Non-oriented electromagnetic steel sheet and method for producing the same
By controlling the content of Si, sol.Al and Mn and optimizing the cold rolling process, the contradiction between high strength and low iron loss in non-oriented electromagnetic steel sheets has been resolved, resulting in non-oriented electromagnetic steel sheets with high strength and excellent magnetic properties, suitable for motor core materials.
Patent Information
- Application Number
- CN202280026522.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-04-02
- Filing Date
- 2022-03-31
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-03-31
Smart Images

Figure BDA0004476524310000191 
Figure BDA0004476524310000201 
Figure HDA0004476524320000011
Abstract
Description
Technical Field
[0001] The invention relates to a non-oriented electromagnetic steel sheet and a method for manufacturing the same.
[0002] This application claims priority based on Japanese Patent Application No. 2021-063642 filed in Japan on April 2, 2021, and the contents are incorporated herein by reference. Background Art
[0003] In recent years, global environmental issues have attracted much attention, and the demand for energy conservation has further increased. Among the demands for energy conservation, there is also a strong demand for high efficiency of electrical equipment. Therefore, in non-oriented electromagnetic steel sheets, which are widely used as core materials for motors and generators, the demand for improved magnetic properties has also been further strengthened. This trend is more significant in drive motors for electric vehicles and hybrid vehicles, and motors for compressors in air conditioners.
[0004] The motor core of the various motors described above is composed of a stator as a fixed part and a rotor as a rotating part. The properties required of the stator and the rotor constituting the motor core are different from each other. For the stator, excellent magnetic properties (low iron loss and high magnetic flux density) are required, and low iron loss is particularly required. On the other hand, for the rotor, excellent mechanical properties (high strength) are required, which are not as good as the stator, but low iron loss is required.
[0005] Since the properties required in the stator and the rotor are different, the desired properties can be achieved by manufacturing the non-oriented electromagnetic steel sheets for the stator and the non-oriented electromagnetic steel sheets for the rotor separately. However, preparing two types of non-oriented electromagnetic steel sheets will cause a decrease in the yield. Therefore, in order to achieve the high strength required for the rotor and the low iron loss required for the stator, a non-oriented electromagnetic steel sheet with excellent strength and excellent magnetic properties has been continuously studied so far.
[0006] For example, Patent Documents 1 to 3 attempt to achieve high strength and excellent magnetic properties.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: International Publication No. 2019 / 017426
[0010] Patent Document 2: International Publication No. 2020 / 091039
[0011] Patent Document 3: International Publication No. 2020 / 153387
[0012] Patent Document 4: Japanese Patent Application Publication No. 2013-91837
[0013] Patent Document 5: Japanese Patent Application Publication No. 2002-14691 Summary of the invention
[0014] Technical problem to be solved by the invention
[0015] However, in order to realize a nonoriented electrical steel sheet having both high strength and low iron loss, it is necessary to contain a large amount of alloy elements as disclosed in Patent Documents 1 to 3, which causes a problem that toughness is reduced and fracture is easily caused during cold rolling.
[0016] The present invention has been made to solve the above-mentioned problems, and an object of the present invention is to stably provide a non-oriented electrical steel sheet having high strength and excellent magnetic properties.
[0017] Technical means for solving technical problems
[0018] The present invention is mainly based on the following non-oriented electrical steel sheet and a method for producing the same.
[0019] (1) The chemical composition of the base material of the non-oriented electrical steel sheet according to one embodiment of the present invention is, in terms of mass %,
[0020] C: 0~0.0050%,
[0021] Si: 3.7-4.8%,
[0022] Mn: 0.05% or more, less than 0.50%,
[0023] sol.Al: 0.05~0.45%,
[0024] P: 0~0.030%,
[0025] S: 0~0.0030%,
[0026] N: 0~0.0040%,
[0027] Ti: 0% or more, less than 0.0050%,
[0028] Nb: 0% or more, less than 0.0050%,
[0029] Zr: 0% or more, less than 0.0050%,
[0030] V: 0% or more, less than 0.0050%,
[0031] Cu: 0% or more, less than 0.200%,
[0032] Ni: 0% or more, less than 0.500%,
[0033] Sn: 0~0.100%,
[0034] Sb: 0 to 0.100%, and
[0035] The rest: Fe and impurities;
[0036] The recrystallization rate is less than 100% in terms of area ratio;
[0037] Satisfy the following formulas (i) and (ii);
[0038] The tensile strength exceeds 700MPa.
[0039] 4.3≤Si+sol.Al+0.5×Mn≤4.9···(i)
[0040] However, the element symbols in the above formulas are the content (mass %) of each element.
[0041] (B 50 (0°)+2×B 50 (45°)+B 50 (90°)) / 4≥1.57···(ii)
[0042] Among them, B in the above formula (ii) 50 (0°) is the magnetic flux density (T) under the magnetizing force of 5000A / m in the rolling direction, B 50 (45°) is the magnetic flux density (T) at a magnetizing force of 5000 A / m at a direction 45° from the rolling direction, B 50 (90°) is the magnetic flux density (T) at a magnetizing force of 5000 A / m in a direction 90° from the rolling direction.
[0043] (2) The chemical composition of the non-oriented electromagnetic steel sheet described in (1) above may include, in mass %,
[0044] Sn: 0.005 to 0.100%, and
[0045] Sb: 0.005~0.100%
[0046] Choose 1 or 2 from the following.
[0047] (3) The nonoriented electrical steel sheet as described in (1) or (2) above may include an insulating film on the surface of the base material.
[0048] (4) A method for producing a non-oriented electrical steel sheet according to another embodiment of the present invention is a method for producing a non-oriented electrical steel sheet as described in any one of (1) to (3) above, and
[0049] In terms of mass %,
[0050] C: 0~0.0050%,
[0051] Si: 3.7-4.8%,
[0052] Mn: 0.05% or more, less than 0.50%,
[0053] sol.Al: 0.05~0.45%,
[0054] P: 0~0.030%,
[0055] S: 0~0.0030%,
[0056] N: 0~0.0040%,
[0057] Ti: 0% or more, less than 0.0050%,
[0058] Nb: 0% or more, less than 0.0050%,
[0059] Zr: 0% or more, less than 0.0050%,
[0060] V: 0% or more, less than 0.0050%,
[0061] Cu: 0% or more, less than 0.200%,
[0062] Ni: 0% or more, less than 0.500%,
[0063] Sn: 0~0.100%,
[0064] Sb: 0 to 0.100%, and
[0065] The rest: Fe and impurities, and
[0066] A steel block having a chemical composition satisfying the following formula (i) is implemented in sequence:
[0067] Hot rolling process,
[0068] The first cold rolling process reduces the plate thickness to less than 1.0 mm.
[0069] Intermediate annealing process,
[0070] Secondary cold rolling process, and
[0071] The final annealing process has a soaking temperature of 700 to 800° C. and a soaking time of 1 to 300 seconds.
[0072] 4.3≤Si+sol.Al+0.5×Mn≤4.9···(i)
[0073] The element symbols in the above formula are the content (mass %) of each element.
[0074] Effects of the Invention
[0075] According to the above-described embodiment of the present invention, a non-oriented electrical steel sheet having high strength and excellent magnetic properties can be stably obtained. BRIEF DESCRIPTION OF THE DRAWINGS
[0076] Figure 1A This is a cross-sectional view of a non-oriented electrical steel sheet for explaining a method of calculating a recrystallization rate.
[0077] Figure 1B This is a cross-sectional view of a non-oriented electrical steel sheet for explaining a method of calculating a recrystallization rate. DETAILED DESCRIPTION
[0078] The present inventors have conducted intensive studies to solve the above-mentioned problems and have obtained the following findings.
[0079] Si, Mn and Sol.Al are elements that increase the electrical resistance of steel and reduce eddy current loss. In addition, these elements are elements that also contribute to the high strength of steel.
[0080] Among Si, Mn and sol.Al, Si is also the element that contributes most effectively to the increase of resistance and strength. Sol.Al is second only to Si in terms of the effect of increasing resistance and strength. On the other hand, Mn is slightly less effective in increasing resistance and strength than Si and sol.Al.
[0081] Therefore, in this embodiment, by adjusting the contents of Si, Sol.Al and Mn within appropriate ranges, high strength and improved magnetic properties are achieved.
[0082] Next, the improvement in toughness during cold rolling of the steel sheet containing a large amount of Si, Sol.Al, and Mn was studied.
[0083] In the past, in order to seek high strength of steel, when a large amount of alloying elements such as Si, Sol.Al and Mn are contained in the steel, there is a problem that the toughness is reduced, and as a result, the steel is prone to fracture during cold rolling. Therefore, the inventors have conducted a concentrated study on improving the toughness of steel plates (high alloy steels) containing a large amount of alloying elements during cold rolling, and found that by omitting the annealing of the hot-rolled plate, even for high-alloy steel, fracture during cold rolling can be suppressed. Specifically, it is understood that for hot-rolled plates that are not annealed, after pickling, the plate thickness is cold-rolled once to less than 1 mm, intermediate annealing is performed, and then secondary cold rolling is performed, thereby ensuring the toughness during secondary cold rolling even for high-alloy steel.
[0084] The secondary cold rolling method has been studied so far. For example, Patent Documents 4 and 5 attempt to achieve excellent magnetic properties and high strength.
[0085] However, in the method disclosed in Patent Document 4, the crystal grain size is relatively coarse, so the high strength required by the present embodiment cannot be obtained. In addition, in the method disclosed in Patent Document 5, the contents of Si, Mn and Al are low, so from the perspective of high strength, it is not satisfactory.
[0086] Therefore, the present inventors have further conducted repeated studies and found that in order to realize a non-oriented electrical steel sheet having excellent toughness during cold rolling, high strength and good magnetic properties, it is important to adjust the contents of Si, Sol.Al and Mn within appropriate ranges, appropriately control the sheet thickness at the start of secondary cold rolling, and further appropriately control the metal structure after final annealing.
[0087] The present invention is completed based on the above-mentioned knowledge. The preferred embodiments of the present invention are described in detail below. However, the present invention is not limited to the configuration disclosed in this embodiment, and various changes can be made within the scope of the present invention.
[0088] 1. Overall composition
[0089] The non-oriented electromagnetic steel sheet of the present embodiment has high strength and excellent magnetic properties, and is therefore preferred for both the stator and the rotor. In the manufacture of the non-oriented electromagnetic steel sheet of the present embodiment, the toughness during cold rolling is excellent, and fracture during rolling can be suppressed, so stable manufacture is possible. In addition, it is preferred that the non-oriented electromagnetic steel sheet of the present embodiment has an insulating film on the surface of the base material (silicon steel sheet) described below.
[0090] 2. Chemical composition of the base material
[0091] In the chemical composition of the base material of the non-oriented electromagnetic steel sheet of the present embodiment, the reasons for limiting each element are as follows. In addition, in the following description, "%" for the content means "mass %". For the numerical limit range recorded between "-", the lower limit and the upper limit are included in the range.
[0092] C: 0~0.0050%
[0093] C (carbon) is an element that causes the iron loss of the non-oriented electromagnetic steel sheet to deteriorate. When the C content exceeds 0.0050%, the iron loss of the non-oriented electromagnetic steel sheet will deteriorate and good magnetic properties cannot be obtained. Therefore, the C content is set to 0.0050% or less. Preferably, the C content is 0.0040% or less, more preferably, 0.0035% or less, and further preferably, 0.0030% or less. The C content can also be 0%. However, since it is difficult to make the C content 0% in practical steel sheets in terms of manufacturing, the C content can also be set to more than 0%. In addition, since C contributes to the high strength of the non-oriented electromagnetic steel sheet, when this effect is to be obtained, it is preferred that the C content is 0.0005% or more, and more preferably, 0.0010% or more.
[0094] Si: 3.7-4.8%
[0095] Si (silicon) is an element that increases the electrical resistance of steel, thereby reducing eddy current loss and improving high-frequency iron loss of non-oriented electromagnetic steel sheets. In addition, Si is an element with a large solid solution strengthening ability, and is therefore also effective in increasing the strength of non-oriented electromagnetic steel sheets. In order to obtain these effects, the Si content is set to 3.7% or more. Preferably, the Si content is 3.8% or more, more preferably 3.9% or more, and further preferably 4.0% or more. On the other hand, when the Si content is excessive, the workability will deteriorate significantly and cold rolling will be difficult. Therefore, the Si content is set to less than 4.8%. Preferably, the Si content is less than 4.7%, and more preferably less than 4.6%.
[0096] Mn: 0.05% or more, less than 0.50%
[0097] Mn (manganese) is an element effective in increasing the resistance of steel and reducing eddy current loss, and improving the high-frequency iron loss of non-oriented electromagnetic steel sheets. In addition, when the Mn content is too low, the effect of increasing the resistance is small, and fine sulfides (MnS) will precipitate into the steel, thereby deteriorating the iron loss. Therefore, the Mn content is set to 0.05% or more. Regarding the Mn content, it is preferably 0.10% or more, and more preferably 0.15% or more. On the other hand, when the Mn content is excessive, the reduction in the magnetic flux density of the non-oriented electromagnetic steel sheet becomes significant. Therefore, the Mn content is set to less than 0.50%. It is preferred that the Mn content is 0.40% or less, and more preferably 0.30% or less.
[0098] sol.Al: 0.05~0.45%
[0099] Sol.Al (aluminum) is an element that has the effect of reducing eddy current loss by increasing the resistance of steel and improving the high-frequency iron loss of the non-oriented electromagnetic steel sheet. In addition, although Sol.Al is not as good as Si, it is also an element that contributes to the high strength of the non-oriented electromagnetic steel sheet through solid solution strengthening. In order to obtain these effects, the Sol.Al content is set to 0.05% or more. Preferably, the Sol.Al content is 0.10% or more, and more preferably, it is 0.15% or more. On the other hand, when the Sol.Al content is excessive, the toughness will deteriorate and the risk of fracture during cold rolling will increase. Therefore, the Sol.Al content is set to 0.45% or less. Preferably, the Sol.Al content is 0.40% or less, and more preferably, it is 0.35% or less.
[0100] In addition, in the present embodiment, the so-called sol.Al means acid-soluble Al, and refers to solid solution Al existing in the steel in a solid solution state.
[0101] In the present embodiment, the electrical resistance of the steel is ensured by appropriately controlling the contents of Si, sol.Al and Mn. In addition, from the viewpoint of ensuring strength, it is also necessary to appropriately control the contents of Si, sol.Al and Mn. On the other hand, from the viewpoint of ensuring magnetic flux density and toughness, an upper limit of the total content of Si, sol.Al and Mn is also required. Therefore, in addition to the contents of Si, sol.Al and Mn being within the above-mentioned ranges, the following formula (i) must also be satisfied. Regarding the middle value of the following formula (i), from the viewpoint of ensuring the electrical resistance and strength of the steel, it is preferably 4.4 or more, and more preferably 4.5 or more. On the other hand, regarding the middle value of the following formula (i), from the viewpoint of ensuring the magnetic flux density and toughness of the steel, it is preferably 4.8 or less, and more preferably 4.7 or less.
[0102] 4.3≤Si+sol.Al+0.5×Mn≤4.9···(i)
[0103] The element symbols in the above formula are the content (mass %) of each element.
[0104] P: 0~0.030%
[0105] P (phosphorus) is contained in steel as an impurity. When its content is excessive, the toughness of the non-oriented electromagnetic steel sheet will be significantly reduced. Therefore, the P content is set to 0.030% or less. Regarding the P content, it is preferably 0.025% or less, and more preferably 0.020% or less. The P content can also be 0%. In addition, an extreme reduction in the P content sometimes causes an increase in manufacturing costs, so regarding the P content, it is preferably 0.003% or more, and more preferably 0.005% or more.
[0106] S: 0~0.0030%
[0107] S (sulfur) is an element that increases iron loss by forming fine precipitates of MnS and deteriorates the magnetic properties of the non-oriented electrical steel sheet. Therefore, the S content is set to 0.0030% or less. The S content is preferably 0.0020% or less, more preferably 0.0018% or less, and further preferably 0.0015% or less. The S content may also be 0%. In addition, an extreme reduction in the S content may sometimes cause an increase in manufacturing costs, so the S content is preferably 0.0001% or more, more preferably 0.0003% or more, and further preferably 0.0005% or more.
[0108] N: 0~0.0040%
[0109] N (nitrogen) is an element that is inevitably mixed into steel, and is an element that forms nitrides to increase iron loss and deteriorate the magnetic properties of non-oriented electrical steel sheets. Therefore, the N content is set to 0.0040% or less. The N content is preferably 0.0030% or less, and more preferably 0.0020% or less. The N content may also be 0%. In addition, an extreme reduction in the N content may sometimes lead to an increase in manufacturing costs, so it is preferred that the N content is 0.0005% or more.
[0110] Ti: 0% or more, less than 0.0050%
[0111] Ti (titanium) is an element that is inevitably mixed into steel, and can be combined with carbon or nitrogen to form precipitates (carbides, nitrides). When carbides or nitrides are formed, these precipitates themselves deteriorate the magnetic properties of the non-oriented electromagnetic steel sheet. Furthermore, the growth of grains in the final annealing is hindered by carbides or nitrides, which deteriorates the magnetic properties of the non-oriented electromagnetic steel sheet. Therefore, the Ti content is set to less than 0.0050%. Regarding the Ti content, it is preferably 0.0040% or less, more preferably 0.0030% or less, and further preferably 0.0020% or less. The Ti content may also be 0%. In addition, an extreme reduction in the Ti content may sometimes lead to an increase in manufacturing costs, so it is preferred that the Ti content is 0.0005% or more.
[0112] Nb: 0% or more, less than 0.0050%
[0113] Nb (niobium) is an element that contributes to high strength by forming precipitates (carbides, nitrides) by combining with carbon or nitrogen, but these precipitates themselves deteriorate the magnetic properties of the non-oriented electrical steel sheet. Therefore, the Nb content is set to less than 0.0050%. The Nb content is preferably 0.0040% or less, more preferably 0.0030% or less, and further preferably 0.0020% or less. In addition, the Nb content is further preferably below the measurement limit, and specifically, it is further preferably less than 0.0001%. Since the lower the Nb content, the better, the Nb content can also be set to 0%.
[0114] Zr: 0% or more, less than 0.0050%
[0115] Zr (zirconium) is an element that contributes to high strength by forming precipitates (carbides, nitrides) by combining with carbon or nitrogen, but these precipitates themselves deteriorate the magnetic properties of the non-oriented electrical steel sheet. Therefore, the Zr content is set to less than 0.0050%. The Zr content is preferably 0.0040% or less, more preferably 0.0030% or less, and further preferably 0.0020% or less. In addition, the Zr content is further preferably below the measurement limit, and specifically, it is further preferably 0.0001% or less. Since the lower the Zr content, the better, the Zr content can also be set to 0%.
[0116] V: 0% or more, less than 0.0050%
[0117] V (vanadium) is an element that contributes to high strength by forming precipitates (carbides, nitrides) by combining with carbon or nitrogen, but these precipitates themselves deteriorate the magnetic properties of the non-oriented electrical steel sheet. Therefore, the V content is set to less than 0.0050%. Regarding the V content, it is preferably 0.0040% or less, more preferably 0.0030% or less, and further preferably 0.0020% or less. Regarding the V content, it is further preferred to be below the measurement limit, and specifically, it is further preferred to be 0.0001% or less. Since the lower the V content, the better, the V content can also be set to 0%.
[0118] Cu: 0% or more, less than 0.200%
[0119] Cu (copper) is an element that is inevitably mixed into steel. When Cu is intentionally contained, the manufacturing cost of the non-oriented electrical steel sheet will increase. Therefore, in this embodiment, it is not necessary to actively contain Cu, and it can be contained at an impurity level. The Cu content is set to be less than the maximum value that may be inevitably mixed in the manufacturing process, that is, 0.200%. Regarding the Cu content, it is preferably 0.150% or less, and more preferably 0.100% or less. The Cu content can also be 0%. In addition, the lower limit of the Cu content is not particularly limited, but an extreme reduction in the Cu content sometimes causes an increase in manufacturing costs. Therefore, regarding the Cu content, it is preferably 0.001% or more, more preferably 0.003% or more, and further preferably 0.005% or more.
[0120] Ni: 0% or more, less than 0.500%
[0121] Ni (nickel) is an element that is inevitably mixed into steel. However, Ni is also an element that improves the strength of non-oriented electromagnetic steel sheets, so it can be intentionally contained. However, since Ni is expensive, the Ni content is set to less than 0.500%. Regarding the Ni content, it is preferably 0.400% or less, and more preferably 0.300% or less. The Ni content can also be 0%. In addition, the lower limit of the Ni content is not particularly limited, but an extreme reduction in the Ni content sometimes causes an increase in manufacturing costs. Therefore, regarding the Ni content, it is preferably 0.001% or more, more preferably 0.003% or more, and further preferably 0.005% or more.
[0122] Sn: 0~0.100%
[0123] Sb: 0~0.100%
[0124] Sn (tin) and Sb (antimony) are useful elements that help ensure low iron loss in non-oriented electromagnetic steel sheets by segregating to the surface of the base material and inhibiting oxidation and nitridation during annealing. In addition, Sn and Sb also have the effect of improving the texture by segregating to the grain boundary and increasing the magnetic flux density of the non-oriented electromagnetic steel sheet. Therefore, it is also possible to contain at least one of Sn and Sb as needed. However, when the content of these elements is excessive, the toughness of the steel sometimes decreases and cold rolling becomes difficult. Therefore, the content of Sn and Sb is set to 0.100% or less. Regarding the content of Sn and Sb, it is preferred that they are 0.060% or less respectively. The content of Sn and Sb can also be 0% respectively. In addition, in the case of reliably obtaining the above-mentioned effect, it is preferred that the content of at least one of Sn and Sb is set to 0.005% or more, and more preferably, it is set to 0.010% or more.
[0125] In the chemical composition of the base material (silicon steel sheet) of the non-oriented electrical steel sheet of the present embodiment, the remainder is Fe and impurities. Here, the so-called "impurities" refer to components mixed in due to various factors such as raw materials such as ore and scrap and manufacturing processes during industrial steel manufacturing, which means that they are allowed within the range that does not adversely affect the characteristics of the non-oriented electrical steel sheet of the present embodiment.
[0126] In addition, the contents of Cr and Mo as impurity elements are not particularly specified in the present embodiment. In the non-oriented electrical steel sheet of the present embodiment, even if these elements are contained in the range of 0.5% or less, the characteristics of the non-oriented electrical steel sheet of the present embodiment are not particularly affected. In addition, even if Ca and Mg are contained in the range of 0.002% or less, the characteristics of the non-oriented electrical steel sheet of the present embodiment are not particularly affected. Even if rare earth elements (REM) are contained in the range of 0.004% or less, the characteristics of the non-oriented electrical steel sheet of the present embodiment are not particularly affected. In addition, in the present embodiment, REM refers to a total of 17 elements consisting of Sc, Y and lanthanoids, and the above-mentioned REM content refers to the total content of these elements.
[0127] O is also an impurity element, but even if it is contained in a range of 0.05% or less, it has no effect on the characteristics of the non-oriented electrical steel sheet of the present embodiment. O may be mixed into the steel during the annealing process, so in the content at the billet stage (i.e., ladle value), even if it is contained in a range of 0.01% or less, it does not particularly affect the characteristics of the non-oriented electrical steel sheet of the present embodiment.
[0128] Furthermore, in addition to the above elements, elements such as Pb, Bi, As, B, and Se may be contained as impurity elements. However, when the content of each element is within the range of 0.0050% or less, the characteristics of the non-oriented electrical steel sheet of the present embodiment are not impaired.
[0129] The chemical composition of the base material of the non-oriented electromagnetic steel sheet of the present embodiment can be measured by ICP emission analysis or spark discharge emission analysis. In addition, C and S can be measured by combustion-infrared absorption method, N can be measured by inert gas combustion-thermal conductivity method, and O can be measured by inert gas melting-non-dispersion infrared absorption method. In addition, when the steel sheet to be measured has an insulating film, etc., it is removed below and the chemical composition is measured.
[0130] 3. Recrystallization rate
[0131] In the non-oriented electromagnetic steel sheet of the present embodiment, in order to ensure strength, the final annealing conditions are adjusted with respect to the recrystallization rate of the base material to be less than 100%. When it is completely recrystallized, the dislocation density is low enough and the desired strength cannot be obtained. Preferably, the recrystallization rate is 99% or less. There is no particular lower limit for the recrystallization rate, but when it is too low, the iron loss will increase, so it is preferably 20% or more. The recrystallization rate can be evaluated by grinding and etching a cross section parallel to the rolling direction of the steel sheet to make the microstructure appear, and measuring the area ratio occupied by the recrystallized grains and the area ratio of the non-recrystallized area.
[0132] The following is a detailed description of the method for measuring the recrystallization rate.
[0133] Figure 1A and Figure 1B A cross section parallel to the rolling direction and the sheet thickness direction of the nonoriented electrical steel sheet according to the present embodiment is shown. Figure 1A "RD" means rolling direction, and "ND" means plate thickness direction (i.e., the direction perpendicular to the plate surface).
[0134] First, a test piece is cut out from the non-oriented electromagnetic steel sheet so that the structure observation surface becomes a cross section parallel to the rolling direction and the plate thickness direction, and the cut test piece is embedded in the resin. Next, the structure observation surface is polished with abrasive paper and then polished to a mirror surface. Figure 1A As shown, the grain boundaries were made to appear in an etching solution (Nital: 5% Nital solution), the structure observation surface was observed with an optical microscope, and the recrystallization rate was measured by the following method.
[0135] Will be along Figure 1A The unetched portion extending in the rolling direction (RD) shown is determined as the non-recrystallized portion, and the recrystallization rate is defined as the area ratio of the portion other than the non-recrystallized portion. Figure 1B As shown in the figure, in a grid set at a pitch of 20μm in the thickness direction (ND) and a pitch of 25μm in the rolling direction (RD), the ratio of the number of intersections excluding the non-recrystallized part to the total number of intersections in the grid is defined as the recrystallization rate (see the following formula). However, because there are some fluctuations in the structure within the same sample, the recrystallization rate is measured at 5 points on the observation surface, and the average value is taken as the recrystallization rate of the test piece. In addition, Figure 1B The "0" mark in the middle represents the intersection of the grid of the non-recrystallized part (in Figure 1B In the case of , the number of intersections of the grid of the non-recrystallized part is "9" and the recrystallization rate is "95%").
[0136] Recrystallization rate (%) = 100 - 100 (number of intersections of the mesh of the non-recrystallized portion / total number of intersections of the mesh)
[0137] In addition, the so-called "recrystallization" can be defined as follows.
[0138] During cold rolling, lattice defects such as dislocations are introduced into the steel sheet, and the internal energy from them is accumulated in the steel sheet. Then, when the cold-rolled steel sheet is kept at a high temperature, atomic diffusion occurs and the lattice defects move. The internal energy is reduced by the combination of positive and negative dislocations or the movement to a stable configuration (rearrangement of dislocations). This phenomenon is called "recovery". At this time, the change in the metal structure cannot be observed at the optical microscope level. Figure 1A The unrecrystallized part (the area surrounded by the dotted line) is the recovery structure. When the high temperature is further maintained, grains with significantly lower dislocation density (recrystallized grains) are newly generated and grown, thereby releasing the internal energy accumulated in the material. This phenomenon is called "recrystallization". Figure 1A The area outside the non-recrystallized part is the recrystallized structure.
[0139] 4.Magnetic properties
[0140] In the non-oriented electrical steel sheet of the present embodiment, the excellent magnetic properties mean that the average iron loss W of the entire circuit is 10 / 400 Low, full-cycle average magnetic flux density B 50 In addition, the iron loss W 10 / 400 This means the iron loss generated under the conditions of maximum magnetic flux density of 1.0T and frequency of 400Hz, magnetic flux density B 50 This means the magnetic flux density in a magnetic field of 5000A / m.
[0141] The so-called full-circle average characteristics refer to the average of the characteristics in the rolling direction, the characteristics in the direction 45° from the rolling direction, and the characteristics in the direction 90° from the rolling direction, as described below. In addition, the so-called 90° direction from the rolling direction refers to the direction perpendicular to the rolling direction in the plate surface (that is, the direction perpendicular to the rolling direction and the plate thickness direction).
[0142] Weekly average value W 10 / 400 =(W 10 / 400 (0°)+2×W 10 / 400 (45°)+W 10 / 400 (90°)) / 4
[0143] Weekly average B 50 =(B 50 (0°)+2×B 50 (45°)+B 50 (90°)) / 4
[0144] Specifically, the iron loss is excellent when the thickness of the non-oriented electromagnetic steel sheet exceeds 0.30 mm and is 0.35 mm or less. 10 / 400 When the value is less than 40.0W / kg, and the value is more than 0.25mm and less than 0.30mm, the average value of the whole week W 10 / 400 When the value is less than 35.0W / kg, and exceeds 0.20mm and is less than 0.25mm, the average value of the whole week W 10 / 400 When the value is less than 30.0W / kg, the average value W of the whole week is less than 0.20mm. 10 / 400 25.0W / kg or less, regardless of plate thickness, average value over the entire week B 50 Here, in this embodiment, regarding the above magnetic properties (iron loss W 10 / 400 and magnetic flux density B 50 ), measured by the Epstein test specified in JIS C 2550-1 (2011) using a magnetic measurement test piece in each direction.
[0145] In addition, when the magnetic measurement test piece is small and measurement based on the Epstein method is difficult, the single sheet magnetic property measurement method (Single Sheet Tester: SST) specified in JIS C2556 (2015) can be used to perform measurement based on machine error correction in the same manner as the measurement value by the Epstein method.
[0146] 5. Mechanical properties
[0147] In the non-oriented electromagnetic steel sheet of the present embodiment, high strength means that the tensile (maximum) strength in the rolling direction exceeds 700 MPa. The tensile strength of the non-oriented electromagnetic steel sheet of the present embodiment exceeds 700 MPa. Preferably, the tensile strength is 710 MPa or more. Here, the tensile strength is measured by performing a tensile test in accordance with JIS Z 2241 (2011).
[0148] According to the non-oriented electrical steel sheet of the present embodiment, it is possible to achieve both high strength and excellent magnetic properties. This cannot be achieved by simply high alloying as in the past. In the present embodiment, in addition to the appropriateness of the total content of alloying elements that contribute to strength (Formula (i)), it is also possible to achieve a non-oriented electrical steel sheet that achieves both high strength and excellent magnetic properties by controlling the conditions of the manufacturing method described later (especially, the secondary cold rolling process and the final annealing process).
[0149] Therefore, the non-oriented electromagnetic steel sheet according to the present embodiment can be preferably used as a core material for rotating machines such as a drive motor or a generator of an electric vehicle or a hybrid vehicle, and a compressor motor of an air conditioner or a large air conditioner.
[0150] 6. Insulation film
[0151] In the non-oriented electromagnetic steel sheet of the present embodiment, it is preferable that an insulating film is provided on the surface of the base material. The non-oriented electromagnetic steel sheet is used after being laminated after punching out the core blank, so that the eddy current between the sheets can be reduced by providing the insulating film on the surface of the base material, and the eddy current loss can be reduced as the core.
[0152] In this embodiment, the type of insulating film is not particularly limited, and a known insulating film used as an insulating film of a non-oriented electrical steel sheet can be used. As such an insulating film, for example, a composite insulating film mainly composed of an inorganic substance and further containing an organic substance can be cited.
[0153] Here, the so-called composite insulating film refers to an insulating film in which fine organic resin particles are dispersed, for example, with at least one of metal salts such as chromate metal salts and phosphate metal salts, or inorganic substances such as colloidal silica, Zr compounds, and Ti compounds as the main component. In particular, from the perspective of reducing the environmental burden during production, which has become increasingly demanded in recent years, it is preferred to use an insulating film using a phosphate metal salt, a coupling agent of Zr or Ti as a starting material, or an insulating film using a phosphate metal salt, a carbonate or an ammonium salt of a coupling agent of Zr or Ti as a starting material.
[0154] The amount of the insulating film applied is not particularly limited, but is preferably 200 to 1500 mg / m2 per side. 2 More preferably, it is set to 300 to 1200 mg / m per single side. 2 By forming the insulating film in such a manner that the adhesion amount is within the above range, excellent uniformity can be maintained. In addition, when the adhesion amount of the insulating film is measured afterwards, various known measurement methods can be used, for example, a method of measuring the mass difference before and after immersion in a sodium hydroxide aqueous solution, or a fluorescent X-ray method using a calibration curve method, etc. can be appropriately used.
[0155] The non-oriented electrical steel sheet of the present embodiment has been described above, but the average grain size of the non-oriented electrical steel sheet of the present embodiment is not particularly limited. However, the average grain size of the recrystallized portion is about 10 μm to 30 μm.
[0156] In addition, the plate thickness of the non-oriented electromagnetic steel sheet of the present embodiment is not particularly limited. Generally, when the plate thickness becomes thinner, the iron loss becomes lower, but the manufacturing cost increases. Based on this point, when the plate thickness is 0.10 mm or more, the iron loss becomes further lower, and the cost increase is suppressed. In addition, when the plate thickness is 0.35 mm or less, the low iron loss can be maintained. Therefore, the preferred plate thickness of the non-oriented electromagnetic steel sheet of the present embodiment is 0.10 to 0.35 mm. More preferably, it is 0.15 to 0.30 mm.
[0157] 7. Manufacturing method
[0158] The non-oriented electrical steel sheet of the present embodiment is not particularly limited in terms of the manufacturing method, but can be manufactured by sequentially performing a hot rolling process, a pickling process, a primary cold rolling process, an intermediate annealing process, a secondary cold rolling process, and a final annealing process on a steel block having the above-mentioned chemical composition, for example, under the conditions shown below. In addition, when an insulating film is formed on the surface of a base material (silicon steel sheet), the insulating film forming process is performed after the above-mentioned final annealing process. Each process is described in detail below.
[0159] <Hot rolling process>
[0160] The steel block (blank) having the above chemical composition is heated, and the heated steel block is hot-rolled to obtain a hot-rolled steel plate. Here, there is no particular provision for the heating temperature of the steel block during hot rolling, and it is preferably set to 1050 to 1250°C, for example. In addition, there is no particular provision for the thickness of the hot-rolled steel plate after hot rolling, but considering the efficiency of hot rolling and subsequent processes, it is preferably set to about 1.5 to 3.0 mm, for example.
[0161] <Pickling process>
[0162] After the hot rolling process, pickling is performed without annealing the hot-rolled sheet. Generally, after the hot rolling process, pickling is often performed after annealing the hot-rolled sheet. However, in the case of steel containing many alloy elements as in the present embodiment, when the hot-rolled sheet is annealed, the toughness will deteriorate, and sometimes it will cause fracture during cold rolling. Therefore, in the present embodiment, annealing of the hot-rolled sheet is omitted. Specifically, pickling is performed on the above-mentioned hot-rolled sheet without annealing, and the oxide scale layer generated on the surface of the base material is removed. Here, the pickling conditions such as the concentration of the acid used for pickling, the concentration of the accelerator used for pickling, and the temperature of the pickling solution are not particularly limited, and can be set to known pickling conditions.
[0163] <Primary cold rolling process>
[0164] After pickling, the plate thickness is reduced to 1.0 mm or less. If the plate thickness after reduction exceeds 1.0 mm, the risk of fracture during secondary cold rolling is high. The plate thickness after reduction is preferably 0.9 mm or less, more preferably 0.8 mm or less.
[0165] <Intermediate annealing process>
[0166] After the primary cold rolling, intermediate annealing is performed to improve the magnetic properties of the non-oriented electromagnetic steel sheet. There is no particular regulation on the heat treatment conditions in the intermediate annealing, but for example, it is preferred to perform annealing at 800 to 1050°C for 1 to 300 seconds for the primary cold rolled sheet. When the soaking temperature in the intermediate annealing is too low, the average magnetic flux density B 50 There is a risk of reduction. Therefore, it is preferred that the soaking temperature in the intermediate annealing is set to 800°C or more, more preferably to 850°C or more, and further preferably to 900°C or more. On the other hand, when the soaking temperature in the intermediate annealing is too high, there is a risk of breakage during the secondary cold rolling. Therefore, regarding the soaking temperature in the intermediate annealing, it is preferably set to 1050°C or less, more preferably to 1040°C or less, and further preferably to 1030°C or less. In addition, when the soaking time in the intermediate annealing is too short, there will be a whole week average value of the magnetic flux density B 50 Therefore, the soaking time in the intermediate annealing is preferably set to be 1 sec or more, more preferably 5 sec or more, and further preferably 10 sec or more. On the other hand, if the soaking time in the intermediate annealing is too long, there is a risk of increased manufacturing costs. Therefore, the soaking time in the intermediate annealing is preferably set to be 300 sec or less, more preferably 200 sec or less, and further preferably 100 sec. In addition, before the intermediate annealing, rolling oil from the first cold rolling is attached, so it is preferably degreased.
[0167] <Second cold rolling process>
[0168] After the above-mentioned intermediate annealing, secondary cold rolling is performed. From the viewpoint of reducing iron loss, in the secondary cold rolling, it is preferred that the final plate thickness of the base material is set to be less than 0.35 mm. In addition, from the viewpoint of the manufacturing cost of the secondary cold rolling and the final annealing, it is preferred to set it to be more than 0.10 mm. In addition, when the intermediate annealing is performed in an oxidizing atmosphere, it is preferred to perform secondary cold rolling after removing the oxide scale. In addition, the reduction rate in the secondary cold rolling is not particularly limited, but for example, it can also be set to be more than 50% and less than 85%.
[0169] <Final annealing process>
[0170] After the secondary cold rolling, final annealing is performed. In the method for producing a non-oriented electrical steel sheet of the present embodiment, a continuous annealing furnace is used for final annealing.
[0171] Here, the final annealing conditions are as follows: the soaking temperature is set to 700 to 800°C, and the soaking time is set to 1 to 300 seconds. 2 The ratio of H is 0 to 100% by volume. 2 Atmosphere or N 2 atmosphere or their mixed atmosphere (i.e., H 2 +N 2 =100 volume %), and the dew point of the atmosphere is set below 30°C.
[0172] When the soaking temperature is less than 700°C, the density of dislocations introduced in the secondary cold rolling is too high, and the iron loss and magnetic flux density of the non-oriented electromagnetic steel sheet deteriorate. On the other hand, when the soaking temperature exceeds 800°C, recrystallization will proceed, and the strength of the non-oriented electromagnetic steel sheet will be insufficient. Regarding the lower limit of the soaking temperature, it is preferably above 710°C, and more preferably above 720°C. Regarding the upper limit of the soaking temperature, it is preferably below 800°C, and more preferably below 790°C. In addition, when the soaking time is less than 1 sec, the dislocation density cannot be fully reduced. On the other hand, when the soaking time exceeds 300 sec, it will cause an increase in manufacturing costs. Therefore, regarding the lower limit of the soaking time, it is preferably above 5 sec, and more preferably above 10 sec. Regarding the upper limit of the soaking time, it is preferably below 200 sec, and more preferably below 100 sec. Regarding H in the atmosphere 2 The ratio of the dew point of the atmosphere is preferably 0 to 90% by volume. The lower the dew point of the atmosphere, the better from the viewpoint of increasing the magnetic flux density. The dew point of the atmosphere is preferably 10°C or less, further preferably 0°C or less, and further preferably -10°C or less.
[0173] <Insulation film forming process>
[0174] After the above-mentioned final annealing, an insulating film forming step is performed as needed. Here, the method for forming the insulating film is not particularly limited, and the known insulating film forming treatment liquid described below can be used to apply and dry the treatment liquid by a known method. As a known insulating film, for example, a composite insulating film mainly composed of inorganic substances and also containing organic substances can be cited.
[0175] The so-called composite insulating film refers to an insulating film in which fine organic resin particles are dispersed, for example, with at least one of metal salts such as chromate metal salts and phosphate metal salts, or inorganic substances such as colloidal silica, Zr compounds, and Ti compounds as the main component. In particular, from the perspective of reducing the environmental burden during manufacturing, which has become increasingly demanded in recent years, it is preferred to use an insulating film using a phosphate metal salt, a coupling agent of Zr or Ti as a starting material, or an insulating film using a phosphate metal salt, a carbonate or an ammonium salt of a coupling agent of Zr or Ti as a starting material.
[0176] The surface of the base material on which the insulating film is formed may be subjected to any pretreatment such as degreasing treatment with alkali or pickling treatment with hydrochloric acid, sulfuric acid, phosphoric acid, etc. before the treatment liquid is applied. Alternatively, the treatment liquid may be applied to the surface of the base material after the final annealing without performing these pretreatments.
[0177] The non-oriented electromagnetic steel sheet of the present embodiment obtained as described above has excellent characteristics such as low iron loss and high strength, and is therefore preferred as a raw material for a rotor core. However, when the non-oriented electromagnetic steel sheet is used for a stator core, the iron loss is high, so there is a risk that excellent motor efficiency cannot be obtained. In this case, it is preferred that after the non-oriented electromagnetic steel sheet is punched, laminated, and the motor core is manufactured, only the stator core is subjected to strain relief annealing. The stator core subjected to strain relief annealing has recrystallization and grain growth progresses, and the iron loss is reduced, so the motor efficiency can be greatly improved.
[0178] The present invention will be described in more detail below through examples, but the conditions in the examples are only examples used to confirm the feasibility and effect of the present invention, and the present invention is not limited to the condition examples. As long as the purpose of the present invention is achieved without departing from the gist of the present invention, various conditions can be adopted.
[0179] Example
[0180] After heating the billet having the chemical composition shown in Table 1 to 1150°C, hot rolling was carried out at a final temperature of 850°C and a final plate thickness of 2.0 mm to produce a hot-rolled steel plate coiled at 650°C. In the obtained hot-rolled steel plate, the oxide scale on the surface was removed by pickling without annealing the hot-rolled plate, and then a cold rolling was carried out to obtain a plate thickness shown in Table 2. Then, after degreasing the steel plate after the first cold rolling, an intermediate annealing was carried out at 950°C for 40 seconds to obtain an intermediate annealed plate. For the intermediate annealed plate, a secondary cold rolling was carried out in a manner to obtain a cold-rolled steel plate with a thickness of 0.20 mm. Furthermore, in H 2 :15%,N 2: 85%, in a mixed atmosphere with a dew point of -30°C as shown in Table 2, final annealing was performed at the soaking temperature and soaking time shown in Table 2. Then, an insulating film was applied to manufacture a non-oriented electromagnetic steel sheet to prepare a test material. In addition, as shown in Test No. 25, a comparative example was also implemented, in which the hot rolled sheet annealing was performed with the soaking condition set to 950°C and 80 seconds.
[0181] The insulating film is formed by applying an insulating film composed of aluminum phosphate and a styrene-acrylic copolymer resin emulsion having a particle size of 0.2 μm to a predetermined adhesion amount and sintering the coating at 350° C. in the air.
[0182] [Table 1]
[0183]
[0184] [Table 2]
[0185]
[0186] The underlined characters indicate outside the scope of the present invention.
[0187] For each test material obtained, Epstein test pieces were collected from the rolling direction, the direction at 45° from the rolling direction, and the direction at 90° from the rolling direction. The magnetic properties (iron loss W 10 / 400 and magnetic flux density B 50 ) was evaluated. The average iron loss W of the whole cycle 10 / 400 The magnetic flux density B is less than 25.0W / kg and the average value of the whole cycle 50 1.57T or more is considered to be excellent in magnetic properties and is judged as qualified. If this condition is not met, the magnetic properties are considered to be poor and are judged as unqualified. In addition, the reason for setting this qualified condition is that the final plate thickness of the cold-rolled material of each test material is 0.20mm or less.
[0188] Furthermore, from each test material, JIS No. 5 tensile test pieces were collected in accordance with JIS Z 2241 (2011) in such a way that the length direction was consistent with the rolling direction of the steel plate. Then, the tensile test was carried out on the above test pieces in accordance with JIS Z 2241 (2011) to measure the tensile strength. The case where the tensile strength exceeded 700 MPa was considered to have a high strength and was judged as qualified. The case where the tensile strength was less than 700 MPa was considered to have a poor strength and was judged as unqualified. In addition, the average crystal grain size of the recrystallized grains of each test material was about 10 μm to 30 μm.
[0189] The results of the Epstein test and the tensile test are shown together in Table 2. In addition, the underlined components in Tables 1 and 2 represent components outside the scope of the present invention. In addition, the "-" in the chemical composition table of Table 1 means that the corresponding element content is 0% in the significant figures (the value to the minimum digit) specified in this embodiment.
[0190] It can be seen from Test Nos. 2, 4-7, 9, 12, 14, 15, 18-21 and 27-29 that the chemical composition and manufacturing conditions of the steel plates meet the requirements of the present invention; the whole-cycle average iron loss is low, the whole-cycle average magnetic flux density is high, and the steel plates have a high tensile strength of more than 700 MPa.
[0191] On the other hand, in Test Nos. 1, 3, 8, 10, 11, 13, 16, 17, 22 to 24, 25, 26, 30, and 31 as comparative examples, at least one of the magnetic properties and the tensile strength was inferior or the toughness was significantly deteriorated, making the production difficult.
[0192] Specifically, in Test No. 1, the Si content was lower than the specified range, resulting in poor tensile strength. In Test No. 3, the soaking temperature of the final annealing was lower than the specified range, resulting in poor iron loss and magnetic flux density. In Test No. 8, the final annealing temperature exceeded the specified range, so the recrystallization rate became 100%, resulting in poor tensile strength.
[0193] In test No. 10, the formula (i) was not satisfied, and the magnetic flux density was poor. In test No. 11, the Mn content exceeded the prescribed range, and the magnetic flux density was poor.
[0194] In test No. 13, the content of Al exceeded the prescribed range, and in test No. 16, formula (i) was not satisfied. In addition, in test No. 17, the plate thickness after the primary cold rolling exceeded the prescribed range. Therefore, in test No. 30, the content of Sn exceeded the prescribed range. Therefore, in test No. 31, the content of Sb exceeded the prescribed range, so the toughness deteriorated and broke during the secondary cold rolling, and the tensile strength and magnetic properties could not be measured. In test No. 25, the hot-rolled plate was annealed, so it broke during the primary cold rolling, and the tensile strength and magnetic properties could not be measured.
[0195] In test No. 22, equation (i) was not satisfied, resulting in poor tensile strength and iron loss. In test No. 23, the Mn content was lower than the specified range, and in test No. 24, the Al content was lower than the specified range, so in either case, the iron loss was poor.
[0196] Industrial Availability
[0197] As described above, according to the present invention, a non-oriented electrical steel sheet having high strength and excellent magnetic properties can be obtained.
Claims
1. A non-oriented electromagnetic steel sheet, wherein the chemical composition of the base material is, by mass%, C: 0-0.0050%, Si: 3.7-4.8%, Mn: 0.05% or more, less than 0.50%, sol.Al: 0.05~0.45%, P:0~0.030%、 S:0~0.0030%、 N:0~0.0040%、 Ti: 0% or more, less than 0.0050%, Nb: 0% or more, less than 0.0050%, Zr: 0% or more, less than 0.0050%, V: 0% or more, less than 0.0050%, Cu: 0% or more, less than 0.200%, Ni: 0% or more, less than 0.500%, Sn: 0~0.100%, Sb: 0 to 0.100%, and The rest: Fe and impurities; The recrystallization rate is 20% or more and less than 100% in terms of area ratio; Satisfy the following formulas (i) and (ii); Tensile strength exceeds 700MPa, 4.3≤Si+sol.Al+0.5×Mn≤4.9···(i) Wherein, the element symbol in the above formula is the content of each element in mass %, (B 50 (0°)+2×B 50 (45°)+B 50 (90°)) / 4≥1.57···(ii) Among them, B in the above formula (ii) 50 (0°) is the magnetic flux density in T at a magnetizing force of 5000 A / m in the rolling direction, B 50 (45°) is the magnetic flux density in T at a magnetizing force of 5000 A / m at a direction 45° from the rolling direction, B 50 (90°) is the magnetic flux density in T at a magnetizing force of 5000 A / m in a direction 90° from the rolling direction.
2. The non-oriented electrical steel sheet according to claim 1, wherein: The chemical components contain, in mass%, Sn: 0.005 to 0.100%, and Sb: 0.005~0.100% Choose 1 or 2 from the following.
3. The non-oriented electrical steel sheet according to claim 1 or 2, wherein: The base material has an insulating film on its surface.
4. A method for producing a non-oriented electromagnetic steel sheet, which is a method for producing a non-oriented electromagnetic steel sheet according to any one of claims 1 to 3, For the steel billet, implement in sequence: Hot rolling process; A cold rolling process, which omits the hot rolled sheet annealing and reduces the sheet thickness to less than 1.0 mm; Intermediate annealing process; Secondary cold rolling process; and The final annealing process has a soaking temperature of 700-800°C and a soaking time of 1-300 seconds. The steel billet has the following chemical composition: In terms of mass %, C:0~0.0050%、 Si: 3.7-4.8%, Mn: 0.05% or more, less than 0.50%, sol.Al: 0.05~0.45%, P:0~0.030%、 S:0~0.0030%、 N:0~0.0040%、 Ti: 0% or more, less than 0.0050%, Nb: 0% or more, less than 0.0050%, Zr: 0% or more, less than 0.0050%, V: 0% or more, less than 0.0050%, Cu: 0% or more, less than 0.200%, Ni: 0% or more, less than 0.500%, Sn: 0~0.100%, Sb: 0 to 0.100%, and The rest: Fe and impurities, And satisfy the following formula (i), 4.3≤Si+sol.Al+0.5×Mn≤4.9···(i) The element symbols in the above formula are the content of each element in mass %.