The conductive receiving belt is used to receive the polyamic acid nanofiber layer obtained by electrostatic spinning and the polyimide foam precursor layer obtained by spraying. If a non-conductive receiving belt is used, the polyamic acid nanofiber layer obtained by electrostatic spinning cannot be received.
[0112] Step (4) Preparation of composite flake intermediate
[0113] The composite nanofiber membrane is dried and then heated for foaming to obtain a composite flake intermediate. The composite flake intermediate comprises alternately stacked polyamic acid nanofiber layers and polyimide foam layers. The polyimide foam layers are derived from the polyimide foam precursor layer.
[0114] The drying may be oven drying, which refers to a process of removing solvents and retaining solid components in a certain manner, usually a process of introducing hot air to evaporate and remove moisture from the material.
[0115] The drying temperature may be 50 to 120°C, preferably 55 to 110°C, and most preferably 60 to 100°C.
[0116] If the drying temperature is too low, the solvent in the polyimide foam precursor (polyester ammonium salt) is not completely removed, and too much residual solvent will make the pores of the polyimide foam obtained by foaming larger, affecting the strength of the foam and thus the strength of the final polyimide composite flakes.
[0117] If the drying temperature is too high, the polyimide foam precursor will foam prematurely without generating sufficient gas, resulting in an uneven cell structure during the subsequent foaming process, thereby affecting the performance of the final polyimide composite flakes.
[0118] The drying time may be 0.3 to 2 hours, preferably 0.4 to 1.5 hours, and most preferably 0.5 to 1 hour.
[0119] If the drying time is too short, there will be too much residual solvent in the polyimide foam precursor (polyester ammonium salt), which will make the pores of the polyimide foam obtained by foaming larger, affecting the strength of the foam and thus affecting the strength of the final polyimide composite flakes.
[0120] If the drying time is too long, the process efficiency will be reduced.
[0121] Heating foaming means that the polyimide foam precursor layer generates low molecular alcohol and water as foaming agents during the heating process, which form a large number of uniform bubble nuclei in the precursor layer, and the bubble nuclei become foam with a certain pore structure after expansion. By heating foaming, the polyimide foam precursor layer is transformed into a polyimide foam layer.
[0122] The temperature for heating and foaming may be 130 to 240°C, preferably 140 to 230°C, and most preferably 150 to 200°C.
[0123] If the foaming temperature is too low, the degree of foaming during the foaming process is small and insufficient gas is generated, resulting in the foam precursor layer having too small a volume expansion force to increase the distance between the nanofiber layers. At the same time, the polyimide foam obtained by foaming will have smaller pores, which is not conducive to the storage of static air, thereby affecting the thermal insulation performance.
[0124] If the foaming temperature is too high, the polyimide foam precursor will soften or melt, and the viscoelasticity will increase, which will surround the bubble nucleus, forming pores and retaining them in the polyimide foam precursor, affecting the structure of the foam and thus the performance of the final polyimide composite flakes.
[0125] The heating foaming time (i.e., the foaming time after reaching the foaming temperature at a certain heating rate, the heating rate is generally 5-15°C / min) can be 0.5-4 hours, preferably 1-3 hours, and most preferably 1-2 hours.
[0126] If the foaming time is too short, not enough gas will be generated during the foaming process to expand the volume of the foam precursor layer to increase the distance between the nanofiber layers. It will also cause the resulting polyimide foam to have smaller cells, which is not conducive to the storage of static air, thereby affecting the thermal insulation performance.
[0127] If the foaming time is too long, the process efficiency will be reduced.
[0128] By heating and foaming, a large number of uniform and fine bubble nuclei are first formed in the polyimide foam precursor, and then the bubble nuclei expand to form foam, and the distance between the nanofiber layers is increased, finally forming a composite flake intermediate with a fluffy structure, and at the same time forming a polyimide foam with a partially closed-cell honeycomb structure.
[0129] There is no particular limitation on the apparatus for performing drying and heating and foaming, and for example, an air-blast drying oven may be used.
[0130] Step (5) Preparation of polyimide composite flakes
[0131] The composite flake intermediate is subjected to thermal imidization treatment to obtain a polyimide composite flake. The polyimide composite flake comprises alternately stacked polyimide nanofiber layers and polyimide foam layers, wherein the polyimide nanofiber layers are derived from the polyamic acid nanofiber layers.
[0132] Thermal imidization refers to the process of dehydrating and cyclizing polyamic acid at high temperature to obtain polyimide, which is a conventional process for preparing polyimide. Through thermal imidization treatment, the polyamic acid nanofiber layer can be dehydrated and cyclized to obtain a polyimide nanofiber layer. In addition, during the thermal imidization treatment, the polyimide foam can be shaped at the same time, thereby giving the composite floccules excellent compressibility and resilience.
[0133] The temperature of thermal imidization may be 300 to 400°C.
[0134] If the temperature is too low, the imidization degree of the polyamic acid nanofibers will be incomplete, and the resulting polyimide nanofiber layer will be easily degraded, affecting the long-term performance of the final composite floccules.
[0135] If the temperature is too high, the polyimide will undergo thermal decomposition, and the foam therein will be prone to defects such as bubble collapse, thereby affecting the performance of the final composite flakes.
[0136] The time of thermal imidization (which refers to the treatment time in a thermal imidization apparatus such as a chain furnace) may be 0.2 to 3 hours, preferably 0.3 to 2 hours, and more preferably 0.5 to 1 hour.
[0137] If the time is too short, the imidization degree of the polyamic acid nanofibers will be incomplete, and the resulting polyimide nanofiber layer will be easily degraded; and the polyimide foam setting time will be too short, resulting in an unstable structure of the resulting polyimide foam layer, which will easily collapse, resulting in reduced performance of the final composite floccules.
[0138] If the time is too long, the polyimide will undergo thermal decomposition, and the foam will be prone to defects such as bubble collapse, reducing the quality of the final composite flakes.
[0139] Polyimide composite flakes
[0140] According to a second aspect of the present invention, there is provided a polyimide composite flake, comprising alternately stacked polyimide nanofiber layers and polyimide foam layers, wherein both outermost layers of the composite flake are polyimide nanofiber layers.
[0141] The polyimide composite flakes can be prepared by the above method of the present invention.
[0142] The density of polyimide composite flakes can be less than 20mg / cm 3 , preferably less than 15 mg / cm 3 , more preferably less than 10 mg / cm 3 ;
[0143] The limiting oxygen index may be greater than 38%, preferably greater than 39%, more preferably greater than 40%;
[0144] The compression rate may be greater than 80%, preferably greater than 85%, and more preferably greater than 90%;
[0145] The recovery rate may be greater than 90%, preferably greater than 92%, and more preferably greater than 95%.
[0146] There is no particular restriction on the thickness of the polyimide composite flakes. For example, when the composite flakes have a gram weight of 30 g / m 2 In the case of , the thickness can be greater than 5 mm and less than 30 mm.
[0147] The density of the composite flakes can be measured as follows:
[0148] First, the surface density was measured according to GB / T 24218.1-2009 (Test methods for textile nonwovens Part 1: Determination of mass per unit area);
[0149] Then, measure its thickness according to GB / T 24218.2-2009 (Textile nonwoven fabric test methods Part 2: Determination of thickness);
[0150] Next, the density is obtained by dividing the area density by the thickness.
[0151] The limiting oxygen index of the composite flakes can be measured according to GB / T 5454-1997 (Oxygen index method for textile burning performance test).
[0152] The compression rate and recovery rate of the composite flakes can be measured according to the test method in Appendix A of FZ / T 64003-2021 (Spray-bonded cotton flakes).
[0153] In one embodiment, the polyimide composite flakes have Figure 1 The partial structure shown, in which the polyimide foam layer 20 is sandwiched between two polyimide nanofiber layers 10.
[0154] Figure 1 Only three layers in the composite flakes are schematically shown. In practice, the composite flakes may include more layers, for example, 10 to 100 polyimide nanofiber layers 10 , and the number of polyimide foam layers 20 is correspondingly one layer less than the number of polyimide nanofiber layers 10 .
[0155] In addition, the thicknesses of the two polyimide nanofiber layers 10 may be the same as or different from each other; the thicknesses of the polyimide nanofiber layer 10 and the polyimide foam layer 20 may also be increased or decreased respectively.
[0156] Example
[0157] Hereinafter, the present invention will be described in detail with reference to embodiments to specifically describe the present invention. However, embodiments of the present invention may be modified into various other forms, and the scope of the present invention should not be construed as being limited to the embodiments described below. Embodiments of the present invention are provided to more fully describe the present invention to those of ordinary skill in the art.
[0158] The experimental methods in the following examples, unless otherwise specified, are generally conventional conditions in the art or conditions recommended by the manufacturer; the raw materials and equipment used are all commercially available from conventional markets, etc., unless otherwise specified.
[0159] The following is based on the same surface density (also known as gram weight, g / m 2 ) Obtain the products of Examples 1 to 6 and Comparative Examples 1 to 2, and compare their thermal insulation properties and other properties.
[0160] Example 1
[0161] The polyimide composite flakes are prepared by a method comprising the following steps.
[0162] Step (1): Prepare polyamic acid spinning solution A
[0163] 200.2 g (1 mol) of diphenyl ether diamine (ODA), 147.1 g (0.5 mol) of biphenyl dianhydride (BPDA), and 109.1 g (0.5 mol) of pyromellitic dianhydride (PMDA) were prepared at a molar ratio of 1:0.5:0.5, and 2586.3 g of N,N-dimethylacetamide (DMAC) as a solvent were prepared. They were stirred in a reactor for 12 hours to perform a polymerization reaction, and a polyamic acid spinning solution A having a solid content (i.e., polyamic acid content) of 15% by mass was obtained.
[0164] Step (2): Preparing polyimide foam precursor solution B
[0165] 109.1 g (0.5 mol) of pyromellitic dianhydride (PMDA) was added to 300 g of methanol, and then the temperature was raised to 85° C. and reacted for 2 h to obtain a solution containing an esterification product;
[0166] Then, 100.1 g (0.5 mol) of diphenyl ether diamine (ODA) was added, and the reaction was continued at 85° C. for 2 h to obtain a homogeneous polyimide foam precursor solution B;
[0167] The heating was stopped, the mixture was cooled to 25° C., and 18 g of polydimethylsiloxane copolyol water-soluble silicone oil as a foam stabilizer was added to obtain a polyimide foam precursor solution B containing a foam stabilizer.
[0168] Step (3): Preparation of composite nanofiber membrane
[0169] A device comprising electrospinning nozzles and electrostatic spraying nozzles arranged in sequence in a straight line (the two are arranged at intervals) is used, wherein the electrospinning nozzles are in three groups and the electrostatic spraying nozzles are in two groups.
[0170] The polyamic acid spinning solution A is electrospun in an electric field with an electric field strength of 25 kV / m, and the spinning amount of each group of electrospinning nozzles is 1 g / min.
[0171] The polyimide foam precursor solution B was electrostatically sprayed in an electric field with an electric field strength of 23 kV / m, and the spraying amount of each group of electrostatic spray nozzles was 0.3 g / min.
[0172] The polyamic acid nanofiber layer and the polyimide foam precursor layer are alternately formed on a conductive stainless steel belt that moves back and forth at a speed of 1 m / min. The time for each electrostatic spinning and electrostatic spraying is 2 minutes, and the total working time is 1 hour and 2 minutes. Thus, a composite nanofiber membrane with a length of 3 m, a width of 0.9 m, and a thickness of 400 μm is obtained. The two outermost layers of the composite nanofiber membrane are both set as polyamic acid nanofiber layers.
[0173] Step (4): Preparation of composite flake intermediate
[0174] The composite nanofiber membrane was heated to 80° C. in a forced air drying oven and dried for 1 hour.
[0175] Then, the mixture was heated to 150° C. at a heating rate of 10° C. / min for foaming for 1.5 hours to obtain a composite flake intermediate with a thickness of 7.8 mm.
[0176] Step (5): Preparation of polyimide composite flakes
[0177] The composite flake intermediate is sent into a 5m long chain furnace for thermal imidization treatment. The chain furnace has 5 temperature zones, the temperature from the inlet end to the outlet end is 100-370°C, and the moving speed of the composite flake intermediate is 0.1m / min.
[0178] The polyimide composite flakes are obtained by the thermal imidization treatment. The two outermost layers of the composite flakes are both polyimide nanofiber layers.
[0179] The surface density of the obtained polyimide composite flakes is 30g / m 2 , density is 5mg / cm 3 , thickness is 6mm.
[0180] Example 2 (Using different polyamic acid spinning solutions A and polyimide foam precursor solutions B to prepare polyimide composite flakes)
[0181] The polyimide composite flakes were prepared by the same method as in Example 1, except for the following steps.
[0182] Step (1): Prepare polyamic acid spinning solution A
[0183] 120.1 g (0.6 mol) of diphenyl ether diamine (ODA), 164.2 g (0.4 mol) of bisphenol A diamine (BAPP), and 294.2 g (1 mol) of biphenyl dianhydride (BPDA) were prepared at a molar ratio of 0.6:0.4:1, and 3278.2 g of N,N-dimethylacetamide (DMAC) as a solvent was also prepared. They were stirred in a reactor for 12 hours to perform a polymerization reaction, and a polyamic acid spinning solution A having a solid content (i.e., polyamic acid content) of 15% by mass was obtained.
[0184] Step (2): Preparing polyimide foam precursor solution B
[0185] 109.1 g (0.5 mol) of pyromellitic dianhydride (PMDA) was added to 300 g of methanol, and then the temperature was raised to 85° C. and reacted for 2 h to obtain a solution containing an esterification product;
[0186] Then, 99.1 g (0.5 mol) of 4,4-diaminodiphenylmethane (MDA) was added, and the reaction was continued at 85° C. for 2 h to obtain a homogeneous polyimide foam precursor solution B;
[0187] The heating was stopped, the mixture was cooled to 25° C., and 17 g of polydimethylsiloxane copolyol water-soluble silicone oil as a foam stabilizer was added to obtain a polyimide foam precursor solution B containing a foam stabilizer.
[0188] The surface density of the obtained polyimide composite flakes is 30g / m 2 , density is 6mg / cm 3 , thickness is 5mm.
[0189] Example 3 (Using different polyamic acid spinning solutions A and polyimide foam precursor solutions B to prepare polyimide composite flakes)
[0190] The polyimide composite flakes were prepared by the same method as in Example 1, except for the following steps.
[0191] Step (1): Prepare polyamic acid spinning solution A
[0192] 140.2 g (0.7 mol) of diphenyl ether diamine (ODA), 63.7 g (0.3 mol) of 4,4-diamino-2,2-dimethylbiphenyl (DMB), 147.1 g (0.5 mol) of biphenyl dianhydride (BPDA), 109.1 g (0.5 mol) of pyromellitic dianhydride (PMDA) were prepared at a molar ratio of 0.7:0.3:0.5:0.5, and 2607.2 g of N,N-dimethylacetamide (DMAC) as a solvent were prepared. They were stirred in a reactor for 12 hours to perform a polymerization reaction, and a polyamic acid spinning solution A having a solid content (i.e., polyamic acid content) of 15% by mass was obtained.
[0193] Step (2): Preparing polyimide foam precursor solution B
[0194] 161.1 g (0.5 mol) of benzophenone dianhydride (BTDA) was added to 400 g of methanol, and then the temperature was raised to 85° C. and reacted for 2 h to obtain a solution containing an esterification product;
[0195] Then, 99.1 g (0.5 mol) of 4,4-diaminodiphenylmethane (MDA) was added, and the reaction was continued at 85° C. for 2 h to obtain a homogeneous polyimide foam precursor solution B;
[0196] The heating was stopped, the mixture was cooled to 25° C., and 26 g of polydimethylsiloxane copolyol water-soluble silicone oil as a foam stabilizer was added to obtain a polyimide foam precursor solution B containing a foam stabilizer.
[0197] The surface density of the obtained polyimide composite flakes is 30g / m 2 , density is 6mg / cm 3 , thickness is 5mm.
[0198] Example 4 (Using different polyamic acid spinning solutions A and polyimide foam precursor solutions B to prepare polyimide composite flakes)
[0199] The polyimide composite flakes were prepared by the same method as in Example 1, except for the following steps.
[0200] Step (1): Prepare polyamic acid spinning solution A
[0201] 100.1 g (0.5 mol) of diphenyl ether diamine (ODA), 205.3 g (0.5 mol) of bisphenol A diamine (BAPP), 130.9 g (0.6 mol) of pyromellitic dianhydride (PMDA) and 117.7 g (0.4 mol) of biphenyl dianhydride (BPDA) were prepared in a molar ratio of 0.5:0.5:0.6:0.4, and 3139.3 g of N,N-dimethylacetamide (DMAC) as a solvent was prepared. They were stirred in a reactor for 12 hours to perform a polymerization reaction, and a polyamic acid spinning solution A having a solid content (i.e., polyamic acid content) of 15% by mass was obtained.
[0202] Step (2): Preparing polyimide foam precursor solution B
[0203] 161.1 g (0.5 mol) of benzophenone dianhydride (BTDA) was added to 420 g of isopropanol, and then the temperature was raised to 90° C. and reacted for 2 h to obtain a solution containing an esterification product;
[0204] Then, 100.1 g (0.5 mol) of diphenyl ether diamine (ODA) was added, and the reaction was continued at 85° C. for 2 h to obtain a homogeneous polyimide foam precursor solution B, and the heating was stopped and cooled to 25° C.;
[0205] 28 g of polydimethylsiloxane copolyol water-soluble silicone oil was added as a foam stabilizer to obtain a polyimide foam precursor solution B containing a foam stabilizer.
[0206] The surface density of the obtained polyimide composite flakes is 30g / m 2 , density is 6mg / cm 3 , thickness is 5mm.
[0207] Example 5 (Using different polyamic acid spinning solutions A and polyimide foam precursor solutions B to prepare polyimide composite flakes)
[0208] The polyimide composite flakes were prepared by the same method as in Example 1, except for the following steps.
[0209] Step (1): Prepare polyamic acid spinning solution A
[0210] 200.2 g (1 mol) of diphenyl ether diamine (ODA), 109.1 g (0.5 mol) of pyromellitic dianhydride (PMDA) and 201.2 g (0.5 mol) of triphenyl diether dianhydride (HQPDA) were prepared at a molar ratio of 1:0.5:0.5, and 2892.8 g of solvent N,N-dimethylacetamide (DMAC) was prepared. They were stirred in a reactor for 12 hours to perform a polymerization reaction, and a polyamic acid spinning solution A having a solid content (i.e., polyamic acid content) of 15% by mass was obtained.
[0211] Step (2): Preparing polyimide foam precursor solution B
[0212] 155.1 g (0.5 mol) of diphenyl ether dianhydride (ODPA) was added to 360 g of methanol, and then the temperature was raised to 85° C. and reacted for 2 h to obtain a solution containing an esterification product;
[0213] Then, 100.1 g (0.5 mol) of diphenyl ether diamine (ODA) was added, and the reaction was continued at 85° C. for 2 h to obtain a homogeneous polyimide foam precursor solution B;
[0214] The heating was stopped, the mixture was cooled to 25° C., and 29 g of polydimethylsiloxane copolyol water-soluble silicone oil as a foam stabilizer was added to obtain a polyimide foam precursor solution B containing a foam stabilizer.
[0215] The surface density of the obtained polyimide composite flakes is 30g / m 2 , density is 4mg / cm 3 , thickness is 7.5mm.
[0216] Example 6 (Using different polyamic acid spinning solutions A and polyimide foam precursor solutions B to prepare polyimide composite flakes)
[0217] The polyimide composite flakes were prepared by the same method as in Example 1, except for the following steps.
[0218] Step (1): Prepare polyamic acid spinning solution A
[0219] 120.1 g (0.6 mol) of diphenyl ether diamine (ODA), 164.2 g (0.4 mol) of bisphenol A diamine (BAPP), 152.7 g (0.7 mol) of pyromellitic dianhydride (PMDA) and 120.7 g (0.3 mol) of triphenyl diether dianhydride (HQPDA) were prepared in a molar ratio of 0.6:0.4:0.7:0.3, and 3160.3 g of N,N-dimethylacetamide (DMAC) as a solvent was prepared. They were stirred in a reactor for 12 hours to perform a polymerization reaction, and a polyamic acid spinning solution A having a solid content (i.e., polyamic acid content) of 15% by mass was obtained.
[0220] Step (2): Preparing polyimide foam precursor solution B
[0221] 155.1 g (0.5 mol) of diphenyl ether dianhydride (ODPA) and 109.1 g (0.5 mol) of pyromellitic dianhydride (PMDA) were added to 800 g of methanol, and then the temperature was raised to 85° C. and reacted for 2 h to obtain a solution containing an esterification product;
[0222] Then, 200.2 g (1 mol) of diphenyl ether diamine (ODA) was added, and the reaction was continued at 85° C. for 2 h to obtain a homogeneous polyimide foam precursor solution B;
[0223] The heating was stopped, the mixture was cooled to 25° C., and 55 g of polydimethylsiloxane copolyol water-soluble silicone oil as a foam stabilizer was added to obtain a polyimide foam precursor solution B containing a foam stabilizer.
[0224] The surface density of the obtained polyimide composite flakes is 30g / m 2 , density is 6mg / cm 3 , thickness is 5mm.
[0225] Comparative Example 1 (blank polyimide nanofiber membrane, no polyimide foam component)
[0226] Only step (1), the electrospinning process in step (3) and step (5) in Example 1 were performed to obtain a blank polyimide nanofiber membrane.
[0227] The surface density of the polyimide nanofiber membrane is 30 g / m 2 , density is 300mg / cm 3 , thickness is 0.1mm.
[0228] Comparative Example 2 (Preparation of Fluffy Polyimide Nanofiber Flakes by High Humidity Environment, Which Does Not Contain Polyimide Foam)
[0229] Step (1) of Example 1 was carried out to obtain a polyamic acid spinning solution A having a solid content (ie, polyamic acid content) of 15% by mass.
[0230] Then, the polyamic acid spinning solution A was electrospun in an electric field with a humidity of 80% and an electric field strength of 32 kV / m using an electrospinning device comprising three groups of spinning nozzles. The polyamic acid nanofibers formed by electrospinning were received by a negatively-voltaged roller, and the electrospinning time was 10 hours, to obtain a fluffy polyamic acid nanofiber membrane with a length of 0.8 m, a width of 0.5 m, and a thickness of 4 mm.
[0231] Then, the polyamic acid nanofiber membrane is subjected to step (5) of Example 1 (ie, thermal imidization treatment) to obtain polyimide nanofiber flakes.
[0232] The surface density of the polyimide nanofiber flakes is 30 g / m 2 , density is 10mg / cm 3 , thickness is 3mm.
[0233] Experimental Example 1: Using a scanning electron microscope to observe the morphology of the flakes
[0234] A scanning electron microscope (TESCAN, model VEGA3) was used to observe the microstructure of the polyimide composite flakes obtained in Example 1 according to GB / T36422-2018 (Scanning electron microscopy method for determination of micromorphology and diameter of chemical fibers). Figure 2a and 2b As shown. Among them,
[0235] Figure 2a This is the SEM image of the polyimide nanofiber layer.
[0236] Figure 2b This is the SEM image of the polyimide foam layer.
[0237] from Figure 2a It can be seen that the polyimide nanofiber layer in the composite flakes maintains the morphology of nanofibers and presents a three-dimensional network structure, which can store a large amount of still air.
[0238] from Figure 2b It can be seen that the polyimide foam layer in the composite flakes has a large number of honeycomb structures with partially closed cells, which is also conducive to the storage of static air and gives the composite flakes excellent compressibility and resilience.
[0239] Experimental Example 2 Measurement of thermal insulation performance
[0240] The thermal insulation performance of the products of Examples 1 to 6 and Comparative Examples 1 to 2 is compared. The thermal insulation performance of the product is expressed by the Crowe value, which is measured according to GB / T 11048-2008 (Determination of thermal and moisture resistance of textiles under steady-state conditions for physiological comfort).
[0241] Specifically, a fabric thermal insulation performance tester (Wenzhou Darong Textile Instrument Co., Ltd., model YG (B) 606E) was used to measure the Cros values of the products of Examples 1 to 6 and Comparative Examples 1 and 2 according to GB / T 11048-2018. The results are shown in Table 1 below.
[0242] Table 1: Cros values of products
[0243] <![CDATA[Clo value (unit: m 2 ·K / W)]]> Example 1 1.6 Example 2 1.45 Example 3 1.52 Example 4 1.41 Example 5 1.6 Example 6 1.53 Comparative Example 1 0.28 Comparative Example 2 0.85
[0244] As can be seen from Table 1, the polyimide composite flakes of Examples 1 to 6 prepared by the method of the present invention have significantly larger Crowe values, indicating that the warmth retention effect is excellent.
[0245] In particular, by comparing the Crowe values of the products of Example 1 and Comparative Examples 1-2, it can be seen that by including the polyimide foam component in the composite flakes, the warmth retention of the obtained flakes can be significantly improved.
[0246] Experimental Example 3 Measurement of Limiting Oxygen Index
[0247] According to GB / T 5454-1997 (Textile Combustion Performance Test - Oxygen Index Method), the limiting oxygen index of the products of Examples 1 to 6 and Comparative Examples 1 and 2 was measured. The results are shown in Table 2 below.
[0248] Table 2: Compression rate and recovery rate of products
[0249] Limiting oxygen index % Example 1 42 Example 2 40 Example 3 41 Example 4 42 Example 5 43 Example 6 41 Comparative Example 1 38 Comparative Example 2 38
[0250] It can be seen from Table 2 that the limiting oxygen index of the polyimide composite flakes of Examples 1 to 6 of the present invention is greater than 40%, and has a good flame retardant effect.
[0251] In contrast, the limiting oxygen index of the products of Comparative Examples 1 and 2 was lower than 40%, indicating that the flame retardant effect thereof was poor.
[0252] Experimental Example 4 Measurement of Compression Rate and Recovery Rate
[0253] The compression rate and recovery rate of the products of Examples 1 to 6 and Comparative Examples 1 and 2 were measured according to the test method of Appendix A of FZ / T 64003-2021 Spray-bonded Cotton Sheets. The results are shown in Table 3 below.
[0254] Table 3: Compression rate and recovery rate of products
[0255] Compression % Response rate % Example 1 83 92 Example 2 85 93 Example 3 84 92 Example 4 82 94 Example 5 86 91 Example 6 83 93 Comparative Example 1 9 7 Comparative Example 2 80 23
[0256] It can be seen from Table 3 that the polyimide composite flakes of Examples 1 to 6 of the present invention have high compression rates and recovery rates, and are suitable for the field of thermal insulation.
[0257] In comparison, the polyimide nanofiber membrane of Comparative Example 1 has significantly lower compression and recovery rates, poor fluffy structure, and is not suitable for the field of thermal insulation materials;
[0258] Although the compression rate of the polyimide nanofiber flakes of Comparative Example 2 is relatively high, the recovery rate is significantly low and is not suitable for the field of thermal insulation materials.
[0259] The above is a detailed introduction to the polyimide composite flakes and the preparation method thereof provided by the present invention. Specific embodiments are used herein to illustrate the principles and implementation methods of the present invention, and the description of the above embodiments is only used to help understand the method and core idea of the present invention. It should be pointed out that for ordinary technicians in this field, without departing from the principles of the present invention, the present invention can also be improved and modified in a number of ways, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.
Claims
1. A method for preparing a polyimide composite flake, the method comprising the following steps: (1) preparing polyamic acid spinning solution A; (2) preparing a polyimide foam precursor solution B; (3) electrospinning the polyamic acid spinning solution A to form a polyamic acid nanofiber layer, spraying the polyimide foam precursor solution B to form a polyimide foam precursor layer, and using a conductive receiving belt to alternately receive the polyamic acid nanofiber layer and the polyimide foam precursor layer to obtain a composite nanofiber membrane comprising the alternately stacked polyamic acid nanofiber layers and the polyimide foam precursor layers, wherein the two outermost layers of the composite nanofiber membrane are both set as polyamic acid nanofiber layers; (4) drying the composite nanofiber membrane and then heating and foaming it to obtain a composite flake intermediate, wherein the polyimide foam precursor layer is transformed into a polyimide foam layer; (5) The composite flake intermediate is subjected to thermal imidization treatment to obtain a polyimide composite flake, wherein the polyamic acid nanofiber layer is converted into a polyimide nanofiber layer.
2. The method according to claim 1, wherein: In step (1), The preparation of the polyamic acid spinning solution A comprises: using a diamine monomer and a dianhydride monomer to prepare the polyamic acid spinning solution A, The diamine monomer is one or more selected from diaminodiphenyl ether diamine (ODA), p-phenylenediamine (PPD), bisphenol A diamine (BAPP), 4,4-diaminodiphenyl sulfone (DDS), biphenyl diamine (Bz) and 4,4-diamino-2,2-dimethylbiphenyl (DMB), The dianhydride monomer is one or more selected from biphenyl dianhydride (BPDA), terephthalic anhydride (PMDA), triphenyl diether dianhydride (HQPDA), diphenyl ether dianhydride (ODPA), benzophenone dianhydride (BTDA) and bisphenol A dianhydride (BPADA).
3. The method according to claim 1, wherein: In step (2), the preparation of the polyimide foam precursor solution B comprises: The dianhydride monomer and the low molecular alcohol are first reacted under heating conditions to obtain a transparent solution containing an esterification product. Then, diamine monomer is added for a second reaction to obtain a homogeneous solution. Then the mixture is cooled to 10-30° C., and a foam stabilizer is added to obtain a polyimide foam precursor solution B.
4. The method according to claim 3, wherein: In step (2), The dianhydride monomer is one or more selected from terephthalic anhydride (PMDA), benzophenone dianhydride (BTDA), diphenyl ether dianhydride (ODPA) and biphenyl dianhydride (BPDA); The low molecular alcohol is one or more selected from methanol, ethanol, propanol, isopropanol and n-butanol. The diamine monomer is one or more selected from diaminodiphenyl ether diamine (ODA), p-phenylenediamine (PPD), 4,4-diaminodiphenylmethane (MDA) and bisphenol A diamine (BAPP), The foam stabilizer is one or more selected from polydimethylsiloxane copolyol water-soluble silicone oil, AK series silicone oil, polyethylene oxide nonionic surfactant and cationic fluorine-containing surfactant.
5. The method according to claim 3, wherein: In step (2), Relative to 100 parts by weight of the dianhydride monomer, the amount of the low molecular alcohol is 50 to 1000 parts by weight, the amount of the foam stabilizer is 5 to 30 parts by weight, and The ratio of the diamine monomer to the dianhydride monomer is an equimolar ratio.
6. The method according to claim 3, wherein: In step (2), The heating allows the first reaction and the second reaction to proceed at 60 to 120°C.
7. The method according to claim 1, wherein: In step (3), The spraying method is one or more selected from electrostatic spraying, air spraying and airless spraying; The conductive receiving belt is one or more selected from a non-porous conductive metal belt, a conductive metal porous mesh belt and a fiber belt containing a conductive coating; In the composite nanofiber membrane, the ratio of the total mass of all polyimide foam precursor layers to the total mass of all polyamic acid nanofiber layers is 10 to 50%.
8. The method according to claim 1, wherein: In step (4), The drying temperature is 50 to 120° C. and the drying time is 0.3 to 2 hours; and The heating and foaming temperature is 130-240° C., and the foaming time is 0.5-4 hours.
9. The method according to claim 1, wherein: In step (5), The temperature of the thermal imidization treatment is 300-400°C.
10. A polyimide composite flake prepared by the method according to claim 1, wherein the polyimide composite flake comprises alternately stacked polyimide nanofiber layers and polyimide foam layers. in, The two outermost layers of the composite flakes are both polyimide nanofiber layers, Wherein, the density of the polyimide composite flakes is less than 20 mg / cm 3 , limiting oxygen index is greater than 38%, compression rate is greater than 80%, and recovery rate is greater than 90%.
Citation Information
Patent Citations
Polyimide nano fiber composite film, and preparation method and application thereof
CN103747609A
Composite nanofiber membrane and preparation method and application thereof
CN107299456A
Porous layer coated polyimide fibrous membrane and preparation method thereof
CN110592952A
Nanofiber flocculus with sandwich structure and preparation method of nanofiber flocculus
CN111485329A
Electrostatically spun fiber flocculus and preparation method thereof
CN112981718A